A method for simultaneously improving water permeation flux and desalination rate of polyamide separation membrane and its application

By changing the contact mode between water and oil in the polymerization process, and adjusting the polyamide separation layer structure by using flow shear force and rotational friction force, the problem of difficult to take into account both the water permeability and desalination rate of the polyamide separation membrane in the prior art is solved. , realizes the preparation and wide application of high-performance films.

CN118320648BActive Publication Date: 2024-11-22ZHEJIANG UNIV
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
CN202410270586.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2024-11-22
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

The existing polyamide separation membranes are difficult to simultaneously increase the water permeability flux while ensuring the desalination rate, and the traditional interface polymerization process is difficult to control, resulting in limited membrane performance.

Method used

By changing the contact method between water and oil during interface polymerization, the oil phase cross-flow or membrane rotation contact method is used to adjust the structure of the polyamide separation layer by using flow shear force and rotation friction force, reducing the thickness and defects of the separation layer, and improving the Water permeability flux and salt retention rate of the membrane.

Benefits of technology

The water permeability flux of the polyamide separation membrane has been increased by 50%-150%, and the salt retention rate has been increased by 5%-50%. The process flow has been simplified and equipment requirements have been reduced. It is suitable for seawater desalination and bitter salt water desalination. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118320648B_ABST
    Figure CN118320648B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane and its application, and relates to the technical field of water treatment membranes. The present invention aims at the shortcomings of a polyamide separation membrane prepared by a traditional interfacial polymerization method, that is, a thick separation layer and many defects. The structure of the polyamide separation layer is adjusted by changing the contact mode of the water-oil two-phases during the interfacial polymerization process, and the flow shear force of the oil phase solution during cross-flow or the shear force between the membrane and the solution during rotation is used to reduce the generation of defects in the separation layer, reduce the thickness of the separation layer, and reduce the water permeation resistance, thereby simultaneously improving the water permeation flux and desalination rate of the polyamide separation membrane. The method of the present invention has low equipment requirements and a simple preparation process, and is easy to improve on the basis of the traditional polyamide separation membrane preparation process to achieve amplified preparation and production. The prepared polyamide separation membrane has broad application prospects in the field of water treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment membranes, and in particular to a method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane and an application thereof. Background Art

[0002] Membrane separation technology has been widely used in seawater desalination, food industry, biomedicine, municipal wastewater treatment and other fields due to its advantages of high processing efficiency, low energy consumption and low economic cost. Among the many membrane technologies, reverse osmosis and nanofiltration technologies have relatively higher separation accuracy than other pressure-driven membrane technologies because the separation process does not involve phase change, and have always been the top priority of membrane technology research. Membrane materials are the core of membrane technology. Since the separation process is pressure-driven, its operating pressure must be greater than the osmotic pressure of the solution, so its energy consumption is difficult to reduce by conventional methods. Therefore, under the same operating conditions, while ensuring a certain high desalination rate, improving the water permeation flux of the polyamide separation membrane is an inevitable choice to reduce operating costs. In order to promote energy conservation, environmental protection and sustainable development of the industry, it is imperative to further develop high-performance polyamide separation membranes.

[0003] At present, most commercial desalination membrane materials are composite structures of aromatic polyamides, which are three-layer structures from top to bottom, namely, polyamide separation layer, porous support layer and non-woven fabric substrate. Among them, the polyamide separation layer plays a vital role in the separation performance of the membrane (i.e., water flux and salt retention rate), while the porous support layer and non-woven fabric substrate are usually used as carriers of the separation layer to improve the mechanical stability of the composite membrane. The polyamide separation layer is usually prepared by the interfacial polymerization reaction of aqueous polyamines and organic polyacyl chlorides in water and oil phases. Due to the competitive relationship between the amide polymerization reaction and the acyl chloride hydrolysis reaction, the polyamide separation layer prepared by the interfacial polymerization reaction has a "trade-off" effect between permeability and selectivity, that is, the water flux and salt retention rate of the membrane cannot be taken into account, thereby limiting the further application of polyamide separation membranes. Therefore, under the premise of ensuring the desalination rate of the polyamide separation membrane, improving the water flux of the membrane is the key challenge facing the current research on polyamide separation membranes.

[0004] In recent years, most studies have focused on adjusting the parameters of the interfacial polymerization process to optimize the structure and properties of the polyamide separation layer, such as reactive monomers, reaction time, temperature, solution concentration, etc.

[0005] For example, the patent document with publication number CN104781001A discloses a polyamide water treatment separation membrane with high desalination rate and high flux properties and a preparation method thereof. The invention forms an aqueous solution layer containing amine compounds on a porous support; a polyamide active layer is formed by bringing an organic solution containing an acyl halide compound and a first organic solvent into contact with the aqueous solution layer; a second organic solvent with lower volatility than the first organic solvent is coated on the polyamide active layer, resulting in a secondary polymerization reaction, thereby forming a polyamide water treatment separation membrane with excellent desalination rate and high permeation flux properties.

[0006] A Chinese patent document with publication number CN114534491A discloses a high water flux reverse osmosis membrane and its preparation method and application. The invention carries out an amino grafting reaction on a porous support membrane to prepare a reactive support membrane; then an aqueous phase solution and an oil phase solution containing a polyacyl chloride oil phase monomer are subjected to interfacial polymerization on the reactive support membrane to prepare a high water flux reverse osmosis membrane.

[0007] However, in the above methods, new raw materials need to be introduced and operating procedures need to be increased. The water-oil two-phase solution is used as the reaction medium, and the interface where the two phases contact each other is bound to have a huge impact on the interfacial polymerization process. The traditional interfacial polymerization process generally adopts a method of static contact of the two-phase solution, and the degree of reaction is controlled by adjusting the contact time. However, the interfacial polymerization reaction speed is extremely fast and the influencing factors are complex. It is difficult to obtain a polyamide separation layer with excellent performance by simply controlling the contact time of the two-phase solution. Therefore, by changing the contact method of the two-phase solution of the traditional interfacial polymerization process, it is expected that the polyamide separation layer structure formed can be optimized to achieve an increase in the water permeation flux of the polyamide membrane. Summary of the invention

[0008] In order to improve the water permeation flux of a polyamide separation membrane and increase its desalination rate at the same time, the present invention provides a method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane. The method has a simple process and is easy to scale up for production. The prepared polyamide separation membrane has high water permeation flux and good desalination rate.

[0009] The specific technical solutions adopted are as follows:

[0010] A method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane, comprising:

[0011] S01 placing the porous support membrane in static contact with an aqueous solution containing a polyamine monomer, and then removing excess liquid on the membrane surface;

[0012] S02 The oil phase solution containing the polyacyl chloride monomer flows in a direction parallel to the membrane surface to contact the membrane surface treated in step S01, and after the polyamine monomer and the polyacyl chloride monomer undergo interfacial polymerization reaction, the excess liquid on the membrane surface is removed; after heat treatment, a polyamide separation membrane is prepared;

[0013] In step S02, during the flow contact, the flow rate of the oil phase solution containing the polyacyl chloride monomer is constant.

[0014] Alternatively, a method for simultaneously improving the water permeation flux and the salt rejection rate of a polyamide separation membrane comprises:

[0015] S11 placing the porous support membrane in contact with an aqueous solution containing a polyamine monomer, and then removing excess liquid;

[0016] S12: the membrane treated in step S11 is coated on a roller, and the roller coated with the membrane is immersed in an oil phase solution containing polyacyl chloride monomers, and the roller is operated at a constant speed. After the polyamine monomers and the polyacyl chloride monomers undergo interfacial polymerization reaction, the excess liquid on the membrane surface is removed; after heat treatment, a polyamide separation membrane is prepared.

[0017] The present invention aims to address the shortcomings of a polyamide separation membrane prepared by a traditional interfacial polymerization method, such as a large separation layer thickness and many defects. The structure of the polyamide separation layer is adjusted by changing the contact mode between the water and oil phases during the interfacial polymerization process, and the flow shear force of the oil phase solution during cross-flow or the shear force between the membrane and the solution during rotation is utilized to reduce the generation of defects in the separation layer and reduce the thickness of the separation layer, thereby achieving the preparation of a high-performance polyamide separation membrane.

[0018] The porous support membrane is selected from polysulfone ultrafiltration membrane, polyethersulfone ultrafiltration membrane, polyacrylonitrile ultrafiltration membrane, polytetrafluoroethylene ultrafiltration membrane, polypropylene ultrafiltration membrane, polyethylene ultrafiltration membrane, polystyrene ultrafiltration membrane, polyimide ultrafiltration membrane, polyvinyl chloride ultrafiltration membrane or hydrolyzed polyacrylonitrile ultrafiltration membrane.

[0019] The polyamine monomer is at least one of m-phenylenediamine, o-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, xylene diamine, ethylenediamine, propylenediamine, tris(2-aminoethyl)amine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, and 2,6-dimethylpiperazine.

[0020] Preferably, in step S01 or step S11, the static contact time is 1-10 min; the static contact method is: pouring the aqueous solution containing the polyamine monomer on the surface of the porous support membrane and letting it stand, or immersing the porous support membrane in the aqueous solution containing the polyamine monomer.

[0021] The polyvalent acyl chloride monomer is at least one of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, pyromellitoyl chloride, malonyl chloride, glutaryl chloride and fumaroyl chloride.

[0022] The solvent of the oil phase solution includes, but is not limited to, n-hexane, cyclohexane, n-heptane, toluene, benzene, isopar G, isopar E, isopar H, isopar L or isopar M.

[0023] Preferably, in the aqueous phase solution, the content of the polyamine monomer is 0.05-2 wt %; in the oil phase solution, the content of the polyacyl chloride monomer is 0.05-2 wt %.

[0024] Preferably, in step S02, the oil phase solution containing polyacyl chloride monomers is made to flow in a direction parallel to the membrane surface by means of a pump to contact the membrane surface treated in step S01, the flow rate of the oil phase solution containing polyacyl chloride monomers is 1-3 LPM, and the interfacial polymerization reaction time is 1-5 min.

[0025] The pump includes but is not limited to a peristaltic pump, a gear pump, a diaphragm pump, a centrifugal pump or a vane pump.

[0026] Preferably, in step S12, the rotation speed of the roller is 10-100 r / min, and the interfacial polymerization reaction time is 1-5 min.

[0027] Preferably, the heat treatment conditions are 50-80°C, 10-20 min.

[0028] The present invention also provides the application of the method for simultaneously improving the water permeation flux and desalination rate of the polyamide separation membrane in the field of water treatment, especially in the fields of seawater desalination, brackish water desalination, etc.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The present invention improves the problem of poor controllability of the traditional interfacial polymerization two-phase static contact reaction by constructing a contact mode of relative movement between the water and oil phases. In the early stage of the interfacial polymerization reaction, the polyamide primary layer is gradually formed, and the oil phase contacts the membrane surface at a certain relative flow rate, which can ensure that sufficient oil phase monomers participate in the reaction, repair the defects in the polyamide separation layer caused by incomplete reaction, make the formed polyamide membrane denser, and thus improve the salt retention rate of the membrane.

[0031] (2) The oil phase cross-flow process can exert a certain shear force on the reaction interface, reduce the diffusion rate of the subsequent unreacted polyamine monomers into the oil phase, improve the self-limiting nature of the reaction, limit the further growth of the polyamide layer, effectively reduce the actual thickness of the polyamide separation layer, reduce the water permeation resistance, and improve the water permeation flux of the prepared polyamide separation membrane.

[0032] (3) When the membrane coated on the roller contacts the oil phase solution in a rotating manner, the rotational friction can cause a certain relative speed between the membrane and the oil phase, thereby reducing the size of the reaction zone of the interfacial polymerization and making the polyamide layer finally formed in the reaction zone relatively thin, thereby reducing the water permeation resistance and improving the water permeation flux of the polyamide separation membrane.

[0033] (4) The polyamide separation membrane prepared by the method of the present invention has a water permeation flux increased by 50%-150% and a salt retention rate increased by 5%-50% compared with the polyamide separation membrane prepared by the traditional interfacial polymerization method.

[0034] (5) The method of the present invention has low equipment requirements and a simple preparation process, and is easy to improve on the basis of the traditional polyamide separation membrane preparation process to achieve scaled-up preparation and production. The prepared polyamide separation membrane has broad application prospects in the field of water treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Schematic diagram of the oil phase cross-flow interfacial polymerization process.

[0036] Figure 2 Schematic diagram of the interfacial polymerization process of the film wrapped on the roller rotating in contact with the oil phase.

[0037] Figure 3 This is a SEM image of the surface of the polyamide separation membrane prepared based on the oil phase cross-flow interfacial polymerization method in Example 1.

[0038] Figure 4 This is a SEM image of the cross-section of the polyamide separation membrane prepared based on the oil phase cross-flow interfacial polymerization method in Example 1. DETAILED DESCRIPTION

[0039] The present invention will be further described below in conjunction with the embodiments and drawings. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0040] Specifically, the schematic diagram of the oil phase cross-flow interfacial polymerization process is as follows Figure 1 As shown in the figure, the schematic diagram of the polymerization process of the film wrapped on the roller rotating in contact with the oil phase interface is as follows Figure 2 shown.

[0041] Example 1

[0042] A commercial polysulfone ultrafiltration membrane was used as the porous support membrane. An aqueous solution containing 0.05 wt% piperazine was poured on the membrane surface. After standing for 1 min, the excess liquid on the membrane surface was removed. Subsequently, with the help of a peristaltic pump, a n-hexane solution containing 0.05 wt% trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 1 LPM and the contact area was 20 cm 2, allowing the piperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 1 minute, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 50°C for 10 minutes to obtain a polyamide separation membrane.

[0043] Example 2

[0044] A commercial polyethersulfone ultrafiltration membrane was used as the porous support membrane. An aqueous solution containing 2 wt% piperazine was poured on the membrane surface. After standing for 10 min, the excess liquid on the membrane surface was removed. Subsequently, with the help of a gear pump, a n-hexane solution containing 2 wt% trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 3 LPM and the contact area was 80 cm 2 , allowing the piperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 5 minutes, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 80°C for 20 minutes to obtain a polyamide separation membrane.

[0045] Example 3

[0046] A commercial polysulfone ultrafiltration membrane was used as the porous support membrane. An aqueous solution containing 1 wt% 2-methylpiperazine was poured on the membrane surface. After standing for 1 min, the excess liquid on the membrane surface was removed. Subsequently, with the help of a diaphragm pump, a n-hexane solution containing 1 wt% trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 2 LPM and the contact area was 50 cm 2 , allowing the 2-methylpiperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 1 minute, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 60°C for 15 minutes to obtain a polyamide separation membrane.

[0047] Example 4

[0048] A commercial polyethersulfone ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 0.05 wt% piperazine. After standing for 1 min, the membrane was fished out to remove excess liquid on the membrane surface. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in a n-hexane solution containing 0.05 wt% trimesoyl chloride. The roller was controlled to run at a speed of 10 r / min, and the contact area between the membrane and the oil phase solution was 20 cm 2 , allowing the piperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 1 minute, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 50°C for 10 minutes to obtain a polyamide separation membrane.

[0049] Example 5

[0050] A commercial polyacrylonitrile ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 2 wt% piperazine. After standing for 10 minutes, the membrane was fished out and the excess liquid on the membrane surface was removed. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in a n-hexane solution containing 1 wt% trimesoyl chloride. The roller was controlled to run at a speed of 100 r / min, and the contact area between the membrane and the oil phase solution was 80 cm 2 , allowing the piperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization for 5 minutes, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 80° C. for 20 minutes to obtain a polyamide separation membrane.

[0051] Example 6

[0052] A commercial polyacrylonitrile ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 1 wt% 2-methylpiperazine. After standing for 5 minutes, the membrane was fished out and the excess liquid on the membrane surface was removed. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in a n-hexane solution containing 1 wt% trimesoyl chloride. The roller was controlled to run at a speed of 50 r / min, and the contact area between the membrane and the oil phase solution was 80 cm 2 , allowing the 2-methylpiperazine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 5 minutes, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 80°C for 10 minutes to obtain a polyamide separation membrane.

[0053] Example 7

[0054] A commercial polyethersulfone ultrafiltration membrane was used as the porous support membrane. An aqueous solution containing 0.05 wt% of m-phenylenediamine was poured on the membrane surface. After standing for 10 min, the excess liquid on the membrane surface was removed. Subsequently, with the help of a peristaltic pump, a n-hexane solution containing 0.05 wt% of trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 1 LPM and the contact area was 20 cm 2 , allowing the m-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization for 5 minutes, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 80°C for 10 minutes to obtain a polyamide separation membrane.

[0055] Example 8

[0056] Using commercial polyethersulfone ultrafiltration membrane as the porous support membrane, an aqueous solution containing 2 wt% m-phenylenediamine was poured on the membrane surface. After standing for 1 min, the excess liquid on the membrane surface was removed. Subsequently, with the help of a peristaltic pump, a n-hexane solution containing 2 wt% trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 3 LPM and the contact area was 80 cm 2, allowing the m-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 5 minutes, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 50°C for 20 minutes to obtain a polyamide separation membrane.

[0057] Example 9

[0058] A commercial polyacrylonitrile ultrafiltration membrane was used as the porous support membrane. An aqueous solution containing 1 wt% o-phenylenediamine was poured on the membrane surface. After standing for 5 minutes, the excess liquid on the membrane surface was removed. Subsequently, with the help of a gear pump, a n-hexane solution containing 0.1 wt% trimesoyl chloride flowed in a direction parallel to the membrane surface to contact the membrane surface. The flow rate was 2 LPM and the contact area was 50 cm 2 , allowing the o-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization for 3 minutes, stopping the cross-flow and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 60°C for 15 minutes to obtain a polyamide separation membrane.

[0059] Example 10

[0060] A commercial polysulfone ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 0.05 wt% m-phenylenediamine. After standing for 1 min, the membrane was fished out to remove excess liquid on the membrane surface. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in a n-hexane solution containing 0.05 wt% trimesoyl chloride. The roller was controlled to run at a speed of 10 r / min, and the contact area between the membrane and the oil phase solution was 20 cm 2 , allowing the m-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 1 minute, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 50°C for 10 minutes to obtain a polyamide separation membrane.

[0061] Embodiment 11

[0062] A commercial polyethersulfone ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 2 wt% m-phenylenediamine. After standing for 10 min, the membrane was fished out to remove excess liquid on the membrane surface. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in a n-hexane solution containing 2 wt% trimesoyl chloride. The roller was controlled to run at a speed of 100 r / min, and the contact area between the membrane and the oil phase solution was 80 cm 2 , allowing the m-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization reaction for 5 minutes, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 80°C for 20 minutes to obtain a polyamide separation membrane.

[0063] Example 12

[0064] A commercial polysulfone ultrafiltration membrane was used as a porous support membrane. The porous support membrane was immersed in an aqueous solution containing 1 wt% o-phenylenediamine. After standing for 5 minutes, the membrane was fished out to remove excess liquid on the membrane surface. The obtained membrane was coated on a motorized roller, and the roller coated with the membrane was immersed in an isopar G solution containing 1 wt% trimesoyl chloride. The roller was controlled to run at a speed of 50 r / min, and the contact area between the membrane and the oil phase solution was 50 cm 2 , allowing the o-phenylenediamine monomer and the trimesoyl chloride monomer to undergo interfacial polymerization for 5 minutes, stopping the rotation and removing excess liquid on the membrane surface; and heat-treating the obtained membrane at 60°C for 15 minutes to obtain a polyamide separation membrane.

[0065] Comparative Example 1

[0066] A commercial polysulfone ultrafiltration membrane was used as a porous support membrane, and an aqueous solution containing 0.05 wt% piperazine was poured on the membrane surface. After standing for 1 minute, excess liquid on the membrane surface was removed. Subsequently, an n-hexane solution containing 0.05 wt% trimesoyl chloride was poured on the membrane surface, and the piperazine monomer and trimesoyl chloride monomer underwent interfacial polymerization reaction for 1 minute, and excess liquid on the membrane surface was removed. The obtained membrane was heat treated at 50°C for 10 minutes to obtain a polyamide separation membrane.

[0067] Comparative Example 2

[0068] A commercial polyethersulfone ultrafiltration membrane was used as a porous support membrane, and an aqueous solution containing 0.05 wt% of m-phenylenediamine was poured on the membrane surface. After standing for 10 minutes, excess liquid on the membrane surface was removed. Subsequently, an n-hexane solution containing 0.05 wt% of trimesoyl chloride was poured on the membrane surface. After interfacial polymerization reaction between m-phenylenediamine monomer and trimesoyl chloride monomer occurred for 5 minutes, excess liquid on the membrane surface was removed. The obtained membrane was heat treated at 80°C for 10 minutes to obtain a polyamide separation membrane.

[0069] Sample analysis

[0070] The microscopic morphology of the polyamide separation membrane prepared by the oil phase cross-flow interfacial polymerization method in Example 1 was analyzed, and the surface SEM results and cross-sectional SEM results were as follows: Figure 3 and Figure 4 As shown, the vesicle structure of the polyamide layer in the polyamide separation membrane prepared after oil phase cross-flow interfacial polymerization is smaller and more uniform, and the thickness of the polyamide layer is thinner.

[0071] The performance of the polyamide separation membranes prepared in Examples 1 to 6 and Comparative Example 1 was tested at room temperature using a cross-flow flat membrane performance evaluation device. The pure water flux of the polyamide separation membrane and the retention rate of a 2000 ppm Na2SO4 aqueous solution and a 2000 ppm NaCl aqueous solution were tested respectively (the test temperature was 25°C and the pressure was 5 bar). The results are shown in Table 1.

[0072] Table 1 Performance test results of polyamide separation membranes prepared in Examples 1 to 6 and Comparative Example 1

[0073]

[0074] The performance of the polyamide separation membranes prepared in Examples 7 to 12 and Comparative Example 2 was tested at room temperature using a cross-flow flat membrane performance evaluation device. The pure water flux of the polyamide separation membrane and the retention rate of a 2000 ppm Na2SO4 aqueous solution and a 2000 ppm NaCl aqueous solution were tested respectively (the test temperature was 25°C and the pressure was 15 bar). The results are shown in Table 2.

[0075] Table 2 Performance test results of polyamide separation membranes prepared in Examples 7 to 12 and Comparative Example 2

[0076]

[0077] It can be seen from the data in Table 1 and Table 2 that the method of the present invention can simultaneously improve the water permeation flux and the desalination rate of the polyamide separation membrane.

[0078] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane, characterized in that: include: S01 placing the porous support membrane in static contact with an aqueous solution containing a polyamine monomer, and then removing excess liquid on the membrane surface; S02 The oil phase solution containing the polyacyl chloride monomer flows in a direction parallel to the membrane surface to contact the membrane surface treated in step S01, and after the polyamine monomer and the polyacyl chloride monomer undergo interfacial polymerization reaction, the excess liquid on the membrane surface is removed; after heat treatment, a polyamide separation membrane is prepared; The porous support membrane is selected from polysulfone ultrafiltration membrane, polyethersulfone ultrafiltration membrane, polyacrylonitrile ultrafiltration membrane, polytetrafluoroethylene ultrafiltration membrane, polypropylene ultrafiltration membrane, polyethylene ultrafiltration membrane, polystyrene ultrafiltration membrane, polyimide ultrafiltration membrane, polyvinyl chloride ultrafiltration membrane or hydrolyzed polyacrylonitrile ultrafiltration membrane; In step S01, the static contact time is 1-10 minutes; the static contact method is: pouring the aqueous phase solution containing the polyamine monomer on the surface of the porous support membrane and letting it stand, or immersing the porous support membrane in the aqueous phase solution containing the polyamine monomer; In step S02, during the flow contact, the flow rate of the oil phase solution containing the polyacyl chloride monomers is constant, the flow rate of the oil phase solution containing the polyacyl chloride monomers is 1-3 LPM, and the interfacial polymerization reaction time is 1-5 min; In the aqueous phase solution, the content of the polyamine monomer is 0.05-2wt%; in the oil phase solution, the content of the polyacyl chloride monomer is 0.05-2wt%.

2. A method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane, characterized in that: include: S11 placing the porous support membrane in contact with an aqueous solution containing a polyamine monomer, and then removing excess liquid; S12: coating the film treated in step S11 on a roller, and immersing the roller coated with the film in an oil phase solution containing polyacyl chloride monomers, and operating at a constant speed, after the polyamine monomers and the polyacyl chloride monomers undergo interfacial polymerization, removing excess liquid on the membrane surface; and preparing a polyamide separation membrane after heat treatment; The porous support membrane is selected from polysulfone ultrafiltration membrane, polyethersulfone ultrafiltration membrane, polyacrylonitrile ultrafiltration membrane, polytetrafluoroethylene ultrafiltration membrane, polypropylene ultrafiltration membrane, polyethylene ultrafiltration membrane, polystyrene ultrafiltration membrane, polyimide ultrafiltration membrane, polyvinyl chloride ultrafiltration membrane or hydrolyzed polyacrylonitrile ultrafiltration membrane; In step S11, the static contact time is 1-10 minutes; the static contact method is: pouring the aqueous phase solution containing the polyamine monomer on the surface of the porous support membrane and letting it stand, or immersing the porous support membrane in the aqueous phase solution containing the polyamine monomer; In step S12, the rotation speed of the roller is 10-100 r / min, and the interfacial polymerization reaction time is 1-5 min; In the aqueous phase solution, the content of the polyamine monomer is 0.05-2wt%; in the oil phase solution, the content of the polyacyl chloride monomer is 0.05-2wt%.

3. The method for simultaneously improving the water permeation flux and the desalination rate of a polyamide separation membrane according to claim 1 or 2, characterized in that: The polyamine monomer is at least one of m-phenylenediamine, o-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, xylene diamine, ethylenediamine, propylenediamine, tris(2-aminoethyl)amine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, 2-methylpiperazine, 2,5-dimethylpiperazine, and 2,6-dimethylpiperazine.

4. The method for simultaneously improving the water permeation flux and the desalination rate of a polyamide separation membrane according to claim 1 or 2, characterized in that: The polyacyl chloride monomer is at least one of trimesoyl chloride, terephthaloyl chloride, phthaloyl chloride, pyromellitoyl chloride, malonyl chloride, glutaryl chloride, and fumaroyl chloride; the solvent of the oil phase solution includes n-hexane, cyclohexane, n-heptane, toluene, benzene, isopar G, isopar E, isopar H, isopar L, or isopar M.

5. The method for simultaneously improving the water permeation flux and the desalination rate of a polyamide separation membrane according to claim 1, characterized in that: In step S02, the oil phase solution containing the polyacyl chloride monomer is made to flow in a direction parallel to the membrane surface by means of a pump to contact the membrane surface treated in step S01.

6. The method for simultaneously improving the water permeation flux and desalination rate of a polyamide separation membrane according to claim 1 or 2, characterized in that: The heat treatment conditions are 50-80°C, 10-20min.

7. Use of the method for simultaneously improving the water permeation flux and the desalination rate of a polyamide separation membrane according to any one of claims 1 to 6 in the field of water treatment.

Citation Information

Patent Citations

  • Polyamide-based water-treatment separation membrane having excellent salt removal rate and permeation flux characteristics, and method for manufacturing same

    CN104781001A

  • Reverse osmosis membrane with high water flux as well as preparation method and application of reverse osmosis membrane

    CN114534491A

  • Process and device for removing monomeric components from the melt flow during melt spinning of polyamides

    CH321054A

  • High-throughput high-retention rate composite nanofiltration membrane preparation method

    CN105617888A

  • Aliphatic polyamide loose reverse osmosis membrane as well as preparation method and application thereof

    CN108246128A