A lightweight antistatic nylon hanging net and preparation method thereof
By using materials such as polyamide-polyetheramine copolymer and hyperbranched polyamide-grafted carbon nanotubes in nylon hanging nets, the mechanical and antistatic properties of nylon hanging nets are improved, and the problem of low collusion strength and low strength of conventional nylon hanging nets is solved. The problem of insufficient antistatic performance is achieved, and efficient application effects are achieved.
Patent Information
- Application Number
- CN202410742930.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Conventional nylon hanging nets have low collusion strength and antistatic properties that cannot meet actual needs, resulting in inconvenient application.
Polyamide-polyetheramine copolymer is used as a reinforcing agent, and hyperbranched polyamide is generated from raw materials such as tris(3-aminophenyl)phosphine oxide, grafted to the surface of carbon nanotubes, and combined with zinc stearate and antioxidants. , ultraviolet absorbers and lubricants, which are formed by melt extrusion and spinning to form a nylon hanging net with excellent mechanical and antistatic properties.
The mechanical properties and antistatic properties of the nylon hanging net are improved, making it suitable for practical applications and highly practical.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nylon hanging nets, in particular to a lightweight antistatic nylon hanging net and a preparation method thereof. Background Art
[0002] A lifting net is a cargo net made of rope-like fibers. It can be lifted by a lifting device and is used to transport and lift small cargo. The material of the lifting net can be synthetic plastic fibers such as nylon, or it can be made of steel fibers. The cargo net made of plastic fibers is denser and can be used to carry small but light items. The mesh of the cargo net made of steel wire rope is relatively large and can carry some small and medium-sized workpieces. It is currently widely used in aviation, railways, ships, steel, mining, oil fields, ports, chemicals, electricity, machinery and other industries.
[0003] Nylon is one of the more commonly used hanging net materials, but the conventional nylon hanging net has low bonding strength and its antistatic performance cannot meet actual needs, which brings inconvenience to practical applications. Based on this situation, the present application discloses a lightweight antistatic nylon hanging net and a preparation method thereof to solve this technical problem. Summary of the invention
[0004] The object of the present invention is to provide a lightweight antistatic nylon hanging net and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a lightweight antistatic nylon hanging net comprises the following steps:
[0007] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 235-240°C under nitrogen atmosphere, reacted for 5-6 hours, depressurized to normal pressure, heated to 245-250°C, reacted for 3-6 hours, and after the reaction, the discharged material is cooled to obtain a polyamide-polyetheramine copolymer;
[0008] Step (2): tris(3-aminophenyl)phosphine oxide, adipic acid, N-methylpyrrolidone and pyridine are mixed and stirred under a nitrogen atmosphere until dissolved, triphenyl phosphite is added, reacted at 20-30°C for 2-3h, then heated to 70-80°C for 1-2h, and then heated to 120-130°C for 5-7h with stirring, then acyl chloride carbon nanotubes are added, and the mixture is kept warm for 1-2h. After the reaction is completed, the mixture is filtered, washed, and vacuum dried to obtain polyamide grafted carbon nanotubes;
[0009] Step (3): nylon, polyamide-polyetheramine copolymer, zinc stearate, antioxidant, ultraviolet absorber, lubricant and polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and stretched to obtain nylon threads, and a plurality of nylon threads are twisted to form braided threads, and the nylon suspension net is braided to obtain the nylon suspension net.
[0010] In a more optimized solution, in step (2), the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide is a, and 1≤a≤1.5.
[0011] In a more optimized solution, in step (3), the specific amounts of the components used are, by weight, 100-110 parts of nylon, 8-10 parts of polyamide-polyetheramine copolymer, 0.3-0.6 parts of zinc stearate, 0.5-1 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 0.2-0.5 parts of lubricant, and 3-5 parts of polyamide grafted carbon nanotubes.
[0012] In a more optimized solution, in step (1), the mass ratio of caprolactam, polyetheramine and hexamethylenediamine adipic acid salt is (74-80):(4-6):(16-20); the amount of adipic acid used is 0.8wt%-1.2wt% of caprolactam; and the amount of deionized water used is 2.5wt%-4wt% of caprolactam.
[0013] In a more optimized scheme, in step (2), the preparation steps of chlorinated carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 70-80°C for 6-7h, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; mixing carboxylated carbon nanotubes and thionyl chloride, adding N,N-dimethylformamide, stirring at 70-80°C for 20-24h, removing the solvent under reduced pressure, and vacuum drying to obtain chlorinated carbon nanotubes.
[0014] In a more optimized solution, the dosage of the carboxylated carbon nanotubes and thionyl chloride is 500 mg:50 mL; the mixed acid is a compound of concentrated nitric acid and concentrated sulfuric acid, and the volume ratio is 1:3.
[0015] In a more optimized solution, in step (3), the spinning temperature is 250-260°C, the spinning speed is 1000 m / min, the pulling speed is 600 m / min, and the pulling multiple is 2-3.
[0016] In a more optimized solution, in step (3), the antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0017] A more optimized solution is a nylon hanging net prepared according to any of the preparation methods described above.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The invention discloses a method for preparing a lightweight antistatic nylon hanging net. The method uses nylon 6 as a main material, adds a polyamide-polyetheramine copolymer as a reinforcing agent, and then adds auxiliary agents and fillers, wherein the auxiliary agents include zinc stearate, an antioxidant, an ultraviolet absorber and a lubricant, and the filler is polyamide grafted carbon nanotubes. After melt extrusion, spinning is performed, and traction and stretching are performed to obtain nylon wires. Then, a plurality of nylon wires are twisted to form braided wires, and the braided wires are used to braid each other to obtain the nylon hanging net. The nylon hanging net has not only excellent mechanical properties, but also excellent antistatic properties and high practicality.
[0020] In this scheme, the present application first utilizes raw materials such as caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine, etc. to polymerize to form a polyamide-polyetheramine copolymer, wherein the "mass ratio of caprolactam, polyetheramine, and hexamethylenediamine adipate is 78:6:16". At this time, the product is a ternary copolymer (PA6-PA66-polyetheramine). The polyamide-polyetheramine copolymer is added to nylon 6 as a toughening agent. On the one hand, the polyamide-polyetheramine copolymer can increase the softness and extensibility of nylon, thereby improving the mechanical properties of the nylon line such as the hooking strength, making it suitable for nylon hanging net products. On the other hand, the increase of the polyamide-polyetheramine copolymer can also introduce hydrophilic segments, improve the moisture regain of the nylon line, and improve its antistatic properties.
[0021] At the same time, the scheme also adds carbon nanotubes. The carbon nanotubes are first subjected to mixed acid oxidation on the surface to obtain carboxylated carbon nanotubes, and then the surface of the carboxylated carbon nanotubes is chlorinated to form chlorinated carbon nanotubes. Then, the scheme uses tris(3-aminophenyl)phosphine oxide and adipic acid as raw materials to generate hyperbranched polyamide, and the hyperbranched polyamide is grafted onto the surface of the chlorinated carbon nanotubes to obtain polyamide-grafted carbon nanotubes. On the one hand, the scheme uses tris(3-aminophenyl)phosphine oxide as a reaction monomer to introduce phosphorus into the system, and the flame retardant properties of the nylon line finally obtained are improved. On the other hand, the scheme limits the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide to a, then 1≤a≤1.5. Under this parameter, not only the grafted carbon nanotubes have good compatibility with the system and excellent dispersibility, but also due to the compound introduction of polyamide-grafted carbon nanotubes and polyamide-polyetheramine copolymers, the product has the most excellent antistatic properties.
[0022] The invention discloses a method for preparing a lightweight antistatic nylon hanging net. The scheme adjusts the dosage of each component raw material in the formula, uses a polyamide-polyetheramine copolymer as a reinforcing agent, and uses polyamide grafted carbon nanotubes as an antistatic filler. The mechanical properties of the prepared nylon hanging net are improved, and the nylon hanging net has very excellent antistatic properties and is highly practical. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In this embodiment, the nylon is specifically nylon 6; the polyetheramine is polyetheramine D2000; the carbon nanotube has a diameter of 20-40 nm and a length of 10-15 μm.
[0025] Embodiment 1: A method for preparing a lightweight antistatic nylon hanging net comprises the following steps:
[0026] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 235°C under nitrogen environment, reacted for 6 hours, depressurized to normal pressure, heated to 245°C, reacted for 6 hours, and after the reaction, the discharged material is cooled to obtain a polyamide-polyetheramine copolymer; the mass ratio of the caprolactam, polyetheramine and hexamethylenediamine adipate is 78:6:16; the amount of the adipic acid is 1.0wt% of the caprolactam; and the amount of the deionized water is 3wt% of the caprolactam.
[0027] Step (2): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0028] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 70° C. for 24 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0029] 2mmol tris(3-aminophenyl)phosphine oxide, 3mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine were mixed and stirred under nitrogen atmosphere until dissolved, 5mL triphenyl phosphite was added, the mixture was reacted at 20°C for 3h, the temperature was raised to 70°C for 2h, the temperature was further raised to 120°C, the mixture was stirred and reacted for 7h, acyl chloride carbon nanotubes were added, the mixture was kept warm for 1h, after the reaction, the mixture was filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide was a, and a=1.5.
[0030] Step (3): 100 parts of nylon 6, 8 parts of polyamide-polyetheramine copolymer, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 4 parts of polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and pulled and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0031] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0032] Embodiment 2: A method for preparing a lightweight antistatic nylon hanging net comprises the following steps:
[0033] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 235°C under nitrogen environment, reacted for 5.5 hours, depressurized to normal pressure, heated to 250°C, reacted for 5 hours, and after the reaction, the discharged material is cooled to obtain a polyamide-polyetheramine copolymer; the mass ratio of the caprolactam, polyetheramine and hexamethylenediamine adipate is 78:6:16; the amount of the adipic acid is 1.0wt% of the caprolactam; and the amount of the deionized water is 3wt% of the caprolactam.
[0034] Step (2): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0035] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 75° C. for 22 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0036] 2mmol tris(3-aminophenyl)phosphine oxide, 3mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine were mixed and stirred under nitrogen atmosphere until dissolved, 5mL triphenyl phosphite was added, the mixture was reacted at 25°C for 2.5h, the temperature was raised to 75°C for 1.5h, the temperature was further raised to 125°C, the mixture was stirred and reacted for 6h, acyl chloride carbon nanotubes were added, the mixture was kept warm for 1.5h, after the reaction, the mixture was filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide was a, then a=1.5.
[0037] Step (3): 100 parts of nylon 6, 9 parts of polyamide-polyetheramine copolymer, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 4 parts of polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0038] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0039] Embodiment 3: A method for preparing a lightweight antistatic nylon hanging net comprises the following steps:
[0040] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 240°C under nitrogen environment, reacted for 5 hours, depressurized to normal pressure, heated to 250°C, reacted for 4 hours, and after the reaction, the discharged material is cooled to obtain a polyamide-polyetheramine copolymer; the mass ratio of the caprolactam, polyetheramine and hexamethylenediamine adipate is 78:6:16; the amount of the adipic acid is 1.0wt% of the caprolactam; and the amount of the deionized water is 3wt% of the caprolactam.
[0041] Step (2): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0042] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 80° C. for 20 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0043] 2mmol tris(3-aminophenyl)phosphine oxide, 3mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine were mixed and stirred under nitrogen atmosphere until dissolved, 5mL triphenyl phosphite was added, the mixture was reacted at 30°C for 2h, the temperature was raised to 80°C for 1h, the temperature was further raised to 130°C, the mixture was stirred and reacted for 5h, acyl chloride carbon nanotubes were added, the mixture was kept warm for 2h, after the reaction, the mixture was filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide was a, then a=1.5.
[0044] Step (3): 100 parts of nylon 6, 10 parts of polyamide-polyetheramine copolymer, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 5 parts of polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0045] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0046] Comparative Example 1: A method for preparing a lightweight antistatic nylon hanging net, comprising the following steps:
[0047] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 240°C under nitrogen environment, reacted for 5 hours, depressurized to normal pressure, heated to 250°C, reacted for 4 hours, and after the reaction, the discharged material is cooled to obtain a polyamide copolymer; the mass ratio of the caprolactam to the hexamethylenediamine adipate is 84:16; the amount of the adipic acid is 1.0wt% of the caprolactam; and the amount of the deionized water is 3wt% of the caprolactam.
[0048] Step (2): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0049] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 80° C. for 20 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0050] 2mmol tris(3-aminophenyl)phosphine oxide, 3mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine were mixed and stirred under nitrogen atmosphere until dissolved, 5mL triphenyl phosphite was added, the mixture was reacted at 30°C for 2h, the temperature was raised to 80°C for 1h, the temperature was further raised to 130°C, the mixture was stirred and reacted for 5h, acyl chloride carbon nanotubes were added, the mixture was kept warm for 2h, after the reaction, the mixture was filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide was a, then a=1.5.
[0051] Step (3): 100 parts of nylon 6, 10 parts of polyamide copolymer, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 5 parts of polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0052] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0053] Comparative Example 1 uses Example 3 as the control group. In Comparative Example 1, no terpolymer is formed, only a binary copolymer is added, and the other steps remain unchanged.
[0054] Comparative Example 2: A method for preparing a lightweight antistatic nylon hanging net, comprising the following steps:
[0055] Step (1): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0056] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 80° C. for 20 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0057] 2mmol tris(3-aminophenyl)phosphine oxide, 3mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine were mixed and stirred under nitrogen atmosphere until dissolved, 5mL triphenyl phosphite was added, the mixture was reacted at 30°C for 2h, the temperature was raised to 80°C for 1h, the temperature was further raised to 130°C, the mixture was stirred and reacted for 5h, acyl chloride carbon nanotubes were added, the mixture was kept warm for 2h, after the reaction, the mixture was filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide was a, then a=1.5.
[0058] Step (2): 100 parts of nylon 6, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 5 parts of polyamide grafted carbon nanotubes are mixed, melt extruded, spun into fibers, and pulled and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0059] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0060] Comparative Example 2 uses Example 3 as the control group, in which no terpolymer is added and the other steps remain unchanged.
[0061] Comparative Example 3: A method for preparing a lightweight antistatic nylon hanging net, comprising the following steps:
[0062] Step (1): caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water are mixed, put into a polymerization kettle, evacuated, heated to 240°C under nitrogen environment, reacted for 5 hours, depressurized to normal pressure, heated to 250°C, reacted for 4 hours, and after the reaction, the discharged material is cooled to obtain a polyamide-polyetheramine copolymer; the mass ratio of the caprolactam, polyetheramine and hexamethylenediamine adipate is 78:6:16; the amount of the adipic acid is 1.0wt% of the caprolactam; and the amount of the deionized water is 3wt% of the caprolactam.
[0063] Step (2): The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 75° C. for 6 hours, cooling, collecting the product by centrifugation, washing and drying to obtain carboxylated carbon nanotubes; the mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:3.
[0064] 500 mg of carboxylated carbon nanotubes and 50 mL of thionyl chloride were mixed, 5 mL of N,N-dimethylformamide was added, and the mixture was stirred at 80° C. for 20 h. The solvent was removed under reduced pressure and the mixture was dried in vacuo to obtain acyl chloride carbon nanotubes.
[0065] 6mmol tris(3-aminophenyl)phosphine oxide, 2mmol adipic acid, 20mL N-methylpyrrolidone and 5mL pyridine are mixed and stirred under nitrogen environment until dissolved, 5mL triphenyl phosphite is added, the mixture is reacted at 30°C for 2h, the temperature is then raised to 80°C for 1h, the temperature is further raised to 130°C, the mixture is stirred and reacted for 5h, acyl chloride carbon nanotubes are added, the mixture is kept warm for 2h, after the reaction is completed, the mixture is filtered, washed and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide is a, then a=1 / 3.
[0066] Step (3): 100 parts of nylon 6, 10 parts of polyamide-polyetheramine copolymer, 0.5 parts of zinc stearate, 0.5 parts of antioxidant, 0.5 parts of ultraviolet absorber, 0.4 parts of lubricant and 5 parts of polyamide grafted carbon nanotubes are mixed, melt-extruded, spun into fibers, and stretched to obtain nylon threads, and several nylon threads are twisted to form braided threads, which are then braided to obtain a nylon hanging net.
[0067] The spinning temperature is 260°C, the spinning speed is 1000 m / min, the traction speed is 600 m / min, and the traction multiple is 2.6. The antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
[0068] Comparative Example 3 takes Example 3 as the control group. In Comparative Example 3, the molar ratio of adipic acid and tris(3-aminophenyl)phosphine oxide is adjusted, and the other steps remain unchanged.
[0069] Detection experiment:
[0070] 1. Take the nylon wire prepared in Examples 1 to 3 and Comparative Examples 1 to 3 as test samples, and test the tensile strength of the nylon wire. The test method refers to GB / T4344-2008. Take two samples, adopt a double-knot stretching knotting method, with a clamping distance of 500 mm and a stretching speed of 500 mm / min, and test the double-knot breaking strength.
[0071] 2. According to the raw materials disclosed in Examples 1 to 3 and Comparative Examples 1 to 3, melt extrusion granulation was performed, and then injection molding was performed into strips. The limiting oxygen index of the strips was tested, and the test standard was referenced to ISO4589. The volume resistivity of the sample was tested, and the sample size was 100 mm × 100 mm × 3 mm, and the test standard was referenced to GB / T1410.
[0072]
[0073] Conclusion: The present invention discloses a method for preparing a lightweight antistatic nylon hanging net. The scheme adjusts the dosage of each component raw material in the formula, uses polyamide-polyetheramine copolymer as a reinforcing agent, and polyamide grafted carbon nanotubes as an antistatic filler. The mechanical properties of the prepared nylon hanging net are improved, and the nylon hanging net has very excellent antistatic properties and is highly practical.
[0074] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a lightweight antistatic nylon hanging net, characterized in that: The following steps are involved: Step (1): mixing caprolactam, hexamethylenediamine adipate, adipic acid, polyetheramine and deionized water, putting into a polymerization reactor, evacuating, heating to 235-240°C under nitrogen environment, reacting for 5-6 hours, releasing the pressure to normal pressure, heating to 245-250°C, reacting for 3-6 hours, discharging and cooling after the reaction to obtain a polyamide-polyetheramine copolymer; the mass ratio of caprolactam, polyetheramine and hexamethylenediamine adipate is (74-80): (4-6): (16-20); the amount of adipic acid used is 0.8wt%-1.2wt% of caprolactam; the amount of deionized water used is 2.5wt%-4wt% of caprolactam; Step (2): tris(3-aminophenyl)phosphine oxide, adipic acid, N-methylpyrrolidone and pyridine are mixed and stirred under a nitrogen atmosphere until dissolved, triphenyl phosphite is added, reacted at 20-30°C for 2-3h, then heated to 70-80°C for 1-2h, further heated to 120-130°C, stirred for 5-7h, then acyl chloride carbon nanotubes are added, kept warm for 1-2h, filtered and washed after the reaction, and vacuum dried to obtain polyamide grafted carbon nanotubes; the molar ratio of adipic acid to tris(3-aminophenyl)phosphine oxide is a, then 1≤a≤1.5; Step (3): mixing nylon, polyamide-polyetheramine copolymer, zinc stearate, antioxidant, ultraviolet absorber, lubricant and polyamide grafted carbon nanotubes, melt extruding, spinning, pulling and stretching to obtain nylon wire, twisting a plurality of nylon wires to form a braided wire, and weaving to obtain a nylon hanging net; The specific amount of each component is, by mass, 100-110 parts of nylon, 8-10 parts of polyamide-polyetheramine copolymer, 0.3-0.6 parts of zinc stearate, 0.5-1 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 0.2-0.5 parts of lubricant, and 3-5 parts of polyamide grafted carbon nanotubes; The preparation steps of acyl chloride carbon nanotubes are as follows: placing carbon nanotubes in mixed acid, ultrasonicating in a water bath at 70-80°C for 6-7h, cooling, collecting products by centrifugation, washing and drying to obtain carboxylation carbon nanotubes; mixing carboxylation carbon nanotubes and thionyl chloride, adding N,N-dimethylformamide, stirring at 70-80°C for 20-24h, removing the solvent under reduced pressure, and vacuum drying to obtain acyl chloride carbon nanotubes.
2. The method for preparing a lightweight antistatic nylon hanging net according to claim 1, characterized in that: The mixed acid is a mixture of concentrated nitric acid and concentrated sulfuric acid in a volume ratio of 1:
3.
3. The method for preparing a lightweight antistatic nylon hanging net according to claim 1, characterized in that: In step (3), the spinning temperature is 250-260°C, the spinning speed is 1000 m / min, the pulling speed is 600 m / min, and the pulling multiple is 2-3.
4. The method for preparing a lightweight antistatic nylon hanging net according to claim 1, characterized in that: In step (3), the antioxidant is antioxidant 1010, the lubricant is liquid paraffin, and the ultraviolet absorber is ultraviolet absorber UV-9.
5. A nylon hanging net prepared according to the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Novel carbon nanotube surface molecularly imprinted polymer and preparation method thereof
CN103044639A
Method for in-situ polymerization preparation of hyperbranched polyamide grafted carbon nanotubes
CN106478988A
Continuous production apparatus of multi-copolymerized nylon
CN106916299A
Production system and production method of high-quality polycaprolactam
CN117244512A
Composite short fiber reinforced composite material and preparation method thereof
CN117887248A