A lithium ion battery
By using specific mononitrile compounds and fluorinated compounds in non-aqueous electrolytes in lithium-ion batteries, combined with lithium nickel manganese oxide cathode materials, the rate performance and cycle life problems of lithium nickel manganese oxide batteries are solved, and high operating voltages are achieved Excellent performance and long life.
Patent Information
- Application Number
- CN202410741857.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Lithium nickel manganese oxide cathode material has the problem of deteriorating rate performance and significantly reducing cycle life in lithium-ion batteries.
A non-aqueous electrolyte containing a specific content of mononitrile compounds and fluorinated compounds is used, combined with lithium nickel manganate as the cathode material, and the electrolyte composition is optimized to improve the cycle stability and rate performance of the battery.
It achieves excellent rate performance and cycle stability of lithium-ion batteries under high operating voltage, extends its service life, has a capacity retention rate of more than 80%, and a DCR growth rate of less than 100%.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a lithium ion battery. Background Art
[0002] At present, lithium-ion batteries are developing rapidly in the fields of electric vehicles and large-scale energy storage, occupying a large market share. With the widespread application of lithium-ion batteries, consumers also have higher demands for the energy density of lithium-ion batteries.
[0003] Increasing the operating voltage of lithium-ion batteries is an effective means to increase the energy density of batteries. Therefore, developing cathode materials with high operating voltage is an important way to achieve high specific energy lithium-ion batteries. Compared with the operating voltage of lithium iron phosphate batteries (3.2V), lithium-ion batteries using nickel manganese oxide cathodes have an operating voltage of up to 4.6V. Under the premise of equal battery capacity, the use of nickel manganese oxide cathodes can increase the energy density of batteries by 44%.
[0004] Although lithium nickel manganese oxide cathode has broad prospects, its high working voltage characteristic also limits the practical application of this material. In practical applications, the rate performance of lithium-ion batteries using lithium nickel manganese oxide as cathode material deteriorates significantly and the cycle life decreases significantly, so lithium nickel manganese oxide cathode material has not been widely used. Summary of the invention
[0005] In order to solve the problem that the battery rate performance deteriorates significantly and the cycle life decreases significantly when the lithium nickel manganese oxide positive electrode material is used in the prior art lithium ion battery, the present invention provides a lithium ion battery. The lithium ion battery of the present invention adopts a specific non-aqueous electrolyte and lithium nickel manganese oxide as the positive electrode material, and can achieve excellent rate performance and excellent cycle stability at a high operating voltage.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions.
[0007] The present invention provides a lithium ion battery, comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein:
[0008] The electrolyte is a non-aqueous electrolyte, which includes a mononitrile compound and a fluorinated compound, wherein the content of the mononitrile compound is 0.1%-25%, and the percentage is the mass percentage of the mononitrile compound in the non-aqueous electrolyte; the content of the fluorinated compound is 10%-60%, and the percentage is the mass percentage of the fluorinated compound in the non-aqueous electrolyte; the fluorinated compound is selected from one or more of trifluoromethylbenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate, decafluoropentane, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl-1,1,2,2-tetrafluoroethyl ether and pentafluoroethylbenzene;
[0009] The positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes lithium nickel manganese oxide, and the chemical formula of the lithium nickel manganese oxide is Li x Ni y Mn 2-y-m M m O4, wherein 0.9≤x≤1.1, 0.3≤y≤0.8, 0≤m≤0.1, and M is one or more of Fe, Ti, Co, Cr, V, Cu, Zn, Zr, Al and Nb.
[0010] The positive and progressive effects of the present invention are:
[0011] The present invention provides a lithium ion battery using lithium nickel manganese oxide as a positive electrode active material. The non-aqueous electrolyte contains a specific content of a mononitrile compound and a specific type and content of a fluorinated compound. The combination of the mononitrile compound and the fluorinated compound has a good synergistic effect, and can simultaneously solve the problems of manganese dissolution and electrolyte instability in the lithium ion battery using lithium nickel manganese oxide as the positive electrode material, thereby realizing a high-voltage lithium ion battery with excellent rate performance, good cycle stability and long service life. DETAILED DESCRIPTION
[0012] The lithium-ion battery of the present invention comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein:
[0013] The electrolyte is a non-aqueous electrolyte, which includes a mononitrile compound and a fluorinated compound, wherein the content of the mononitrile compound is 0.1%-25%, and the percentage is the mass percentage of the mononitrile compound in the non-aqueous electrolyte; the content of the fluorinated compound is 10%-60%, and the percentage is the mass percentage of the fluorinated compound in the non-aqueous electrolyte; the fluorinated compound is selected from one or more of trifluoromethylbenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate, decafluoropentane, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl-1,1,2,2-tetrafluoroethyl ether and pentafluoroethylbenzene;
[0014] The positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes lithium nickel manganese oxide, and the chemical formula of the lithium nickel manganese oxide is Li x Ni y Mn 2-y-m M m O4, wherein 0.9≤x≤1.1, 0.3≤y≤0.8, 0≤m≤0.1, and M is one or more of Fe, Ti, Co, Cr, V, Cu, Zn, Zr, Al and Nb.
[0015] Electrolyte
[0016] In some embodiments, the mononitrile compound is selected from one or more of monofluoroacetonitrile, n-butyronitrile, isobutyronitrile, n-valeronitrile, isovaleronitrile and n-hexanenitrile.
[0017] In some embodiments, the content of the mononitrile compound is 8%-20%.
[0018] In some specific embodiments, the content of the mononitrile compound is 0.1%, 0.3%, 8%, 20% or 25%.
[0019] In some embodiments, the content of the fluorinated compound is 25%-50%.
[0020] In some specific embodiments, the content of the fluorinated compound is 10%, 15%, 25%, 30%, 50% or 60%.
[0021] In some preferred embodiments, the content of the mononitrile compound is 8%-20%, and the content of the fluorinated compound is 25%-50%.
[0022] In some preferred embodiments, the mononitrile compound is monofluoroacetonitrile, n-valeronitrile, isovaleronitrile or n-hexanenitrile; the fluorinated compound is trifluoromethylbenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate, decafluoropentane or 2,2,2-trifluoroethyl acetate.
[0023] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is trifluoromethylbenzene.
[0024] In a specific embodiment, the mononitrile compound is monofluoroacetonitrile, and the fluorinated compound is trifluoromethylbenzene.
[0025] In a specific embodiment, the mononitrile compound is isovaleronitrile, and the fluorinated compound is trifluoromethylbenzene.
[0026] In a specific embodiment, the mononitrile compound is n-hexanenitrile, and the fluorinated compound is trifluoromethylbenzene.
[0027] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether.
[0028] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is bis(2,2,2-trifluoroethyl) ether.
[0029] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is trifluoroethyl methyl carbonate.
[0030] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is decafluoropentane.
[0031] In a specific embodiment, the mononitrile compound is n-valeronitrile, and the fluorinated compound is 2,2,2-trifluoroethyl acetate.
[0032] In some embodiments, the non-aqueous electrolyte further includes an additive, the additive being selected from one or more of triallyl isocyanurate, dicyclohexylcarbodiimide, 1,6-hexamethylene diisocyanate and lithium difluorobisoxalate phosphate, and the content of the additive is 0.01%-2%, for example 0.1% or 0.5%, where the percentage is the mass percentage of the additive in the non-aqueous electrolyte.
[0033] In a specific embodiment, the mononitrile compound is n-valeronitrile, the fluorinated compound is trifluoromethylbenzene, and the additive is triallyl isocyanurate.
[0034] In another specific embodiment, the mononitrile compound is n-valeronitrile, the fluorinated compound is trifluoromethylbenzene, and the additive is dicyclohexylcarbodiimide.
[0035] In some embodiments, the non-aqueous electrolyte includes carbonate esters as non-aqueous solvents.
[0036] When the carbonate includes one or more of ethylene carbonate, ethyl methyl carbonate, propylene carbonate and diethyl carbonate; the content of the carbonate is 5%-65%, and the percentage is the mass percentage of the carbonate in the non-aqueous electrolyte.
[0037] When the carbonate includes dimethyl carbonate, the content of the dimethyl carbonate does not exceed 5%, where the percentage is the mass percentage of the dimethyl carbonate in the non-aqueous electrolyte.
[0038] In a specific embodiment, the carbonate is ethylene carbonate and ethyl methyl carbonate, and the volume ratio of ethylene carbonate to ethyl methyl carbonate is 3:7.
[0039] In some embodiments, the non-aqueous electrolyte includes a lithium salt.
[0040] Among them, the lithium salt can be a conventional lithium salt used as an electrolyte in the art, preferably including one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), lithium difluorobis(oxalatophosphate) (LiODFP), lithium difluorooxalatoborate (LiODFB), lithium difluorophosphate (LiPO2F2) and lithium trifluoromethylsulfonate (CF3SO3Li).
[0041] Wherein, the concentration of lithium salt in the non-aqueous electrolyte is 0.1 mol / L-2 mol / L, for example, 1 mol / L.
[0042] In some embodiments, the non-aqueous electrolyte can be prepared by the following preparation method: the non-aqueous electrolyte is prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1 ppm, and the water content is 0.1 ppm; the carbonate as a non-aqueous solvent is mixed evenly, other components other than lithium salt are added, mixed evenly, and then lithium salt is added and mixed evenly. Among them, "other components other than lithium salt" include mononitrile compounds and fluorinated compounds; when the non-aqueous electrolyte also includes additives, "other components other than lithium salt" include mononitrile compounds, fluorinated compounds and additives.
[0043] positive electrode
[0044] In some embodiments, in the positive electrode active material layer, the content of the lithium nickel manganese oxide is 50%-98.5%, where the percentage is the mass percentage of the lithium nickel manganese oxide in the positive electrode active material layer.
[0045] In some embodiments, in the lithium nickel manganese oxide, the atomic percentage of manganese in the transition metal is not less than 50%, preferably 50%-75%.
[0046] In a specific embodiment, the chemical formula of the lithium nickel manganese oxide is LiNi 0.5 Mn 1.5 O4.
[0047] In a specific embodiment, the chemical formula of the lithium nickel manganese oxide is LiNi 0.5 Mn 1.48 Fe 0.02 O4.
[0048] In a specific embodiment, the chemical formula of the lithium nickel manganese oxide is LiNi 0.5 Mn 1.47 Zr 0.03 O4.
[0049] In a specific embodiment, the chemical formula of the lithium nickel manganese oxide is LiNi 0.5 Mn 1.45 Al 0.05 O4.
[0050] In some embodiments, the positive electrode active material layer further includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.
[0051] In some embodiments, the positive electrode active material layer further includes a conductive agent.
[0052] Among them, the type of the conductive agent is not particularly limited, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black SP, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0053] In some embodiments, the positive electrode active material layer further includes a binder.
[0054] Among them, the type of the binder is not particularly limited, and can be selected from polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer and its sulfonate, styrene-butadiene rubber, fluororubber and various copolymers.
[0055] In some embodiments, the positive electrode active material layer further includes a thickener, such as sodium carbon methyl cellulose.
[0056] In some embodiments, the positive electrode includes a positive electrode current collector, and the positive electrode active material layer is disposed on at least one surface of the positive electrode current collector.
[0057] Among them, the positive electrode current collector is a substrate supporting the positive electrode active material layer, which is usually a metal foil with a thickness of 3μm-500μm. There is no special restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the secondary battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The positive electrode current collector usually has a smooth surface, but fine lines can also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the positive electrode current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the positive electrode current collector is aluminum foil.
[0058] In the present invention, the positive electrode can be prepared by conventional methods in the art, generally comprising: fully stirring and mixing the components of the positive electrode material layer in a solvent to obtain a positive electrode slurry, coating the positive electrode slurry on a positive electrode current collector, drying, cold pressing, and slitting.
[0059] negative electrode
[0060] In some embodiments, the negative electrode includes a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material.
[0061] Among them, as the negative electrode active material, a compound that can reversibly embed and deintercalate lithium can be used. Specific examples of negative electrode active materials include but are not limited to: carbon materials such as crystalline carbon (natural graphite and artificial graphite, etc.), amorphous carbon, carbon-coated graphite and resin-coated graphite, or oxide materials such as indium oxide, silicon oxide, tin oxide, lithium titanate, zinc oxide, lithium oxide, etc., and can also be lithium metal or a metal material that can form an alloy with lithium; wherein the metal material that can form an alloy with lithium is, for example, Cu, Sn, Si, Co, Mn, Fe, Sb and Ag. Binary or ternary alloys containing these metals and lithium can also be used as negative electrode active materials. These negative electrode active materials can be used alone or in combination of two or more. From the perspective of high energy density, carbon materials such as graphite can also be used in combination with Si, Si alloys, Si oxides and other Si-based materials.
[0062] In some embodiments, the negative electrode active material includes any one of soft carbon, hard carbon, artificial graphite, natural graphite, silicon, silicon oxides, silicon carbon compounds, or lithium titanate, or a combination of at least two thereof.
[0063] In some embodiments, the negative electrode active material layer further includes a conductive agent.
[0064] Among them, the type of the conductive agent is not particularly limited, and can be selected from graphite materials such as natural graphite and artificial graphite, carbon black SP, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black and other carbon black materials, carbon fibers, metal fibers and other conductive fibers, metal powders such as carbon fluoride powder, aluminum powder, nickel powder and other metal powders, zinc oxide, potassium titanate and other conductive whiskers, and titanium dioxide and other conductive metal oxides or polyphenylene derivatives.
[0065] In some embodiments, the negative electrode active material layer further includes a binder.
[0066] Among them, the type of the binder is not particularly limited, and can be selected from polyvinylidene fluoride, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer and its sulfonate, styrene-butadiene rubber, fluororubber and various copolymers.
[0067] In some embodiments, the negative electrode active material layer further includes a thickener, such as sodium carbon methyl cellulose.
[0068] In some embodiments, the negative electrode includes a negative electrode current collector, and the negative electrode active material layer is disposed on at least one surface of the negative electrode current collector.
[0069] Among them, the negative electrode current collector is a substrate supporting the negative electrode active material, usually a metal foil with a thickness of 3μm-500μm. There is no special restriction on the material, as long as it has high conductivity and does not produce chemical reactions in the secondary battery system. For example, it can be a foil formed after surface treatment of nickel, titanium, aluminum, nickel, silver, stainless steel, carbon, etc. The negative electrode current collector usually has a smooth surface, but fine lines can also be formed on its surface to increase the adhesion between the positive electrode active material and the current collector. In addition to the foil, the negative electrode current collector can also be used in any one or more combinations of various forms such as film, mesh, porous, foam or non-woven fabric. Generally, the negative electrode current collector is copper foil.
[0070] In the present invention, the negative electrode can be prepared by conventional methods in the art, generally comprising: fully stirring and mixing the components of the negative electrode material layer in a solvent to obtain a negative electrode slurry, coating the negative electrode slurry on a negative electrode current collector, drying, cold pressing, and cutting.
[0071] Diaphragm
[0072] The separator between the positive electrode and the negative electrode uses an insulating film with high ion permeability and high mechanical strength. The typical thickness of the separator is 9μm-18μm; the pore size is 5μm-300μm; the air permeability is 180 s / 100mL - 380s / 100mL; the porosity is 30% to 50%. As a separator, a sheet or non-woven fabric made of the following substances is usually used: an olefin polymer such as polypropylene or polyethylene; or, further, the aforementioned sheet or non-woven fabric is used as a base film and coated with a coating (such as a nano-alumina coating).
[0073] In a specific embodiment, polyethylene with a thickness of 9 μm is used as a base film, and a nano-aluminum oxide coating with a thickness of 3 μm is coated on the base film to obtain a diaphragm.
[0074] Lithium-ion battery
[0075] In the present invention, the lithium-ion battery is generally a square hard-shell battery, a soft-pack battery and a cylindrical battery.
[0076] In the present invention, the lithium-ion battery can be prepared by conventional methods in the art. Taking a soft-pack battery as an example, the preparation method of the lithium-ion battery includes the following steps: stacking the positive electrode, the separator, and the negative electrode in order, so that the separator is located between the positive electrode and the negative electrode to play an isolating role, and stacking to obtain a bare cell; putting the bare cell into an aluminum-plastic film, drying and removing water, injecting the corresponding electrolyte and sealing, and then going through the processes of standing, hot and cold pressing, forming, clamping, and capacity separation to obtain a finished soft-pack lithium-ion battery.
[0077] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention. The present invention is further illustrated by way of examples below, but the present invention is not limited to the scope of the embodiments described. The experimental methods in the following examples that do not specify specific conditions are selected according to conventional methods and conditions, or according to the product specifications. Unless otherwise specified, the reagents and raw materials used in the present invention are commercially available.
[0078] Example 1
[0079] This embodiment provides a lithium ion battery, and the preparation method of the lithium ion battery is as follows:
[0080] (1) Preparation of positive electrode
[0081] The positive electrode active material LiNi 0.5 Mn 1.5 O4, conductive agent acetylene black and binder polyvinylidene fluoride are fully stirred and mixed in an N-methylpyrrolidone solvent system in a mass ratio of 95:3:2 to obtain a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil, dried, cold pressed and cut to obtain a positive electrode.
[0082] (2) Preparation of negative electrode
[0083] The negative electrode active material graphite, the conductive agent acetylene black, the binder styrene butadiene rubber and the thickener sodium carbon methyl cellulose are fully stirred and mixed in a deionized water solvent system in a mass ratio of 96:2:1:1 to obtain a negative electrode slurry, and the negative electrode slurry is coated on a copper foil, dried, cold pressed and cut to obtain a negative electrode.
[0084] (3) Preparation of diaphragm
[0085] A polyethylene with a thickness of 9 μm was used as a base film, and a nano-aluminum oxide coating with a thickness of 3 μm was coated on the base film to obtain a separator.
[0086] (4) Preparation of electrolyte
[0087] The electrolyte is prepared by the following preparation method: the electrolyte is prepared in a glove box, the nitrogen content in the glove box is 99.999%, the actual oxygen content in the glove box is 0.1 ppm, and the water content is 0.1 ppm; the components of the carbonate as a non-aqueous solvent are mixed evenly, the mononitrile compound and the fluorine-containing compound are added, mixed evenly, and then the lithium salt is added and mixed evenly. The electrolyte of this embodiment is a non-aqueous electrolyte, which includes 8% of n-valeronitrile, 30% of trifluoromethylbenzene, and the lithium salt is lithium hexafluorophosphate with a concentration of 1 mol / L. The remainder is a carbonate as a non-aqueous solvent, and the carbonate is composed of ethylene carbonate and ethyl methyl carbonate in a mass ratio of 3:7.
[0088] (5) Assembling batteries
[0089] The positive electrode, the separator, and the negative electrode are stacked in order, so that the separator is between the positive electrode and the negative electrode to play an isolating role, and the sheets are stacked to obtain a bare cell. The bare cell is loaded into an aluminum-plastic film, and then baked at 80°C to remove water, and then the electrolyte is injected and sealed. After standing, hot and cold pressing, formation, clamping, and capacity division, a finished soft-package lithium-ion battery is obtained. The energy density of the lithium-ion battery prepared in this embodiment is 263Wh / kg.
[0090] Embodiment 2-5
[0091] The contents of n-valeronitrile in the electrolytes of Examples 2-5 are 0.1%, 0.3%, 20% and 25% respectively, and the other conditions are the same as those of Example 1.
[0092] Embodiment 6-9
[0093] The contents of trifluoromethylbenzene in the electrolytes of Examples 6-9 are 10%, 15%, 50% and 60% respectively, and the other conditions are the same as those of Example 1.
[0094] Examples 10-12
[0095] The mononitrile compounds in the electrolytes of Examples 10-12 are monofluoroacetonitrile, isovaleronitrile and n-hexanenitrile, respectively, and the other conditions are the same as those of Example 1.
[0096] Examples 13-15
[0097] The fluorine-containing compounds in the electrolytes of Examples 13-15 are bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate and 2,2,2-trifluoroethyl acetate, respectively, and the other conditions are the same as those of Example 1.
[0098] Example 16
[0099] The fluorine-containing compound in the electrolyte of Example 16 is 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and the content is 25%. The other conditions are the same as those of Example 1.
[0100] Embodiment 17
[0101] The fluorine-containing compound in the electrolyte of Example 17 is decafluoropentane, and the content is 25%. The other conditions are the same as those of Example 1.
[0102] Embodiment 18
[0103] 0.5% of triallyl isocyanurate is added as an additive to the electrolyte of Example 18. When the electrolyte is prepared, the additive is added together with the mononitrile compound and the fluorine-containing compound. The other conditions are the same as those of Example 1.
[0104] Embodiment 19
[0105] 0.1% of dicyclohexylcarbodiimide was added as an additive to the electrolyte of Example 19. When the electrolyte was prepared, the additive was added together with the mononitrile compound and the fluorine-containing compound. The other conditions were the same as those of Example 1.
[0106] Embodiment 20
[0107] The electrolyte of Example 20 also includes 10% dimethyl carbonate. When preparing the electrolyte, dimethyl carbonate is mixed with ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate as one of the components of the carbonate. The other conditions are the same as those of Example 1.
[0108] Embodiment 21
[0109] The positive electrode active material in Example 21 is LiNi 0.5 Mn 1.48 Fe 0.02 O4, the other conditions are the same as in Example 1.
[0110] Embodiment 22
[0111] The positive electrode active material in Example 22 is LiNi 0.5 Mn 1.47 Zr 0.03 O4, the other conditions are the same as in Example 1.
[0112] Embodiment 23
[0113] The positive electrode active material in Example 23 is LiNi 0.5 Mn 1.45 Al 0.05 O4, the other conditions are the same as in Example 1.
[0114] Comparative Example 1
[0115] In this comparative example, except that the electrolyte does not contain n-valeronitrile and trifluoromethylbenzene, other conditions are the same as those of Example 1.
[0116] Comparative Example 2
[0117] In this comparative example, except that the electrolyte does not contain trifluoromethylbenzene, other conditions are the same as those of Example 1.
[0118] Comparative Example 3
[0119] Except that the electrolyte does not contain n-valeronitrile, the other conditions of this comparative example are the same as those of Example 1.
[0120] Comparative Example 4
[0121] In the electrolyte of this comparative example, the content of n-valeronitrile is 0.05%, and the other conditions are the same as those in Example 1.
[0122] Comparative Example 5
[0123] In the electrolyte of this comparative example, the content of trifluoromethylbenzene is 5%, and the other conditions are the same as those in Example 1.
[0124] Comparative Example 6
[0125] In the electrolyte of this comparative example, the content of n-valeronitrile is 28%, the content of trifluoromethylbenzene is 62%, and the other conditions are the same as those in Example 1.
[0126] Comparative Example 7
[0127] In the electrolyte of this comparative example, the n-valeronitrile in Example 1 is replaced by adiponitrile, and the other conditions are the same as those in Example 1.
[0128] Comparative Example 8
[0129] In the electrolyte of this comparative example, the trifluoromethylbenzene in Example 1 is replaced by toluene, and the other conditions are the same as those in Example 1.
[0130] Comparative Example 9
[0131] In the electrolyte of this comparative example, the fluorine-containing compound is bis(2,2,2-trifluoroethyl) carbonate, and the other conditions are the same as those in Example 1.
[0132] Comparative Example 10
[0133] The positive electrode active material of this comparative example is NCM (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), and the other conditions are the same as those in Example 1. The energy density of the lithium ion battery prepared in this comparative example is 250Wh / kg.
[0134] Comparative Example 11
[0135] The positive electrode active material of this comparative example is NCM (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), and the other conditions are the same as those in Comparative Example 1. The energy density of the lithium-ion battery prepared in this comparative example is 250Wh / kg.
[0136] Effect Example 1: Cyclic Capacity Retention Rate at Room Temperature (25°C)
[0137] At 25°C, the lithium-ion battery is charged to 4.85V at a constant current of 1C, then charged to a current of less than 0.05C at a constant voltage of 4.85V, and after being left for 10 minutes, it is discharged to 3.5V at a constant current of 1C. The discharge capacity of the lithium-ion battery at this time is tested, which is the discharge capacity of the first cycle; the lithium-ion battery is cycled multiple times under the above conditions, and the discharge capacity corresponding to 400 cycles is recorded. The capacity retention rate after 400 cycles is calculated according to the following formula:
[0138] Capacity retention rate (%) = (discharge capacity corresponding to 400 cycles / discharge capacity of the first cycle) × 100%.
[0139] The above tests were performed on the lithium ion batteries prepared in Examples 1-23 and Comparative Examples 1-11, respectively. The test results are shown in Table 1.
[0140] Table 1
[0141]
[0142] Effect Example 2: DCR Growth Rate at 50% SOC
[0143] Adjust the temperature of the incubator to a constant 25°C, let it stand for 10 minutes, charge the lithium-ion battery to 4.85V at a constant current of 0.33C, then keep the voltage constant to 0.05C, let it stand for 10 minutes, and discharge it to 3.5V at 0.33C to obtain the theoretical capacity of the battery; then charge it to 4.85V at a constant current of 0.33C, then keep the voltage constant to 0.05C, let it stand for 10 minutes, and discharge it at 0.33C to adjust the capacity to 50%SOC. After standing for 1 hour, record the initial voltage V1 of the battery. Then discharge the battery at a current I0 of 4C for 30s, and record the battery voltage V2 after discharge. Calculate the DCR of the battery at 50% SOC according to the following formula:
[0144] DCR(mΩ)=(V1-V2) / I0
[0145] The lithium-ion battery was cycled 400 times according to the conditions in Example 1, and the DCR of the battery was recorded before and after the cycle, which were DCR0 and DCR1, respectively. The DCR growth rate of the battery after 400 cycles was calculated according to the following formula:
[0146] DCR inc.(%)=(DCR1-DCR0) / DCR0
[0147] The above tests were performed on the lithium ion batteries prepared in Examples 1-23 and Comparative Examples 1-11, respectively. The test results are shown in Table 1.
[0148] As can be seen from Table 1, in the embodiment of the present invention, lithium nickel manganese oxide is used as the positive electrode active material, and the electrolyte contains a specific content of mononitrile compounds and a specific type and content of fluorinated compounds. The prepared lithium ion battery has excellent cycle stability and rate performance at a high operating voltage (4.85V), specifically: the capacity retention rate of 400 cycles at 25°C is above 80%, and in some preferred embodiments it can reach above 90%; the DCR growth rate of 400 cycles at 25°C is below 100%, in some preferred embodiments it can reach below 50%, in more preferred embodiments it can reach below 20%, and even below 10%.
[0149] According to Comparative Examples 1-3, when the electrolyte does not contain a mononitrile compound and a fluorine-containing compound, or contains only one of the components, the cycle stability and rate performance of the obtained lithium ion battery are poor. According to Comparative Examples 4-6, even if the mononitrile compound and the fluorine-containing compound of the present invention are contained at the same time, if the contents of the two are not within the scope of the present invention, for example, the content of one component is too low or the contents of the two components are too high, the cycle capacity retention rate of the finally obtained lithium ion battery will be greatly reduced, and the DCR growth rate will be greatly increased.
[0150] The cyano functional group of the mononitrile compound has good coordination ability, and can be complexed and coordinated with the manganese ions in the positive electrode of lithium nickel manganese oxide, passivating it and inhibiting the dissolution of manganese ions; At the same time, the mononitrile compound has low viscosity and good lithium salt dissociation ability, which can greatly improve the dynamics of the battery. However, the effect of the mononitrile compound on the cycle performance and rate performance of lithium ion batteries is not a simple linear correspondence. According to Examples 1-5, when only the content of n-valeronitrile changes and other conditions remain unchanged, when the content of n-valeronitrile is 8%, the cycle capacity retention rate is the highest and the DCR growth rate is the lowest, and when the content of n-valeronitrile is low or high, the cycle capacity retention rate and the DCR growth rate are either increased or decreased, and there is no obvious regularity.
[0151] Furthermore, if the mononitrile compound of the present invention is replaced by a polynitrile compound, such as in Comparative Example 7, where n-valeronitrile is replaced by adiponitrile on the basis of Example 1, the cycle capacity retention rate of the prepared lithium ion battery is ultimately greatly reduced, and the DCR growth rate is greatly increased.
[0152] Fluorinated compounds have excellent oxidation stability due to the effect of fluorine atoms. Adding fluorinated solvents to the electrolyte can reduce the electrochemical reactivity of active components at high voltages, improve the overall antioxidant capacity of the electrolyte, and greatly reduce the oxidative decomposition side reactions of the electrolyte. If the fluorinated compounds of the present invention are replaced with non-fluorinated compounds with similar structures, such as Comparative Example 8, excellent cycle stability and rate performance at high operating voltages cannot be achieved. However, not all fluorinated compounds can achieve the technical effects of the present invention. If the fluorinated compounds of the present invention are replaced with other types of fluorinated compounds, such as Comparative Example 9, excellent cycle stability and rate performance at high operating voltages cannot be achieved. Similarly, the effects of fluorinated compounds on the cycle performance and rate performance of lithium-ion batteries are not simply linearly corresponding. According to Examples 1 and 6-9, when only the content of fluorine-containing compounds changes while other conditions remain unchanged, when the content of trifluoromethylbenzene is 30%, the cycle capacity retention rate is the highest and the DCR growth rate is the lowest, while when the content of trifluoromethylbenzene is lower or higher, the cycle capacity retention rate and the DCR growth rate either increase or decrease, with no obvious regularity.
[0153] Comparing Example 1 with Example 15, it can be seen that the performance of the fluorocarboxylic acid ester (2,2,2-trifluoroethyl acetate) in terms of capacity retention and DCR growth rate is slightly worse than that of trifluoromethylbenzene.
[0154] By comparing Example 1 with Examples 18 and 19, it can be seen that, on the basis of Example 1, if an additive having a film-forming effect is further added, the cycle stability and rate performance can be further improved.
[0155] From the perspective of non-aqueous solvents, dimethyl carbonate is not preferred in the system of the present invention. Even if dimethyl carbonate is contained, its content needs to be controlled to be no more than 5%. According to Example 20, compared with Example 1, 10% dimethyl carbonate is used in the electrolyte, and the cycle capacity retention rate of the lithium ion battery finally obtained is lower than that of Example 1, while the DCR growth rate is improved.
[0156] In addition, the specific non-aqueous electrolyte of the present invention is developed for lithium nickel manganese oxide positive electrode materials and is used in conjunction with lithium nickel manganese oxide positive electrode materials. 0.5 Mn 1.5 The lithium-ion battery prepared with O4 as the positive electrode material has excellent cycle stability and rate performance at a high working voltage (4.85V). In Examples 21-23, lithium nickel manganese oxide positive electrode materials LiNi 0.5 Mn 1.48 Fe 0.02 O4、LiNi 0.5 Mn 1.47 Zr0.03 O4 and LiNi 0.5 Mn 1.45 Al 0.05 The lithium-ion battery made of O4 also has excellent cycle stability and rate performance, with a capacity retention rate of more than 90% and a DCR growth rate of less than 15%. However, according to Comparative Example 11, for lithium-ion batteries using NCM as the positive electrode material, if a conventional electrolyte (not containing mononitrile compounds and fluorinated compounds) is used, the battery cycle capacity retention rate is 71.6% and the DCR growth rate is 144.8%; if the electrolyte of Example 1 is used in the NCM positive electrode material (as shown in Comparative Example 10), the cycle capacity retention rate increases slightly (75.1%), and the DCR growth rate decreases slightly (135.2%), but the degree of increase or decrease is very low. Compared with Comparative Example 1, the cycle capacity retention rate of Example 1 of the present invention is greatly improved, and the DCR growth rate is greatly reduced. It can be seen that there is a certain synergistic relationship between the non-aqueous electrolyte of the present invention and the lithium nickel manganese oxide positive electrode material.
[0157] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A lithium ion battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, characterized in that: The electrolyte is a non-aqueous electrolyte, which includes a mononitrile compound and a fluorinated compound, wherein the content of the mononitrile compound is 0.1%-25%, and the percentage is the mass percentage of the mononitrile compound in the non-aqueous electrolyte; the content of the fluorinated compound is 10%-60%, and the percentage is the mass percentage of the fluorinated compound in the non-aqueous electrolyte; the fluorinated compound is selected from one or more of trifluoromethylbenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate, decafluoropentane and acetic acid-2,2,2-trifluoroethyl ester; the mononitrile compound is selected from one or more of monofluoroacetonitrile, n-butyronitrile, isobutyronitrile, n-valeronitrile, isovaleronitrile and n-hexanenitrile; The positive electrode includes a positive electrode active material layer, the positive electrode active material layer includes lithium nickel manganese oxide, and the chemical formula of the lithium nickel manganese oxide is Li x Ni y Mn 2-y-m M m O4, wherein 0.9≤x≤1.1, 0.3≤y≤0.8, 0≤m≤0.1, M is one or more of Fe, Ti, Co, Cr, V, Cu, Zn, Zr, Al and Nb; the content of the lithium nickel manganese oxide is 50%-98.5%, and the percentage is the mass percentage of the lithium nickel manganese oxide in the positive electrode active material layer.
2. The lithium-ion battery according to claim 1, characterized in that The mononitrile compound is monofluoroacetonitrile, n-valeronitrile, isovaleronitrile or n-hexanenitrile; the fluorinated compound is trifluoromethylbenzene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, bis(2,2,2-trifluoroethyl) ether, trifluoroethyl methyl carbonate, decafluoropentane or 2,2,2-trifluoroethyl acetate.
3. The lithium-ion battery according to claim 1, characterized in that The non-aqueous electrolyte also includes an additive, which is selected from one or more of triallyl isocyanurate, dicyclohexylcarbodiimide, 1,6-hexamethylene diisocyanate and lithium difluorobisoxalate phosphate, and the content of the additive is 0.01%-2%, where the percentage is the mass percentage of the additive in the non-aqueous electrolyte.
4. The lithium-ion battery according to claim 1, characterized in that: The content of the mononitrile compound is 8%-20%; the content of the fluorinated compound is 25%-50%.
5. The lithium-ion battery according to claim 1, characterized in that: The non-aqueous electrolyte includes carbonate, and the carbonate includes one or more of ethylene carbonate, ethyl methyl carbonate, propylene carbonate and diethyl carbonate; the content of the carbonate is 5%-65%, and the percentage is the mass percentage of the carbonate in the non-aqueous electrolyte.
6. The lithium-ion battery according to claim 1, characterized in that The non-aqueous electrolyte includes dimethyl carbonate, and the content of the dimethyl carbonate does not exceed 5%, where the percentage is the mass percentage of the dimethyl carbonate in the non-aqueous electrolyte.
7. The lithium-ion battery according to claim 1, characterized in that: The non-aqueous electrolyte includes a lithium salt, and the lithium salt includes one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate), lithium difluorooxalatoborate, lithium difluorophosphate and lithium trifluoromethylsulfonate.
8. The lithium-ion battery according to claim 1, characterized in that The positive electrode active material layer further includes one or more of lithium iron phosphate, lithium manganese iron phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide.