A hydrotalcite-based carbonyl sulfide hydrolysis catalyst, preparation method and use thereof
The hydrotalcite-based composite metal oxide catalyst rich in surface oxygen defects solves the problems of short catalyst service life and unsatisfactory selectivity in the existing technology, and achieves efficient catalysis of carbonyl sulfide hydrolysis at low temperatures, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202410768053.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-14
AI Technical Summary
The existing technology has harsh reaction conditions, short catalyst service life, unsatisfactory selectivity and conversion rate during the catalytic hydrolysis of carbonyl sulfide, and it is difficult to obtain high conversion rate and high selectivity at the same time.
Using a hydrotalcite-based composite metal oxide catalyst rich in surface oxygen defects, the layered double metal hydroxide precursor is synthesized through the nucleation and crystallization isolation method, and is calcined in different atmospheres and temperatures to control the surface oxygen defect structure of the catalyst. , to improve catalytic activity and selectivity.
It achieves efficient catalysis of carbonyl sulfide hydrolysis at low temperature, extends the service life of the catalyst, improves the conversion rate and selectivity of the reaction, is suitable for industrial applications, and reduces the reaction temperature and energy consumption.
Smart Images

Figure CN118320811B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of desulfurization catalysts, and in particular to a hydrotalcite-based carbonyl sulfide hydrolysis catalyst, a preparation method and use thereof. Background Art
[0002] At room temperature and pressure, carbonyl sulfide is a colorless toxic gas with the smell of rotten eggs. It is commonly found in industrial gases such as yellow phosphorus tail gas, calcium carbide furnace tail gas, and natural gas. The clean utilization of blast furnace gas is a major demand for the country's sustainable development. Carbonyl sulfide in blast furnace gas will corrode equipment pipelines, and trace amounts of carbonyl sulfide can cause catalyst poisoning and deactivation, causing economic losses. If carbonyl sulfide is discharged into the atmosphere, acid rain will form and pollute the atmospheric environment. At the same time, when the concentration of carbonyl sulfide is greater than 20 mg / L, it will irritate the human upper respiratory system and endanger human health. "Deep desulfurization at the source" of blast furnace gas is currently the most effective technology for controlling ultra-low sulfur emissions. It is relatively easy to remove inorganic sulfur H2S from blast furnace gas, but organic sulfur carbonyl sulfide is difficult to remove due to its relatively stable chemical properties. The catalytic carbonyl sulfide hydrolysis method is an important unit of the "source deep desulfurization" technology of blast furnace gas. It has become a commonly used method for removing carbonyl sulfide in industry due to its mild reaction conditions, few side reactions, and the conversion of difficult-to-remove carbonyl sulfide into H2S, which is easier to remove. At present, the catalysts used for catalytic carbonyl sulfide hydrolysis are divided into two types: supported catalysts (usually with γ-Al2O3, TiO2 and activated carbon as carriers, and alkali metals, rare earth metals, metal oxides and hydroxides as active components for catalytic carbonyl sulfide hydrolysis) and solid base catalysts (mainly hydrotalcite-like and its derived oxides). The active components of supported catalysts are easy to lose, while solid base catalysts can directly catalyze the hydrolysis of carbonyl sulfide without loading active components, which has become a hot topic of research.
[0003] CN101690893A discloses a method for preparing a composite metal oxide by calcining nickel-aluminum hydrotalcite as a precursor to catalyze the hydrolysis of carbonyl sulfide, wherein the molar ratio of divalent metal ions to trivalent metal ions is 2+ / M 3+ =1-4, and the molar ratio between the two divalent metal ions is 0.25-1. The hydrotalcite-like substance is prepared by coprecipitation method, the pH is controlled at 8-10, and crystallization is carried out in a water bath at 40-80°C for 12 hours. The prepared hydrotalcite-like substance is calcined at 350-450°C in an air atmosphere for 2 hours. The hydrotalcite-like substance derived composite oxide catalyst is obtained. The activity test of the catalyst is carried out in a fixed bed reactor under the conditions that the reactor diameter is 8mm, the catalyst height is 4cm, the reaction temperature is 50°C, and the space velocity is 1000h -1 , carbonyl sulfide concentration is 1200mg / m 3, relative humidity is 2.4%, and activity is expressed by carbonyl sulfide hydrolysis removal rate and sulfur capacity. Compared with the prior art, the carbonyl sulfide hydrolysis catalyst of the invention has the advantages of being able to remove carbonyl sulfide in the gas and H2S produced by hydrolysis at the same time, with high desulfurization accuracy. However, it still has the disadvantages of harsh reaction conditions, short catalyst life, unsatisfactory selectivity and conversion rate.
[0004] In addition, during the carbonyl sulfide hydrolysis process, carbonyl sulfide and H2O compete for adsorption on the active sites on the catalyst surface, making it difficult to simultaneously obtain high conversion and high selectivity in the carbonyl sulfide hydrolysis reaction. The catalysts disclosed in the prior art that can simultaneously improve activity and selectivity are extremely limited. Therefore, providing a catalyst with mild reaction conditions, long life, high conversion and selectivity has become a technical problem to be solved urgently. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a hydrotalcite-based composite metal oxide carbonyl sulfide hydrolysis catalyst rich in surface oxygen defects. The catalyst forms a surface oxygen defect structure at the spinel position, which can promote the adsorption and activation of carbonyl sulfide and water on the catalyst surface, thereby being able to efficiently catalyze the hydrolysis of carbonyl sulfide at low temperature, so that the carbonyl sulfide hydrolysis reaction conditions using the catalyst of the present invention are mild, the catalyst activity is high, the service life is long, and it is more suitable for industrial applications.
[0006] The present invention provides a hydrotalcite-based composite metal oxide carbonyl sulfide hydrolysis catalyst rich in surface oxygen defects, wherein the catalyst is composed of ZnM2O4 or a mixture of ZnM2O4 and ZnO, wherein the divalent metal ion Zn 2+ and trivalent metal ions M 3+ The molar ratio is (0.5-0.9):1, and based on the total amount of oxygen elements on the catalyst surface as a percentage, the relative content of surface oxygen defects is 5-40%.
[0007] Further preferably, based on the total amount of oxygen elements on the catalyst surface as a percentage, the relative content of surface oxygen defects is 10.83-30.41%.
[0008] Furthermore, the catalyst uses a layered double metal hydroxide synthesized by a nucleation crystallization isolation method as a precursor, and the precursor is calcined to obtain a hydrotalcite-derived oxide catalyst rich in surface oxygen defects.
[0009] Furthermore, BET data showed that the specific surface area of the catalyst was 56.3-111.7 m 2 / g.
[0010] Furthermore, the defect structure of the catalyst was regulated by changing the calcination conditions of the ZnO and ZnAl2O4 mixture; the applicant conducted a sample comparison experiment by calcining the ZnO and ZnAl2O4 mixture at 450°C, 550°C, and 650°C for 2-8h in air and CO atmosphere, and the XRD test results showed that the products calcined in CO atmosphere had only a 2θ angle of 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 (220), (311), (422), (511), and (440) were observed at 31.7°, and no other peaks were observed except the characteristic peaks of spinel. o , 34.4 o , 36.2 o , 67.9 o The characteristic diffraction peaks of ZnO (100), (002), (101), and (112) appeared; therefore, the present application can achieve the presence of a specific spinel structure in the catalyst only under a specific formulation, a specific preparation method, and specific calcination conditions.
[0011] The present invention also provides a method for preparing the aforementioned hydrotalcite-derived oxide carbonyl sulfide hydrolysis catalyst rich in surface oxygen defects, the method comprising the following steps:
[0012] Step 1: Preparation of layered double hydroxides by nucleation crystallization isolation method
[0013] Weigh ZnCl2 and AlCl3∙6H2O in a beaker and dissolve them in deionized water and stir to mix them evenly to obtain a metal salt solution, in which Zn 2+ / Al 3+ The molar ratio is (1-4):1;
[0014] Weigh NaOH and Na2CO3 and dissolve them in deionized water in a beaker to obtain a mixed alkaline solution, wherein the molar ratio of NaOH to Na2CO3 is (6.4-16):1;
[0015] The uniformly mixed metal salt solution and the mixed alkali solution are simultaneously and rapidly poured into a colloid mill to obtain a slurry, and then the slurry is statically crystallized at 65-120° C. for 4-24 hours to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a layered double metal hydroxide. The XRD spectrum of the layered double metal hydroxide has a 2θ angle of 11.7 o , 23.6 o , 34.7 o , 39.3o , 46.9 o , 60.4 o and 61.8 o The characteristic diffraction peaks of hydrotalcite (003), (006), (012), (015), (018), (110) and (113) were clearly observed. Except for the characteristic peaks of hydrotalcite, no other diffraction peaks appeared.
[0016] Step 2: Calcination of the catalyst at different temperatures in a CO atmosphere to control the specific surface area and relative content of surface oxygen defects
[0017] The layered double hydroxide is weighed, tableted, granulated into 40-60 mesh, and calcined in a CO atmosphere, with the starting temperature being room temperature and the heating rate being 5-10° C. / min to reach the calcination temperature, the calcination temperature being 450-650° C., the calcination time being 4-6 h, and the CO gas flow rate being 10-50 mL / min, to obtain the carbonyl sulfide hydrolysis catalyst.
[0018] Furthermore, in step 1, in the metal salt solution, Zn 2+ The concentration is 0.05-0.2 mol / L, Al 3+ The concentration is 0.05-0.3mol / L.
[0019] Further, in step 1, in the alkaline solution, Na + The concentration is 0.36-0.42mol / L.
[0020] Furthermore, in step 1, the uniformly mixed metal salt solution and alkali solution are quickly poured into the colloid mill at the same time, the rotation speed of the colloid mill is controlled to be 5000-10000 rpm, the distance between the stator and the moving rotor is 300-600 nm, and the mixing time is 1-3 min.
[0021] Furthermore, in step 1, the precipitate is washed and then dried in an oven at 60-80° C. overnight.
[0022] The present invention also provides a use of the above-mentioned carbonyl sulfide hydrolysis catalyst for carbonyl sulfide hydrolysis reaction, wherein the catalyst is loaded into a reactor, the reaction temperature is controlled to be 30-60°C, a raw gas containing carbonyl sulfide gas and N2 is first introduced into a bubbler whose temperature is controlled by a water bath, and then the raw gas carrying water vapor is introduced into the reactor, the water bath temperature is controlled to be 30-70°C, and the reaction time is 10-30h, wherein the concentration of carbonyl sulfide in the introduced raw gas is 50-200mg / m 3 , the N2 is the balance gas, and the mass air velocity is set to 10000-48000h -1 , the product is hydrogen sulfide.
[0023] Furthermore, the reactor is a quartz fixed bed reactor with a length of 100-300 mm and an inner diameter of 3-8 mm.
[0024] Furthermore, the catalyst is first sieved through 40-60 meshes and then loaded into the U-tube reactor.
[0025] Furthermore, when the relative content of surface oxygen defects in the catalyst is 25.18%, the conversion rate of the carbonyl sulfide hydrolysis reaction is greater than 90%, and the concentration of product hydrogen sulfide measured by gas chromatography is greater than 30 mg / m 3 .
[0026] The beneficial effects of the present invention are as follows:
[0027] 1. The catalyst of the present invention is prepared by synthesizing a layered double hydroxide precursor by a nucleation crystallization isolation method, and calcining the layered double hydroxide precursor under different atmospheres and temperatures for comparison, thereby adjusting the relative content of surface oxygen defects to 5-40%. The surface oxygen defects unexpectedly significantly enhance the ability of the catalyst to activate water, while improving the activity and selectivity of the carbonyl sulfide hydrolysis reaction, and can operate stably without being easily deactivated, thus facilitating industrial applications.
[0028] 2. The catalyst of the present invention also has unexpected technical effects when applied in a specific reaction field. The present invention finds that by regulating the defect content and position of surface oxygen to an appropriate range, the hydrotalcite-based composite metal oxide carbonyl sulfide hydrolysis catalyst with surface oxygen defects improves the conversion rate of carbonyl sulfide reaction by about 20% compared with the hydrotalcite-based composite metal oxide carbonyl sulfide hydrolysis catalyst without surface oxygen defects, and the catalyst is used for the carbonyl sulfide catalytic reaction for the first time.
[0029] 3. The catalyst of the present invention has achieved innovative breakthroughs in specific reaction mechanisms. Compared with the prior art, the catalyst can effectively reduce the activation energy barrier of water molecules due to its unique defect structure, thereby promoting the dissociation of water molecules and producing more reactive OH. In addition, the metal-oxygen free radicals MO and OH on the surface of the catalyst work together to effectively activate carbonyl sulfide. By precisely regulating the reaction sites of activated water molecules and carbonyl sulfide on the catalyst surface, the catalyst of the present invention achieves a match between the activation rates of water molecules and carbonyl sulfide on the catalyst surface, thereby significantly improving the selectivity of the reaction while increasing the conversion rate of the reactants. This innovative design not only promotes the development of catalyst science, but also provides important technical support for the optimization of related industrial processes.
[0030] 4. The hydrotalcite-based composite metal oxide catalyst rich in surface oxygen defects used in the present invention has high activity, low energy consumption and milder conditions compared with the reaction temperature of 70-100°C used in other catalysts for hydrolysis of carbonyl sulfide in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 XRD diagram of the sample of the present invention
[0032] Figure 2 XPS diagram of the sample of the present invention
[0033] Figure 3 The EPR diagram of the sample of the present invention is
[0034] Figure 4 The conversion rate of carbonyl sulfide
[0035] Figure 5 The catalyst stability diagram DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be described in detail below in conjunction with specific embodiments of the present invention. The described embodiments are only a part of the present invention, and the present invention is not limited to the embodiments described below.
[0037] Example 1
[0038] A hydrotalcite-derived oxide carbonyl sulfide hydrolysis catalyst ZnM2O4 rich in surface oxygen defects, the divalent metal ion Zn 2+ and trivalent metal ions Al 3+ The molar ratio is 0.5, among which the relative content of surface oxygen defects is 25.18%.
[0039] The preparation method is as follows:
[0040] 8.2 g of ZnCl2 and 14.4 g of AlCl3∙6H2O were weighed and dissolved in 600 mL of deionized water, and stirred to mix evenly; 7.7 g of NaOH and 3.2 g of Na2CO3 were weighed and dissolved in 600 mL of deionized water; the uniformly mixed salt solution and alkaline solution were quickly poured into the colloid mill at the same time, the speed of the colloid mill was controlled to be 7000 rpm, the distance between the stator and the moving rotor was 500 nm, and the mixing time was 2 min; then the obtained slurry was placed in a hydrothermal autoclave, statically crystallized at 90°C for 4 h, and the precipitate was filtered, washed, and dried in an oven at 60°C overnight to obtain a layered double hydroxide sample 1;
[0041] Weigh 1 g of the layered double hydroxide sample 1, press it into tablets, granulate it into 40 mesh, and calcine it in a CO atmosphere at 550° C. for 4 h, with a heating rate of 5° C. / min, a heating time of 90 min, and a gas flow rate of 30 mL / min; calcine to obtain catalyst 1, named ZnAl2O4-550° C.-CO;
[0042] Carbonyl sulfide hydrolysis reaction: tested in a quartz fixed bed reactor with a length of 200 mm and an inner diameter of 5 mm, 0.05 g of the sieved catalyst 1 was weighed and loaded into a U-shaped tube, fixed with 1-3 μm heat-resistant quartz wool, the reaction temperature of the test was controlled by an intelligent cycle thermostat, the carbonyl sulfide component content was detected by a gas chromatograph GC-9720, and the tail gas was discharged after being treated by an absorption device;
[0043] Among them, the composition of the raw gas is: 100mg / m 3 Carbonyl sulfide, N2 as balance gas, mass space velocity 48000h -1 The activity test conditions of the catalyst 1 are: normal pressure, water bath temperature of 40°C, reaction temperature of 30-170°C, and reaction time of 1h;
[0044] The carbonyl sulfide conversion rate was 94%, and the concentration of product hydrogen sulfide was 31 mg / m 3 , the catalyst 1 has no obvious deactivation phenomenon.
[0045] Example 2
[0046] A mixture of ZnM2O4 and ZnO, a hydrotalcite-derived oxide rich in surface oxygen defects, is used as a catalyst for the hydrolysis of carbonyl sulfide. The divalent metal ion Zn in the catalyst is 2+ and trivalent metal ions Al 3+ The molar ratio is 0.6, wherein the relative content of surface oxygen defects is 20%.
[0047] The preparation method is as follows:
[0048] 8.92 g of ZnCl2 and 13.04 g of AlCl3∙6H2O were weighed and dissolved in 600 mL of deionized water, and stirred to mix evenly; 7.7 g of NaOH and 2.9 g of Na2CO3 were weighed and dissolved in 600 mL of deionized water; the uniformly mixed salt solution and alkaline solution were quickly poured into the colloid mill at the same time, the speed of the colloid mill was controlled to 7000 rpm, the distance between the stator and the moving rotor was 500 nm, and the mixing time was 2 min; then the obtained slurry was placed in a hydrothermal autoclave, statically crystallized at 90°C for 4 h, and the precipitate was filtered, washed, and dried in an oven at 60°C overnight to obtain layered double metal hydroxide sample 2;
[0049] Weigh 1 g of the layered double hydroxide sample 2, press it into tablets, granulate it into 40 mesh, and calcine it in a CO atmosphere at 550°C for 4 hours, with a heating rate of 5°C / min, a heating time of 90 minutes, and a gas flow rate of 30 mL / min; calcine to obtain catalyst 2, named ZnAl2O4 / ZnO-550°C-CO;
[0050] Carbonyl sulfide hydrolysis reaction: tested in a quartz fixed bed reactor with a length of 200 mm and an inner diameter of 5 mm, 0.05 g of the sieved catalyst 2 was weighed and loaded into a U-shaped tube, fixed with 1-3 μm heat-resistant quartz wool, the reaction temperature of the test was controlled by an intelligent cycle thermostat, the carbonyl sulfide component content was detected by a gas chromatograph GC-9720, and the tail gas was discharged after being treated by an absorption device;
[0051] Among them, the composition of the raw gas is: 100mg / m 3 Carbonyl sulfide, N2 as balance gas, mass space velocity 48000h -1 The activity test conditions of the catalyst 2 are: normal pressure, water bath temperature of 40°C, reaction temperature of 30-170°C, and reaction time of 1h;
[0052] The carbonyl sulfide conversion rate is 90%, and the concentration of product hydrogen sulfide is 25 mg / m 3 , the catalyst 2 has no obvious deactivation phenomenon.
[0053] Example 3
[0054] A mixture of ZnM2O4 and ZnO, a hydrotalcite-derived oxide rich in surface oxygen defects, is used as a catalyst for the hydrolysis of carbonyl sulfide. The divalent metal ion Zn in the catalyst is 2+ and trivalent metal ions Al 3+ The molar ratio is 0.7, among which the relative content of surface oxygen defects is 18%.
[0055] 9.54 g of ZnCl2 and 12.02 g of AlCl3∙6H2O were weighed and dissolved in 600 mL of deionized water, and stirred to mix evenly; 7.7 g of NaOH and 2.6 g of Na2CO3 were weighed and dissolved in 600 mL of deionized water; the uniformly mixed salt solution and alkaline solution were quickly poured into the colloid mill at the same time, the speed of the colloid mill was controlled to 7000 rpm, the distance between the stator and the moving rotor was 500 nm, and the mixing time was 2 min; then the obtained slurry was placed in a hydrothermal autoclave, statically crystallized at 90°C for 4 h, and the precipitate was filtered, washed, and dried in an oven at 60°C overnight to obtain layered double metal hydroxide sample three;
[0056] 1 g of the layered double hydroxide sample 3 was weighed, tableted, granulated into 40 mesh, and calcined at 550°C in a CO atmosphere for 4 h, with a heating rate of 5°C / min, a heating time of 90 min, and a gas flow rate of 30 mL / min; the catalyst 3 was obtained by calcination and named ZnAl2O4 / ZnO-550°C-CO;
[0057] Carbonyl sulfide hydrolysis reaction: tested in a quartz fixed bed reactor with a length of 200 mm and an inner diameter of 5 mm, 0.05 g of the sieved catalyst 3 was weighed and loaded into a U-shaped tube, fixed with 1-3 μm heat-resistant quartz wool, the reaction temperature of the test was controlled by an intelligent cycle thermostat, the carbonyl sulfide component content was detected by a gas chromatograph GC-9720, and the tail gas was discharged after being treated by an absorption device;
[0058] Among them, the composition of the raw gas is: 100mg / m 3 Carbonyl sulfide, N2 as balance gas, mass space velocity 48000h -1 The activity test conditions of the catalyst 3 are: normal pressure, water bath temperature of 40°C, reaction temperature of 30-170°C, and reaction time of 1h;
[0059] The carbonyl sulfide conversion rate was 88%, and the concentration of product hydrogen sulfide was 18 mg / m 3 , the catalyst 3 has no obvious deactivation phenomenon.
[0060] Comparative Example 1
[0061] 1 g of the layered double hydroxide sample 1 was weighed, tableted, granulated into 40 mesh, and calcined at 450°C in air atmosphere for 4 h, with a heating rate of 5°C / min, a heating time of 90 min, and a gas flow rate of 30 mL / min; the catalyst 4 was obtained by calcination and named ZnAl2O4 / ZnO-450°C-Air;
[0062] Carbonyl sulfide hydrolysis reaction: tested in a quartz fixed bed reactor with a length of 200 mm and an inner diameter of 5 mm, 0.05 g of the sieved catalyst 4 was weighed and loaded into a U-shaped tube, fixed with 1-3 μm heat-resistant quartz wool, the reaction temperature of the test was controlled by an intelligent cycle thermostat, the carbonyl sulfide component content was detected by a gas chromatograph GC-9720, and the tail gas was discharged after being treated by an absorption device;
[0063] Among them, the composition of the raw gas is: 100mg / m 3 Carbonyl sulfide, N2 as balance gas, mass space velocity 48000h -1 The activity test conditions of the catalyst 4 are: normal pressure, water bath temperature of 40°C, reaction temperature of 30-170°C, and reaction time of 1h;
[0064] The carbonyl sulfide conversion rate was 80.82%, and the concentration of product hydrogen sulfide was 20 mg / m 3 , the catalyst 4 is obviously deactivated.
[0065] The characteristics of the examples and comparative examples as well as the conversion rate of carbonyl sulfide hydrolysis and the concentration of product H2S are shown in the table below.
[0066]
[0067] Figure 1 This is the XRD diagram of the sample of the present invention.
[0068] Figure 1 (a) is the XRD test result of zinc-aluminum hydrotalcite prepared by nucleation crystallization isolation method. o , 23.6 o , 34.7 o , 39.3 o , 46.9 o , 60.4 o , and 61.8 o The characteristic diffraction peaks of hydrotalcite (003), (006), (012), (015), (018), (110) and (113) were clearly observed. Except for the characteristic peaks of hydrotalcite, no other diffraction peaks appeared, indicating that hydrotalcite with complete crystal form and no impurities was prepared.
[0069] Figure 1 (b) is the product calcined at 450℃ in air and CO atmosphere for 4h, respectively, and is denoted as ZnO / ZnAl2O4-450℃-Air and ZnO / ZnAl2O4-450℃-CO. In ZnO / ZnAl2O4-450℃-CO, the 2θ angle is 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 at (220), (311), (422), (511), and (440) were observed. In ZnO / ZnAl2O4-450℃-Air, except for the 2θ angle of 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 (220), (311), (422), (511), and (440) were observed at 2θ angle of 31.7. o , 34.4 o, 36.2 o , 67.9 o The characteristic diffraction peaks of ZnO (100), (002), (101), and (112) appeared, proving that the product calcined at 450℃ in air atmosphere is a mixture of ZnAl2O4 and ZnO.
[0070] Figure 1 (c) is the product of calcination at 550℃ in air and CO atmosphere for 4h, respectively, denoted as ZnO / ZnAl2O4-550℃-Air and ZnAl2O4-550℃-CO; in ZnAl2O4-550℃-CO, the 2θ angle is 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 at (220), (311), (422), (511), and (440) were observed. In ZnO / ZnAl2O4-550℃-Air, except for the 2θ angle of 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 (220), (311), (422), (511), and (440) were observed at 2θ angle of 31.7. o , 34.4 o , 36.2 o , 67.9 o The characteristic diffraction peaks of ZnO (100), (002), (101), and (112) appeared, proving that the product calcined at 550℃ in air atmosphere was a mixture of ZnAl2O4 and ZnO.
[0071] Figure 1 (d) is the product calcined at 650℃ in air and CO atmosphere for 4h, respectively, and is denoted as ZnO / ZnAl2O4-650℃-Air and ZnAl2O4-650℃-CO; in ZnAl2O4-650℃-CO, the 2θ angle is 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 at (220), (311), (422), (511), and (440) were observed. In ZnO / ZnAl2O4-650℃-Air, except for the 2θ angle of 31.2o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 (220), (311), (422), (511), and (440) were observed at 2θ angle of 31.7. o , 34.4 o , 36.2 o , 67.9 o The characteristic diffraction peaks of ZnO (100), (002), (101), and (112) appeared, proving that the calcined product in air atmosphere at 650°C is a mixture of ZnAl2O4 and ZnO.
[0072] Figure 2 This is the XPS graph of the sample of the present invention.
[0073] Figure 2 (a) is the O 1s XPS graph of the product calcined in air at 450℃, 550℃, and 650℃. The spectrum of the sample ZnAl2O4 / ZnO-450℃-Air can be fitted into two peaks. The main peak centered at 531.00 eV can be attributed to the lattice oxygen (O ZA ), is the energy spectrum of Zn-O and Al-O in the sample, and 532.27 eV can be attributed to the surface adsorbed oxygen (O a The spectra of samples ZnAl2O4 / ZnO-550℃-Air and ZnAl2O4 / ZnO-650℃-Air can be divided into three peaks. In the sample ZnAl2O4 / ZnO-550℃-Air, the three peaks are 530.83eV, 531.4eV and 542.54eV respectively. Among them, the main peak of 530.83eV is attributed to lattice oxygen, and 531.4eV is related to the defects in the ZnO lattice (O v ), indicating that there are some oxygen defects in the sample; 542.54eV can be attributed to surface adsorbed oxygen; the attribution of the three peaks of the sample ZnAl2O4 / ZnO-650℃-Air is the same as that of the sample ZnAl2O4 / ZnO-550℃-Air; among them, the percentage of defective oxygen in the sample ZnAl2O4 / ZnO-650℃-Air is the highest;
[0074] Figure 2(b) is the O 1s XPS graph of the products calcined in CO atmosphere at 450℃, 550℃ and 650℃; the spectra of samples ZnAl2O4 / ZnO-450℃-CO, ZnAl2O4-550℃-CO and ZnAl2O4-650℃-CO can be fitted into three peaks, which are 541.04-531.70eV, 532.40-532.54eV and 533.57-534.06eV, corresponding to lattice oxygen, defect oxygen and surface oxygen, respectively; among them, the relative content of defect oxygen in sample ZnAl2O4-550℃-CO is the highest.
[0075] Figure 3 This is the EPR diagram of the sample of the present invention.
[0076] Figure 3 (a) is the EPR spectra of the products of zinc aluminum hydrotalcite calcined at 450°C, 550°C, and 650°C in air and CO atmospheres, respectively; the catalyst prepared after calcination in air atmosphere has a signal at g=1.955, indicating that there are chemical substances with unpaired electrons in the catalyst; the catalyst prepared after calcination in CO atmosphere has a signal at g=2.002, indicating that there are also chemical substances with unpaired electrons in the catalyst;
[0077] Figure 3 (b) is the EPR spectrum of the calcined product after zinc oxide removal. It can be seen from the figure that after zinc oxide is removed from the calcined product in an air atmosphere, the signal at g=1.955 disappears, indicating that chemical substances with unpaired electrons exist on the ZnO structure. After ZnO is removed from the calcined product in a CO atmosphere, a signal still appears at g=2.002, indicating that a defect structure exists on the ZnAl2O4 structure.
[0078] Figure 4 This is a graph showing the conversion rate of carbonyl sulfide.
[0079] like Figure 4 As shown, the defects of samples ZnAl2O4 / ZnO-450℃-CO, ZnAl2O4-550℃-CO, and ZnAl2O4-650℃-CO calcined in CO atmosphere are on the spinel, so the conversion rate is high and the catalytic performance is good; the defects of samples ZnAl2O4 / ZnO-450℃-Air, ZnAl2O4 / ZnO-550℃-Air, and ZnAl2O4 / ZnO-650℃-Air calcined in air atmosphere are on ZnO, so the conversion rate is low and the catalytic performance is poor.
[0080] Figure 5 The stability diagram of the catalyst.
[0081] The stability of the catalyst at 90 °C is Figure 5As shown, the catalyst ZnAl2O4-550℃-CO was tested for stability at 90℃, and there was no obvious deactivation of the catalyst after the reaction was carried out for 20 hours; after ZnAl2O4-550℃-Air ran at 90℃ for 20 hours, the catalytic activity decreased by about 13%, and the stability was poor.
[0082] The above-mentioned embodiments only express several implementation methods of the present invention, which is convenient for understanding the technical solution of the present invention in detail, but it cannot be understood as limiting the scope of the invention patent protection. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A carbonyl sulfide hydrolysis catalyst, characterized in that: The catalyst is composed of a hydrotalcite-based composite metal oxide rich in surface oxygen defects; The hydrotalcite-based composite metal oxide catalyst rich in surface oxygen defects is composed of ZnM2O4 or a mixture of ZnO and ZnM2O4. 3+ Represents trivalent metal cation Al 3+ The divalent metal ion Zn in the catalyst 2+ and trivalent metal ions M 3+ The molar ratio is (0.5-0.9):1; The surface oxygen defects of the hydrotalcite-based composite metal oxide catalyst rich in surface oxygen defects are on the spinel structure. Based on the total amount of oxygen elements on the surface of the catalyst as a percentage, the relative content of the surface oxygen defects is 5-40%. In the XRD spectrum, the catalyst has a 2θ angle of 31.2 o , 36.8 o , 55.7 o , 59.3 o , 65.2 o The characteristic diffraction peaks of ZnAl2O4 (220), (311), (422), (511), and (440) are clearly observed, and there are no other peaks except the characteristic peaks of spinel; The preparation method of the carbonyl sulfide hydrolysis catalyst comprises the following steps: Step 1: Preparation of layered double hydroxides by nucleation crystallization isolation method Weigh ZnCl2 and AlCl3∙6H2O and dissolve them in deionized water in a beaker, stir and mix to obtain a metal salt solution. 2+ / Al 3+ The molar ratio is (1-4):1; Weigh NaOH and Na2CO3 and dissolve them in deionized water in a beaker to obtain a mixed alkaline solution, wherein the molar ratio of NaOH to Na2CO3 is (6.4-16):1; The uniformly mixed metal salt solution and the mixed alkali solution are simultaneously and rapidly poured into a colloid mill to obtain a slurry, and then the slurry is statically crystallized at 65-120° C. for 4-24 hours to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a layered double metal hydroxide. The XRD spectrum of the layered double metal hydroxide has a 2θ angle of 11.7 o , 23.6 o , 34.7 o , 39.3 o , 46.9 o , 60.4 o and 61.8 o The characteristic diffraction peaks of hydrotalcite (003), (006), (012), (015), (018), (110) and (113) were clearly observed. Except for the characteristic peaks of hydrotalcite, no other diffraction peaks appeared. Step 2: Calcination of the catalyst at different temperatures in a CO atmosphere to control the specific surface area and relative content of surface oxygen defects The layered double hydroxide is weighed, tableted, granulated into 40-60 mesh, and calcined in a CO atmosphere, with the starting temperature being room temperature and the heating rate being 5-10° C. / min to reach the calcination temperature, the calcination temperature being 450-650° C., the calcination time being 4-6 h, and the CO gas flow rate being 10-50 mL / min, to obtain the carbonyl sulfide hydrolysis catalyst.
2. The catalyst according to claim 1, characterized in that The specific surface area of the catalyst is 56.3-111.7 m 2 / g.
3. A method for preparing the catalyst according to any one of claims 1 or 2, characterized in that: The method comprises the following steps: Step 1: Preparation of layered double hydroxides by nucleation crystallization isolation method Weigh ZnCl2 and AlCl3∙6H2O and dissolve them in deionized water in a beaker, stir and mix to obtain a metal salt solution. 2+ / Al 3+ The molar ratio is (1-4):1; Weigh NaOH and Na2CO3 and dissolve them in deionized water in a beaker to obtain a mixed alkaline solution, wherein the molar ratio of NaOH to Na2CO3 is (6.4-16):1; The uniformly mixed metal salt solution and the mixed alkali solution are simultaneously and rapidly poured into a colloid mill to obtain a slurry, and then the slurry is statically crystallized at 65-120° C. for 4-24 hours to obtain a precipitate, and the precipitate is filtered, washed, and dried to obtain a layered double metal hydroxide. The XRD spectrum of the layered double metal hydroxide has a 2θ angle of 11.7 o , 23.6 o , 34.7 o , 39.3 o , 46.9 o , 60.4 o and 61.8 o The characteristic diffraction peaks of hydrotalcite (003), (006), (012), (015), (018), (110) and (113) were clearly observed. Except for the characteristic peaks of hydrotalcite, no other diffraction peaks appeared. Step 2: Calcination of the catalyst at different temperatures in a CO atmosphere to control the specific surface area and relative content of surface oxygen defects The layered double hydroxide is weighed, tableted, granulated into 40-60 mesh, and calcined in a CO atmosphere, with the starting temperature being room temperature and the heating rate being 5-10° C. / min to reach the calcination temperature, the calcination temperature being 450-650° C., the calcination time being 4-6 h, and the CO gas flow rate being 10-50 mL / min, to obtain the carbonyl sulfide hydrolysis catalyst.
4. The preparation method according to claim 3, characterized in that: In step 1, in the metal salt solution, Zn 2+ The concentration is 0.05-0.2 mol / L, Al 3+ The concentration is 0.05-0.3mol / L.
5. The preparation method according to claim 3, characterized in that: In step 1, in the alkaline solution, Na + The concentration is 0.36-0.42mol / L.
6. The preparation method according to claim 3, characterized in that: In step 1, the uniformly mixed metal salt solution and alkali solution are quickly poured into the colloid mill at the same time, the rotation speed of the colloid mill is controlled to be 5000-10000 rpm, the distance between the stator and the moving rotor is 300-600 nm, and the mixing time is 1-3 minutes.
7. Use of the carbonyl sulfide hydrolysis catalyst according to any one of claims 1 or 2 for carbonyl sulfide hydrolysis reaction, characterized in that: The catalyst is loaded into a reactor, the reaction temperature is controlled at 30-60°C, the raw gas containing carbonyl sulfide gas and N2 is first introduced into a bubbler whose temperature is controlled by a water bath, and then the raw gas carrying water vapor is introduced into the reactor, the water bath temperature is controlled at 30-70°C, and the reaction time is 10-30h, wherein the concentration of carbonyl sulfide in the introduced raw gas is 50-200mg / m 3 , the N2 is the balance gas, and the mass air velocity is set to 10000-48000h -1 , the product is hydrogen sulfide.
8. The use according to claim 7, characterized in that The reactor is a quartz fixed bed reactor with a length of 100-300 mm and an inner diameter of 3-8 mm.
9. The use according to claim 7, characterized in that: The conversion rate of the carbonyl sulfide hydrolysis reaction is greater than 90%, and the concentration of the product hydrogen sulfide measured by gas chromatography is greater than 30 mg / m 3 .
Citation Information
Patent Citations
Carbonyl sulfide hydrolysis and preparation method thereof
CN101690893A
Deep purification fine desulfuration agent and preparation method thereof
CN106179328A
Green long-lasting phosphor material with Zn-site and O-site defects as luminescent center
CN106905962A
Copper-cobalt-based catalyst for organic sulfur hydrolysis removal and preparation method of copper-cobalt-based catalyst
CN112619648A
Hydrolysis catalyst for removing carbonyl sulfide in coal gas at low temperature and preparation method thereof
CN114505069A
Cited By
Method for absorbing and removing carbonyl sulfide in blast furnace gas by adopting eutectic solvent
CN119746585A