Quasi-vertical structure PIN diode and preparation method thereof

Through the inverted structure, the P-type epitaxial layer of gallium nitride material and the N-type gallium nitride epitaxial layer are combined to solve the current edge collection effect and carrier diffusion problems of traditional gallium nitride PIN diodes. , improves the device's operating frequency and response time, and achieves higher performance.

CN118315442BActive Publication Date: 2024-11-15SUZHOU MOORE GALLIUM CORE SEMICON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410467806.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-11-15
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

Due to the material characteristics, traditional gallium nitride PIN diodes have reached the limit of operating frequency, withstand power and response time, which is difficult to further improve. There are current edge collection effect and carrier diffusion problems, resulting in degradation of device performance.

Method used

The quasi-vertical structure PIN diode with an inverted structure is used to grow a P-type epitaxial layer based on gallium nitride, an intrinsic gallium nitride epitaxial layer and an N-type gallium nitride epitaxial layer on the substrate, and the P-type epitaxial layer is combined with this The hole diffusion and background carrier recombination are achieved at the interface of the gallium nitride epitaxial layer, reducing contact resistance and reducing the doping concentration of the intrinsic layer.

Benefits of technology

It effectively reduces the series resistance of the device, improves the current density and breakdown characteristics, and achieves better conductivity modulation, thereby improving device performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118315442B_ABST
    Figure CN118315442B_ABST
Patent Text Reader

Abstract

The present invention relates to a quasi-vertical structure PIN diode and a preparation method thereof. The quasi-vertical structure PIN diode comprises: a substrate; a P-type epitaxial layer based on gallium nitride, located on one side of the substrate; an intrinsic gallium nitride epitaxial layer, located on the side of the P-type epitaxial layer away from the substrate; an N-type gallium nitride epitaxial layer, located on the side of the intrinsic gallium nitride epitaxial layer away from the substrate; an anode electrode, located on the side of the P-type epitaxial layer away from the substrate; and a cathode electrode, located on the side of the N-type gallium nitride epitaxial layer away from the substrate. The above-mentioned PIN diode is an inverted structure, and the P-type ohmic contact, which is greatly affected by the contact area, is placed under the table. The series resistance can be greatly reduced compared with the traditional upright structure, and the current density is improved; the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, and the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, thereby improving the device breakdown characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a quasi-vertical structure PIN diode and a preparation method thereof. Background Art

[0002] The third generation semiconductors have significant characteristics such as large bandgap, high breakdown field strength and high carrier mobility, which makes LED devices, microwave devices and power electronic devices made of the third generation semiconductor material gallium nitride have great advantages. Currently, PIN diodes use Si or GaAs materials. Due to their material properties, their operating frequency, withstand power and response time have reached their limits and are difficult to improve further. It is urgent to study high-power gallium nitride PIN diodes to achieve a significant improvement in performance.

[0003] The traditional GaN PIN diode uses a heavily Mg-doped P+GaN layer with low carrier concentration and activation rate. In order to reduce the impact of the device current edge effect, the active area table and anode surface of the device are extremely small, resulting in large anode ohmic contact resistance and large P-type region resistance, which makes the series resistance of the GaN PIN diode large and the forward current reduced. In addition, the intrinsic layer of the traditional GaN PIN diode is above the heavily doped N-type layer. Due to the significant carrier diffusion during the high-temperature epitaxial process, the electrons in the N-type layer easily diffuse to the intrinsic layer, resulting in an increase in the carrier concentration of the intrinsic layer and a decrease in the breakdown voltage of the diode. At the same time, the intrinsic layer with a high carrier concentration significantly deteriorates the conductivity modulation of the device and reduces the device performance. Summary of the invention

[0004] Based on this, it is necessary to provide a quasi-vertical structure PIN diode and a preparation method thereof in order to improve the performance of the device.

[0005] A quasi-vertical structure PIN diode, the quasi-vertical structure PIN diode comprising:

[0006] substrate;

[0007] A P-type epitaxial layer based on gallium nitride, located on one side of the substrate;

[0008] An intrinsic gallium nitride epitaxial layer, located on a side of the P-type epitaxial layer away from the substrate;

[0009] An N-type gallium nitride epitaxial layer, located on a side of the intrinsic gallium nitride epitaxial layer away from the substrate;

[0010] an anode electrode, located on a side of the P-type epitaxial layer away from the substrate; and

[0011] The cathode electrode is located on a side of the N-type gallium nitride epitaxial layer away from the substrate.

[0012] The quasi-vertical PIN diode of the technical solution of the present invention is an inverted structure. On the one hand, the quasi-vertical PIN diode has a smaller electrode size on the table surface to avoid the current crowding effect, while the table surface of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area. The P-type ohmic contact, which is greatly affected by the contact area, is placed under the table surface, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical PIN diode can be greatly reduced compared with the traditional upright structure, and the current density is improved; on the other hand, the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, while the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted quasi-vertical PIN diode structure of the present invention is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation, thereby improving device performance.

[0013] In a feasible implementation, the P-type epitaxial layer is a P-type gallium nitride epitaxial layer.

[0014] In a feasible implementation, the thickness of the P-type gallium nitride epitaxial layer is 10 nm to 10 μm; the material of the P-type gallium nitride epitaxial layer is heavily doped gallium nitride with a doping concentration of 1×10 17 cm -3 ~1×10 21 cm -3 .

[0015] In a feasible implementation, the P-type epitaxial layer includes a stacked barrier layer and a gallium nitride layer, the barrier layer is arranged close to the substrate, and there is a two-dimensional hole gas at the interface between the barrier layer and the gallium nitride layer.

[0016] In a feasible implementation, the barrier layer is selected from at least one of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer.

[0017] In a feasible implementation, in the P-type epitaxial layer, the thickness of the barrier layer is 10 nm to 1 μm, and the doping concentration of the barrier layer is 1×10 17 cm -3 ~1×10 21 cm -3 ;

[0018] In the P-type epitaxial layer, the thickness of the gallium nitride layer is 10 nm to 500 nm, and the doping concentration of the gallium nitride layer is 1×10 17 cm -3 ~1×10 21 cm -3 .

[0019] In a feasible implementation, the thickness of the N-type gallium nitride epitaxial layer is 10 nm to 10 μm; the material of the N-type gallium nitride epitaxial layer is heavily doped gallium nitride with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 .

[0020] In a feasible implementation, the thickness of the intrinsic gallium nitride epitaxial layer is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer is lightly doped gallium nitride with a doping concentration of 1×10 14 cm -3 ~1×10 17 cm -3 .

[0021] A method for preparing a quasi-vertical structure PIN diode comprises the following steps:

[0022] epitaxially growing a P-type epitaxial layer based on gallium nitride on a substrate;

[0023] epitaxially growing an intrinsic gallium nitride epitaxial layer on the P-type epitaxial layer;

[0024] epitaxially growing an N-type gallium nitride epitaxial layer on the intrinsic gallium nitride epitaxial layer;

[0025] Etching the N-type gallium nitride epitaxial layer and the intrinsic gallium nitride epitaxial layer to form an electrode region on the P-type epitaxial layer; and

[0026] An anode electrode is formed in the electrode region of the P-type epitaxial layer, and a cathode electrode is formed on the N-type gallium nitride epitaxial layer to obtain a quasi-vertical structure PIN diode.

[0027] The preparation method of the quasi-vertical structure PIN diode using the technical solution of the present invention can prepare an inverted gallium nitride quasi-vertical structure PIN diode. On the one hand, the quasi-vertical structure PIN diode has a smaller electrode size on the table surface to avoid the current crowding effect, while the table surface of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area. The P-type ohmic contact, which is greatly affected by the contact area, is placed under the table surface, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical structure PIN diode can be greatly reduced compared with the traditional upright structure, and the current density is improved. On the other hand, the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, while the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted quasi-vertical structure PIN diode structure of the present invention is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation, thereby improving the device performance.

[0028] In a feasible implementation, the epitaxial growth method is a MOCVD method, the temperature is 600 degrees to 1300 degrees, and the chamber pressure is 10 Torr to 200 Torr;

[0029] The epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 is a schematic diagram of a quasi-vertical PIN diode according to a first embodiment of the present invention;

[0031] Figure 2 This is a flow chart of a method for preparing a quasi-vertical PIN diode according to a first embodiment of the present invention;

[0032] Figure 3 It is a schematic diagram of the process of preparing the quasi-vertical structure PIN diode according to the first embodiment of the present invention after the epitaxial growth of the barrier layer;

[0033] Figure 4 It is a schematic diagram of epitaxially growing a gallium nitride layer in the preparation process of a quasi-vertical structure PIN diode according to the first embodiment of the present invention;

[0034] Figure 5 It is a schematic diagram of epitaxially growing an intrinsic gallium nitride epitaxial layer in the preparation process of the quasi-vertical structure PIN diode according to the first embodiment of the present invention;

[0035] Figure 6 It is a schematic diagram of epitaxially growing an N-type gallium nitride epitaxial layer in the preparation process of the quasi-vertical structure PIN diode according to the first embodiment of the present invention;

[0036] Figure 7 It is a schematic diagram of etching to form an electrode region during the preparation process of the quasi-vertical structure PIN diode according to the first embodiment of the present invention;

[0037] Figure 8 is a schematic diagram of a quasi-vertical PIN diode according to a second embodiment of the present invention;

[0038] Fig. 9 is a flow chart of a method for preparing a quasi-vertical structure PIN diode according to a second embodiment of the present invention;

[0039] Fig.10 It is a schematic diagram of epitaxially growing a P-type gallium nitride epitaxial layer in the preparation process of a quasi-vertical structure PIN diode according to the second embodiment of the present invention;

[0040] Fig.11 It is a schematic diagram of epitaxially growing an intrinsic gallium nitride epitaxial layer in the preparation process of a quasi-vertical structure PIN diode according to the second embodiment of the present invention;

[0041] Fig.12 It is a schematic diagram of epitaxially growing an N-type gallium nitride epitaxial layer in the preparation process of a quasi-vertical structure PIN diode according to the second embodiment of the present invention;

[0042] Fig.13 It is a schematic diagram of the electrode region after etching is formed in the preparation process of the quasi-vertical structure PIN diode according to the second embodiment of the present invention. DETAILED DESCRIPTION

[0043] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0044] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.

[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0046] Traditional GaN quasi-vertical PIN diodes are usually upright structures. This is because the intrinsic material of GaN is N-type material, and it is natural to dope GaN to form a P-type layer through compensation method. However, for upright quasi-vertical PIN diodes, due to the significant carrier diffusion during the high-temperature epitaxy process, the N-type layer electrons easily diffuse to the intrinsic layer, resulting in an increase in the intrinsic layer carrier concentration and a decrease in the diode breakdown voltage. At the same time, the intrinsic layer with high carrier concentration significantly deteriorates the device's conductivity modulation and reduces device performance. At the same time, due to the current edge collection effect, the table must be made smaller to improve device performance, so the contact electrode area on the table is very small. The table of the traditional GaN quasi-vertical PIN diode is a P-type ohmic contact, and the resistance of the P-type region itself is relatively large, so it is more difficult to make low resistance with a small P-type region area.

[0047] To this end, the present invention creatively proposes an inverted quasi-vertical PIN diode, which includes a substrate, a P-type epitaxial layer based on gallium nitride, an intrinsic gallium nitride epitaxial layer, an N-type gallium nitride epitaxial layer, an anode electrode, and a cathode electrode. Among them, the P-type epitaxial layer based on gallium nitride refers to the P-type epitaxial layer at least including a gallium nitride epitaxial layer, and the P-type epitaxial layer refers to being located on one side of the substrate; the intrinsic gallium nitride epitaxial layer is located on the side of the P-type epitaxial layer away from the substrate; the N-type gallium nitride epitaxial layer is located on the side of the intrinsic gallium nitride epitaxial layer away from the substrate; the anode electrode is located on the side of the P-type epitaxial layer away from the substrate; and the cathode electrode is located on the side of the N-type gallium nitride epitaxial layer away from the substrate.

[0048] The quasi-vertical PIN diode of the technical solution of the present invention is an inverted structure. On the one hand, the quasi-vertical PIN diode has a smaller electrode size on the table surface to avoid the current crowding effect, while the table surface of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area. The P-type ohmic contact, which is greatly affected by the contact area, is placed under the table surface, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical PIN diode can be greatly reduced compared with the traditional upright structure, and the current density is improved; on the other hand, the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, while the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted quasi-vertical PIN diode structure of the present invention is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation, thereby improving device performance.

[0049] The principle of compensatory doping by hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic GaN epitaxial layer is as follows: for GaN, the intrinsic GaN epitaxial layer itself is a light N-type layer. In the upright structure, the N-type GaN epitaxial layer is formed first, and then the intrinsic GaN epitaxial layer is formed on the N-type GaN epitaxial layer. In this process, the N doping in the N-type GaN epitaxial layer will penetrate into the intrinsic GaN epitaxial layer, resulting in the intrinsic GaN epitaxial layer. The N carrier concentration in the gallium epitaxial layer is too high; the quasi-vertical structure PIN diode of the present application is an inverted structure, a P-type gallium nitride epitaxial layer is formed first, and then an intrinsic gallium nitride epitaxial layer is formed on the P-type gallium nitride epitaxial layer. During this process, the P carriers in the P-type gallium nitride epitaxial layer will penetrate into the intrinsic gallium nitride epitaxial layer and recombine with the N carriers in the intrinsic gallium nitride epitaxial layer, reducing the N carrier concentration in the intrinsic gallium nitride epitaxial layer, thereby achieving compensatory doping.

[0050] See also Figure 1 The quasi-vertical PIN diode 100 of the first embodiment of the present invention includes a substrate 110, a P-type epitaxial layer 120 based on gallium nitride, an intrinsic gallium nitride epitaxial layer 130, an N-type gallium nitride epitaxial layer 140, an anode electrode 150 and a cathode electrode 160. The P-type epitaxial layer 120 based on gallium nitride means that the P-type epitaxial layer 120 includes at least a gallium nitride epitaxial layer.

[0051] The quasi-vertical structure PIN diode 100 of this embodiment is a gallium nitride inverted quasi-vertical structure PIN diode of a quasi-vertical structure, wherein a P-type epitaxial layer 120 is located on one side of a substrate 110, and the P-type epitaxial layer 120 includes a stacked barrier layer 121 and a gallium nitride layer 122, wherein the barrier layer 121 is disposed close to the substrate 110, and a two-dimensional hole gas (2DHG) is present at the heterojunction interface between the barrier layer 121 and the gallium nitride layer 122. The two-dimensional hole gas can further reduce the resistance of the P-type epitaxial layer 120.

[0052] Among them, the intrinsic gallium nitride epitaxial layer 130 is located on the side of the P-type epitaxial layer 120 away from the substrate 110, the N-type gallium nitride epitaxial layer 140 is located on the side of the intrinsic gallium nitride epitaxial layer 130 away from the substrate 110, the anode electrode 150 is located on the side of the P-type epitaxial layer 140 away from the substrate 110, and the cathode electrode 160 is located on the side of the N-type gallium nitride epitaxial layer 140 away from the substrate 110.

[0053] On the basis of the above-mentioned embodiment, the barrier layer 121 is selected from at least one of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer. Among them, the barrier layer 121 can be an aluminum nitride barrier layer, an aluminum gallium nitride barrier layer, or a composite layer of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer. When the barrier layer 121 is a composite layer of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer, the positions of the aluminum nitride barrier layer and the aluminum gallium nitride barrier layer are not limited, for example, the aluminum nitride barrier layer can be located between the aluminum gallium nitride barrier layer and the gallium nitride layer 122, or the aluminum gallium nitride barrier layer can be located between the aluminum nitride barrier layer and the gallium nitride layer 122.

[0054] On the basis of the above-mentioned embodiment, in the P-type epitaxial layer 120, the thickness of the barrier layer 121 is 10 nm to 1 μm, and the doping concentration of the barrier layer 121 is 1×10 17 cm -3 ~1×10 21 cm -3 The doping element may be Mg. The thickness of the barrier layer 121 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm or 1 μm, and the doping concentration may be, but is not limited to, 1×10 17 cm -3 , 1×10 18 cm -3 , 1×10 19 cm -3 , 1×10 20 cm -3 or 1×10 21 cm -3 .

[0055] In the P-type epitaxial layer 120, the thickness of the GaN layer 122 is 10 nm to 500 nm, and the doping concentration of the GaN layer 122 is 1×10 17 cm -3 ~1×10 21 cm -3 The doping element may be Mg. The thickness of the gallium nitride layer 122 may be, but is not limited to, 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, and the doping concentration may be, but is not limited to, 1×10 17 cm -3 , 1×10 18 cm -3 , 1×10 19 cm -3 , 1×10 20 cm -3 or 1×10 21 cm -3 In this embodiment, the thickness of the GaN layer 122 is 10 nm to 500 nm, which can prevent the two-dimensional holes at the interface between the GaN layer 122 and the barrier layer 121 from being too far away from the intrinsic GaN epitaxial layer 130 and causing performance disadvantages.

[0056] In the quasi-vertical structure PIN diode 100 of this embodiment, the P-type epitaxial layer 120 is a heterojunction of a barrier layer and a gallium nitride layer. Due to the polarization effect, there is a two-dimensional hole gas with high carrier surface density and high mobility at the heterojunction interface. At the same time, the P-type epitaxial layer 120 adopts a high concentration of doping, which can further increase the hole concentration and help to further reduce the resistance of the P-type epitaxial layer.

[0057] Based on the above-mentioned embodiment, the thickness of the N-type GaN epitaxial layer 140 is 10 nm to 10 μm; the material of the N-type GaN epitaxial layer 140 is heavily doped GaN with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 The doping element may be Si. The thickness of the N-type GaN epitaxial layer 140 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, and the doping concentration may be, but is not limited to, 1×10 16 cm -3 , 1×10 17 cm -3 , 1×1018 cm -3 , 1×10 19 cm -3 or 1×10 20 cm -3 .

[0058] Based on the above-mentioned embodiment, the thickness of the intrinsic gallium nitride epitaxial layer 130 is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer 130 is lightly doped gallium nitride with a doping concentration of 1×10 14 cm -3 ~1×10 17 cm -3 The doping element may be Si or Mg. The thickness of the intrinsic GaN epitaxial layer 130 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, and the doping concentration may be, but is not limited to, 1×10 14 cm -3 , 1×10 15 cm -3 , 1×10 16 cm -3 or 1×10 17 cm -3 .

[0059] Based on the above embodiments, the material of the substrate 110 is selected from at least one of Si, SiC, sapphire and GaN. Further, the thickness of the substrate 110 is 50 μm to 1000 μm.

[0060] On the basis of the foregoing embodiment, the anode electrode 150 is a Ni / Au metal layer, wherein the Ni metal layer is arranged close to the substrate 110, and the Au metal layer is arranged away from the substrate 110. The thickness of the Ni / Au metal layer can be (5-200) nm / (5-200) nm, preferably 10 nm / 15 nm. The anode electrode 150 of this type of material can achieve a contact with a lower resistance. Of course, the anode electrode 150 is not limited to this, and can also be other feasible electrodes. Furthermore, the area of ​​the anode electrode 150 is not limited and can be designed according to requirements.

[0061] Based on the above-mentioned embodiment, the cathode electrode 160 is a Ti / Al / Ni / Au metal layer, and the thickness of the Ti / Al / Ni / Au metal layer is 20nm / 120nm / 40nm / 50nm. The cathode electrode 160 made of such material can achieve a contact with a relatively low resistance.

[0062] It should be noted that the material and thickness of the anode electrode and the cathode electrode in the gallium nitride inverted quasi-vertical structure PIN diode of the present invention are not limited thereto, and may be any feasible material and thickness.

[0063] The quasi-vertical structure PIN diode of the technical solution of the present invention is an inverted structure. Due to the polarization effect, there is a two-dimensional hole gas with high carrier surface density and high mobility at the heterojunction interface of the P-type epitaxial layer, which is beneficial to reducing the resistance of the P-type epitaxial layer; the quasi-vertical structure PIN diode has a small electrode size on the table to avoid the current edge collection effect, while the table of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area. The P-type ohmic contact, which is greatly affected by the contact area, is placed under the table, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical structure PIN diode of the present invention can be greatly reduced compared with the traditional upright structure, and the current density is improved; the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, and the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted PIN structure is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation, thereby improving the device performance.

[0064] See also Figure 2 to Figure 7 The method for preparing the quasi-vertical structure PIN diode according to the first embodiment of the present invention comprises the following steps:

[0065] S10 , epitaxially growing a P-type epitaxial layer 120 based on gallium nitride on the substrate 110 .

[0066] In step S10 , the P-type epitaxial layer 120 based on gallium nitride includes a stacked barrier layer 121 and a gallium nitride layer 122 . The barrier layer 121 is disposed close to the substrate 110 . A two-dimensional hole gas is present at a heterojunction interface between the barrier layer 121 and the gallium nitride layer 122 .

[0067] In step S10, the operation of epitaxially growing the P-type epitaxial layer 120 based on gallium nitride on the substrate 110 is as follows: first, epitaxially growing the barrier layer 121 on the substrate 110, such as Figure 3 Then, a gallium nitride layer 122 is epitaxially grown on the barrier layer 121 to form a P-type epitaxial layer 120, as shown in FIG. Figure 4 shown.

[0068] In a feasible implementation, the barrier layer 121 is selected from at least one of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer. The barrier layer 121 may be an aluminum nitride barrier layer, an aluminum gallium nitride barrier layer, or a composite layer of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer. When the barrier layer 121 is a composite layer of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer, the positions of the aluminum nitride barrier layer and the aluminum gallium nitride barrier layer are not limited, for example, the aluminum nitride barrier layer may be located between the aluminum gallium nitride barrier layer and the gallium nitride layer 122, or the aluminum gallium nitride barrier layer may be located between the aluminum nitride barrier layer and the gallium nitride layer 122.

[0069] In a feasible implementation, in the P-type epitaxial layer 120, the thickness of the barrier layer 121 is 10 nm to 1 μm, and the doping concentration of the barrier layer 121 is 1×10 17 cm -3 ~1×10 21 cm -3 In the P-type epitaxial layer 120, the thickness of the gallium nitride layer 122 is 10 nm to 500 nm, and the doping concentration of the gallium nitride layer 122 is 1×10 17 cm -3 ~1×10 21 cm -3 .

[0070] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a barrier layer 121 and a gallium nitride layer 122 are epitaxially grown on the substrate 110 by the MOCVD method as a P-type epitaxial layer 120; wherein the epitaxial growth temperature is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0071] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0072] In step S10 , a P-type epitaxial layer 120 is epitaxially grown on the substrate 110 . The thickness and carrier concentration of the P-type epitaxial layer 120 can be designed more flexibly. The growth quality of the P-type epitaxial layer 120 is high, and the activation rate and carrier concentration are higher.

[0073] S20 , epitaxially growing an intrinsic gallium nitride epitaxial layer 130 on the P-type epitaxial layer 120 obtained in step S10 .

[0074] In a feasible implementation, the thickness of the intrinsic gallium nitride epitaxial layer 130 is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer 130 is heavily doped gallium nitride with a doping concentration of 1×10 14 cm -3 ~1×10 17 cm -3 .

[0075] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a GaN layer is epitaxially grown on the P-type epitaxial layer 120 obtained in step S10 using the MOCVD method as the intrinsic gallium nitride epitaxial layer 130. Figure 5 As shown; wherein, the temperature of epitaxial growth is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0076] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0077] S30 , epitaxially growing an N-type GaN epitaxial layer 140 on the intrinsic GaN epitaxial layer 130 obtained in step S20 .

[0078] In a feasible implementation, the thickness of the N-type GaN epitaxial layer 140 is 10 nm to 10 μm; the material of the N-type GaN epitaxial layer 140 is heavily doped GaN with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 .

[0079] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a GaN layer is epitaxially grown on the intrinsic GaN epitaxial layer 130 obtained in step S20 by using the MOCVD method as the N-type GaN epitaxial layer 140. Figure 6 As shown; wherein, the temperature of epitaxial growth is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0080] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0081] S40 , etching the N-type gallium nitride epitaxial layer 140 and the intrinsic gallium nitride epitaxial layer 130 obtained in step S30 to form an electrode region on the P-type epitaxial layer 120 .

[0082] Specifically, the N-type gallium nitride epitaxial layer 140 and the intrinsic gallium nitride epitaxial layer 130 obtained in step S30 are etched by an etching process, and an electrode region is formed on the P-type epitaxial layer 120 after etching, such as Figure 7 shown.

[0083] S50 , forming an anode electrode 150 in the electrode region of the P-type epitaxial layer 120 obtained in step S40 , and forming a cathode electrode 160 on the N-type gallium nitride epitaxial layer 140 , thereby obtaining a quasi-vertical structure PIN diode 100 .

[0084] In step S50 , the electrode region of the P-type epitaxial layer 120 obtained in step S40 is evaporated and photolithographically manufactured to form an anode electrode 150 . The area of ​​the anode electrode 150 is not limited and can be designed according to requirements.

[0085] In step S50 , the cathode electrode 160 is formed on the N-type GaN epitaxial layer 140 by evaporation and photolithography.

[0086] In step S50, after forming the anode electrode 150 and the cathode electrode 160, the device manufacturing is completed, and the quasi-vertical structure PIN diode 100 is obtained. Figure 1 shown.

[0087] The preparation method of the quasi-vertical structure PIN diode using the technical solution of the present invention can prepare an inverted structure gallium nitride quasi-vertical structure PIN diode. Due to the polarization effect, there is a two-dimensional hole gas with high carrier surface density and high mobility at the heterojunction interface of the P-type epitaxial layer, which is beneficial to reducing the resistance of the P-type epitaxial layer. The quasi-vertical structure PIN diode has a small electrode size on the table surface to avoid the current edge gathering effect. The table surface of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area, while the P-type ohmic contact, which is greatly affected by the contact area, is smaller. The contact is placed under the table, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical structure PIN diode of the present invention can be greatly reduced compared with the traditional upright structure, and the current density is improved; the hole diffusion and background carrier recombination at the interface between the P-type epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, and the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted PIN structure is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation.

[0088] See also Figure 8The quasi-vertical structure PIN diode 100 of the second embodiment of the present invention includes a substrate 110 , a P-type gallium nitride epitaxial layer 120 , an intrinsic gallium nitride epitaxial layer 130 , an N-type gallium nitride epitaxial layer 140 , an anode electrode 150 and a cathode electrode 160 .

[0089] The quasi-vertical structure PIN diode 100 of this embodiment is a gallium nitride inverted quasi-vertical structure PIN diode with a quasi-vertical structure, wherein the P-type gallium nitride epitaxial layer 120 is located on one side of the substrate 110, the intrinsic gallium nitride epitaxial layer 130 is located on the side of the P-type gallium nitride epitaxial layer 120 away from the substrate 110, the N-type gallium nitride epitaxial layer 140 is located on the side of the intrinsic gallium nitride epitaxial layer 130 away from the substrate 110, the anode electrode 150 is located on the side of the P-type gallium nitride epitaxial layer 140 away from the substrate 110, and the cathode electrode 160 is located on the side of the N-type gallium nitride epitaxial layer 140 away from the substrate 110.

[0090] Based on the above embodiments, the material of the substrate 110 is selected from at least one of Si, SiC, sapphire and GaN. Further, the thickness of the substrate 110 is 50 μm to 1000 μm.

[0091] On the basis of the above-mentioned embodiment, the thickness of the P-type GaN epitaxial layer 120 is 10 nm to 10 μm; the material of the P-type GaN epitaxial layer 120 is heavily doped GaN with a doping concentration of 1×10 17 cm -3 ~1×10 21 cm -3 The doping element may be Mg. The thickness of the P-type GaN epitaxial layer 120 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, and the doping concentration may be, but is not limited to, 1×10 17 cm -3 , 1×10 18 cm -3 , 1×10 19 cm -3 , 1×10 20 cm -3 or 1×10 21 cm -3 .

[0092] Based on the above-mentioned embodiment, the thickness of the intrinsic gallium nitride epitaxial layer 130 is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer 130 is lightly doped gallium nitride with a doping concentration of 1×10 14 cm -3~1×10 17 cm -3 The doping element may be Si or Mg. The thickness of the intrinsic GaN epitaxial layer 130 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or 100 μm, and the doping concentration may be, but is not limited to, 1×10 14 cm -3 , 1×10 15 cm -3 , 1×10 16 cm -3 or 1×10 17 cm -3 .

[0093] Based on the above-mentioned embodiment, the thickness of the N-type GaN epitaxial layer 140 is 10 nm to 10 μm; the material of the N-type GaN epitaxial layer 140 is heavily doped GaN with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 The doping element may be Si. The thickness of the N-type GaN epitaxial layer 140 may be, but is not limited to, 10 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm or 10 μm, and the doping concentration may be, but is not limited to, 1×10 16 cm -3 , 1×10 17 cm -3 , 1×10 18 cm -3 , 1×10 19 cm -3 or 1×10 20 cm -3 .

[0094] Based on the above implementation, the thickness of the P-type GaN epitaxial layer 120 is 500nm-10μm, and the thickness of the N-type GaN epitaxial layer 140 is 10nm-1μm. In the conventional upright GaN quasi-vertical structure PIN diode, the thickness of the P-type GaN epitaxial layer is small, the contact resistance is large, and the resistance of the P-type GaN epitaxial layer itself is also large, resulting in a large resistance of the entire device. In the present embodiment, the P-type gallium nitride epitaxial layer 120 is below the intrinsic gallium nitride epitaxial layer 130, and can grow thicker during epitaxial growth, specifically, the thickness is 500nm~10μm, the doping concentration can be higher, and the contact area can be larger, so that the contact resistance and the resistance of the P-type gallium nitride epitaxial layer 120 can be reduced; at the same time, the N-type gallium nitride epitaxial layer 140 is above the intrinsic gallium nitride epitaxial layer 130, and epitaxial growth is easier. Therefore, in the present embodiment, the thickness of the N-type gallium nitride epitaxial layer 140 is 10nm~1μm, which can avoid the performance degradation caused by the relatively large resistance of the P-type gallium nitride epitaxial layer 120.

[0095] On the basis of the above-mentioned embodiment, the anode electrode 150 is a Ni / Au metal layer, wherein the Ni metal layer is arranged close to the substrate 110, and the Au metal layer is arranged away from the substrate 110. The thickness of the Ni / Au metal layer can be (5-200) nm / (5-200) nm, preferably 10 nm / 15 nm. The anode electrode 150 of this type of material can achieve a contact with a lower resistance. Furthermore, the area of ​​the anode electrode 150 is not limited and can be designed according to requirements.

[0096] Based on the above-mentioned embodiment, the cathode electrode 160 is a Ti / Al / Ni / Au metal layer, and the thickness of the Ti / Al / Ni / Au metal layer is 20nm / 120nm / 40nm / 50nm. The cathode electrode 160 made of such material can achieve a contact with a relatively low resistance.

[0097] It should be noted that the material and thickness of the anode electrode and the cathode electrode in the gallium nitride inverted quasi-vertical structure PIN diode of the present invention are not limited thereto, and may be any feasible material and thickness.

[0098] The gallium nitride inverted quasi-vertical structure PIN diode using the technical solution of the present invention has, on the one hand, a smaller electrode size on the table top in order to avoid the current crowding effect, while the table top of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area, while the P-type ohmic contact, which is greatly affected by the contact area, is placed under the table top, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical structure PIN diode of the present invention can be greatly reduced compared with the traditional upright structure, and the current density is improved; on the other hand, the hole diffusion and background carrier recombination at the interface between the P-type gallium nitride epitaxial layer and the intrinsic gallium nitride epitaxial layer realize compensatory doping, while the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted quasi-vertical structure PIN diode structure of the present invention is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation, thereby improving device performance.

[0099] See also Figures 9 to 13 The method for preparing the quasi-vertical structure PIN diode according to the second embodiment of the present invention comprises the following steps:

[0100] S10 , epitaxially growing a P-type gallium nitride epitaxial layer 120 on the substrate 110 .

[0101] In a feasible implementation, the thickness of the P-type GaN epitaxial layer 120 is 10 nm to 10 μm; the material of the P-type GaN epitaxial layer 120 is heavily doped GaN with a doping concentration of 1×10 17 cm -3 ~1×10 21 cm -3 .

[0102] On the basis of the above-mentioned embodiment, the thickness of the P-type gallium nitride epitaxial layer 120 is 500nm to 10μm. In the conventional upright gallium nitride quasi-vertical structure PIN diode, the thickness of the P-type gallium nitride epitaxial layer is small, the contact resistance is large, and the resistance of the P-type gallium nitride epitaxial layer itself is also large, resulting in a large resistance of the entire device. In this embodiment, the P-type gallium nitride epitaxial layer 120 is below the intrinsic gallium nitride epitaxial layer 130, and can grow thicker during epitaxial growth. Specifically, the thickness is 500nm to 10μm, the doping concentration can be higher, and the contact area can be larger, so that the contact resistance and the resistance of the P-type gallium nitride epitaxial layer 120 can be reduced.

[0103] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a GaN layer is epitaxially grown on the substrate 110 by a MOCVD method as the P-type gallium nitride epitaxial layer 120. Fig.10As shown; wherein, the temperature of epitaxial growth is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0104] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0105] In step S10, a P-type gallium nitride epitaxial layer 120 is epitaxially grown on the substrate 110, so that the thickness and carrier concentration of the P-type gallium nitride epitaxial layer 120 can be designed more flexibly. The growth quality of the P-type gallium nitride epitaxial layer 120 is high, and the activation rate and carrier concentration are higher.

[0106] S20 , epitaxially growing an intrinsic gallium nitride epitaxial layer 130 on the P-type gallium nitride epitaxial layer 120 obtained in step S10 .

[0107] In a feasible implementation, the thickness of the intrinsic gallium nitride epitaxial layer 130 is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer 130 is heavily doped gallium nitride with a doping concentration of 1×10 14 cm -3 ~1×10 17 cm -3 .

[0108] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a GaN layer is epitaxially grown on the P-type GaN epitaxial layer 120 obtained in step S10 by using the MOCVD method as the intrinsic GaN epitaxial layer 130. Fig.11 As shown; wherein, the temperature of epitaxial growth is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0109] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0110] S30 , epitaxially growing an N-type GaN epitaxial layer 140 on the intrinsic GaN epitaxial layer 130 obtained in step S20 .

[0111] In a feasible implementation, the thickness of the N-type GaN epitaxial layer 140 is 10 nm to 10 μm; the material of the N-type GaN epitaxial layer 140 is heavily doped GaN with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 .

[0112] Based on the above-mentioned embodiment, the thickness of the N-type GaN epitaxial layer 140 is 10nm-1μm. The N-type GaN epitaxial layer 140 is above the intrinsic GaN epitaxial layer 130, and epitaxial growth is easier. Therefore, in this embodiment, the thickness of the N-type GaN epitaxial layer 140 is 10nm-1μm to avoid performance degradation caused by the relatively large resistance of the P-type GaN epitaxial layer 120.

[0113] In a feasible implementation, the epitaxial growth method is a MOCVD method, that is, a GaN layer is epitaxially grown on the intrinsic GaN epitaxial layer 130 obtained in step S20 by using the MOCVD method as the N-type GaN epitaxial layer 140. Fig.12 As shown; wherein, the temperature of epitaxial growth is 600 degrees to 1300 degrees, and the chamber pressure is 10Torr to 200Torr.

[0114] In a feasible implementation, the epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.

[0115] S40 , etching the N-type GaN epitaxial layer 140 and the intrinsic GaN epitaxial layer 130 obtained in step S30 to form an electrode region on the P-type GaN epitaxial layer 120 .

[0116] Specifically, the N-type GaN epitaxial layer 140 and the intrinsic GaN epitaxial layer 130 obtained in step S30 are etched by an etching process, and an electrode region is formed on the P-type GaN epitaxial layer 120 after etching, such as Fig.13 shown.

[0117] S50 , forming an anode electrode 150 in the electrode region of the P-type GaN epitaxial layer 120 obtained in step S40 , and forming a cathode electrode 160 on the N-type GaN epitaxial layer 140 , to obtain a quasi-vertical structure PIN diode 100 .

[0118] In step S50, the electrode region of the P-type gallium nitride epitaxial layer 120 obtained in step S40 is evaporated and photolithographically manufactured to form an anode electrode 150. The area of ​​the anode electrode 150 is not limited and can be designed according to requirements.

[0119] In step S50 , the cathode electrode 160 is formed on the N-type GaN epitaxial layer 140 by evaporation and photolithography.

[0120] In step S50, after forming the anode electrode 150 and the cathode electrode 160, the device manufacturing is completed, and the quasi-vertical structure PIN diode 100 is obtained. Figure 8 shown.

[0121] The preparation method of the quasi-vertical structure PIN diode using the technical solution of the present invention, on the one hand, in order to avoid the current edge gathering effect, the electrode size on the table of the quasi-vertical structure PIN diode is small, while the table of the inverted structure of the present invention is an N-type ohmic contact, and the contact resistance is less affected by the area, and the P-type ohmic contact, which is greatly affected by the contact area, is placed under the table, and the contact resistance is greatly reduced. Therefore, the series resistance of the quasi-vertical structure PIN diode of the present invention can be greatly reduced compared with the traditional upright structure, and the current density is improved; on the other hand, an intrinsic gallium nitride epitaxial layer is grown on the P-type gallium nitride epitaxial layer, and the hole diffusion and background carrier recombination at the interface between the P-type gallium nitride epitaxial layer and the intrinsic gallium nitride epitaxial layer can achieve compensatory doping, while the N-type gallium nitride epitaxial layer grown on the intrinsic gallium nitride epitaxial layer is usually thin, the high-temperature growth time is short, and the electron diffusion is weak. Therefore, the inverted quasi-vertical structure PIN diode structure of the present invention is easier to grow an intrinsic gallium nitride epitaxial layer with a low doping concentration, improve the device breakdown characteristics, and achieve better conductivity modulation.

[0122] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0123] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A quasi-vertical PIN diode, characterized in that: The quasi-vertical structure PIN diode comprises: substrate; A P-type epitaxial layer based on gallium nitride, located on one side of the substrate; An intrinsic gallium nitride epitaxial layer, located on a side of the P-type epitaxial layer away from the substrate; An N-type gallium nitride epitaxial layer, located on a side of the intrinsic gallium nitride epitaxial layer away from the substrate; an anode electrode, located on a side of the P-type epitaxial layer away from the substrate; and A cathode electrode, located on a side of the N-type gallium nitride epitaxial layer away from the substrate; The P-type epitaxial layer includes a stacked barrier layer and a gallium nitride layer, the barrier layer is arranged close to the substrate, and a two-dimensional hole gas is present at the interface between the barrier layer and the gallium nitride layer.

2. The quasi-vertical structure PIN diode according to claim 1, characterized in that: The barrier layer is selected from at least one of an aluminum nitride barrier layer and an aluminum gallium nitride barrier layer.

3. The quasi-vertical PIN diode according to claim 1, characterized in that: In the P-type epitaxial layer, the thickness of the barrier layer is 10 nm to 1 μm, and the doping concentration of the barrier layer is 1×10 17 cm -3 ~1×10 21 cm -3 .

4. The quasi-vertical PIN diode according to claim 1, characterized in that: In the P-type epitaxial layer, the thickness of the gallium nitride layer is 10 nm to 500 nm, and the doping concentration of the gallium nitride layer is 1×10 17 cm -3 ~1×10 21 cm -3 .

5. The quasi-vertical structure PIN diode according to claim 1, characterized in that: The thickness of the N-type gallium nitride epitaxial layer is 10 nm to 10 μm; the material of the N-type gallium nitride epitaxial layer is heavily doped gallium nitride with a doping concentration of 1×10 16 cm -3 ~1×10 20 cm -3 .

6. The quasi-vertical PIN diode according to claim 1, characterized in that: The thickness of the intrinsic gallium nitride epitaxial layer is 10 nm to 100 μm; the material of the intrinsic gallium nitride epitaxial layer is lightly doped gallium nitride with a doping concentration of 1×10 14 cm -3 ~1×10 17 cm -3 .

7. A method for preparing a quasi-vertical structure PIN diode according to any one of claims 1 to 6, characterized in that: The steps include: Epitaxially growing a P-type epitaxial layer based on gallium nitride on a substrate, wherein the P-type epitaxial layer comprises a stacked barrier layer and a gallium nitride layer, wherein the barrier layer is arranged close to the substrate, and a two-dimensional hole gas is present at an interface between the barrier layer and the gallium nitride layer; epitaxially growing an intrinsic gallium nitride epitaxial layer on the P-type epitaxial layer; epitaxially growing an N-type gallium nitride epitaxial layer on the intrinsic gallium nitride epitaxial layer; Etching the N-type gallium nitride epitaxial layer and the intrinsic gallium nitride epitaxial layer to form an electrode region on the P-type epitaxial layer; as well as An anode electrode is formed in the electrode region of the P-type epitaxial layer, and a cathode electrode is formed on the N-type gallium nitride epitaxial layer to obtain a quasi-vertical structure PIN diode.

8. The method for preparing a quasi-vertical structure PIN diode according to claim 7, characterized in that: The epitaxial growth method is a MOCVD method, the temperature is 600 to 1300 degrees, and the chamber pressure is 10 Torr to 200 Torr; or The epitaxial growth method is the MBE method, and the process conditions are: the temperature is 550 degrees to 700 degrees, the gallium beam current is 5.0×10 -7 Torr~7.5×10 -7 Torr, and the nitrogen beam flow is 0.5sccm~2.5sccm.