A high-strength corrosion-resistant oil casing and its preparation process
By forming a high-temperature oxide film on the surface of the oil casing and using sealants to fill the holes, the problem of corrosion resistance of the oil casing in high-temperature corrosive environments is solved, significantly improving its heat and corrosion resistance, extending its service life and reducing Corrosion rate and environmental pollution.
Patent Information
- Application Number
- CN202410740986.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-11
AI Technical Summary
Petroleum casing is severely corroded in harsh high-temperature corrosive environments, and it is difficult to effectively solve its corrosion resistance problem with existing technology.
High-temperature oxide film and sealant processes are used to form an aluminum film through assisted plating, hot-dip aluminum and oxidation, and silicone sealants are used to fill the pores in the oxide film to enhance the corrosion resistance of the oil casing.
It significantly improves the heat resistance and corrosion resistance of the oil casing, extends its service life, and reduces the corrosion rate and environmental pollution.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil casing and surface treatment thereof, in particular to a high-strength corrosion-resistant oil casing and a preparation process thereof. Background Art
[0002] As a bridge connecting drilling and oil production, in the process of oil production, oil casing is a key part of the long-term stable and high production of oil fields. It is used in large quantities and has high requirements for safety and stability. Once it is put into the well, it must be used for a long time. Oil casing works underground in a harsh high-temperature and corrosive environment. With the extension of oil field development time and the investment of new technologies such as water injection and flooding, the corrosion of casing has become increasingly serious with the application of these technologies. Therefore, we propose a high-strength corrosion-resistant oil casing and its preparation process. Summary of the invention
[0003] The object of the present invention is to provide a high-strength corrosion-resistant oil casing and a preparation process thereof, so as to solve the problems raised in the above-mentioned background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a preparation process of a high-strength corrosion-resistant oil casing, comprising the following processes: taking a steel billet, heating and perforating it in sequence to form a rough pipe; rolling to obtain a rough pipe; sizing, straightening, and heat treatment to obtain the oil casing;
[0005] Aluminum coating and sealing are used to obtain high-strength and corrosion-resistant oil casing.
[0006] Further, the aluminum coating process is as follows: auxiliary plating: place the oil casing in an auxiliary plating solution at 95-100°C for 9-12 minutes, take it out, and dry it at 78-82°C for 60-100 minutes to form a salt film;
[0007] Hot-dip aluminum: Place the oil casing in molten aluminum at 720-740℃, hot-dip for 120-180s, take it out, water-cool, wash, and dry to form an aluminum film;
[0008] Oxidation: Place at 750-1050℃ for 0.5-4h to form an oxide film.
[0009] Furthermore, the plating solution includes the following mass components: 10-15 g / L potassium fluoride, 1.2-2.0 g / L sodium fluoride, 1.2-1.4 g / L calcium chloride, 4.0-5.2 g / L tin chloride, 4-8 g / L zinc chloride, 1.0-2.0 g / L sodium chloride, 0.5-1.5 g / L potassium chloride, 1.0-1.6 g / L potassium fluorozirconate, and the solvent is water.
[0010] In the above technical scheme, the plating process forms a dense and complete salt film on the surface of the oil casing, which can avoid the oxidation of the substrate and improve the wettability between the substrate and molten aluminum; and can activate the substrate surface, making the substrate surface more easily react with molten aluminum. Potassium fluoride, as the main component of the plating solution, is deposited on the surface of the substrate to form a grinding, which can effectively protect the substrate to improve the quality of the aluminum film made by hot-dip aluminum. Potassium fluorozirconate in the plating solution is thermally decomposed during the hot-dip aluminum process, which can dissolve and eliminate aluminum oxide in the system, improve the wettability between the oil casing substrate and the molten aluminum interface, and increase the reaction rate of the substrate surface. Sodium chloride and potassium chloride can effectively reduce the smoke generated on the substrate surface during the hot-dip aluminum process and reduce the harm to the environment. Sodium fluoride is used to prevent secondary oxidation of the surface of the oil casing and can effectively improve the wettability between the substrate and molten aluminum liquid.
[0011] In the hot-dip aluminum process, the molten aluminum contacts the surface of the oil casing substrate, and an aluminum film is formed on the substrate surface, which can effectively improve the heat resistance and corrosion resistance of the oil casing and is suitable for the environment in which the oil casing is located. In the early stage of hot-dip aluminum, diffusion occurs between aluminum and iron atoms, and intermetallic compounds (FeAl3, Fe2Al5) are formed to achieve metallurgical bonding and form a metallurgical layer; and as the process proceeds, the diffusion intensifies, promoting the growth of the metallurgical layer, and the thickness of the aluminum film increases, which helps to improve the surface hardness of the aluminum film and the corrosion resistance of the oil casing. The intermetallic compound (Fe2Al5) is a brittle hard phase, and due to the diffusion difference between aluminum atoms and iron atoms, the intermetallic compound (Fe2Al5) penetrates into the substrate, affecting the performance of the substrate. Excessive temperature will also promote the dissolution of iron on the substrate surface, increase the viscosity of the molten aluminum at the interface, reduce the fluidity of the molten aluminum and the wettability of the substrate surface, and affect the quality of the aluminum film. Therefore, controlling the temperature of molten aluminum at 720-740°C can help reduce the Fe2Al5 content, reduce the brittleness of the aluminum film, promote close bonding between the aluminum film and the oil casing, and improve the quality of the aluminum film.
[0012] The aluminum film is then oxidized to form aluminum oxide on its surface. The aluminum oxide grows and contacts to form a dense oxide film, which can further enhance the corrosion resistance of the oil casing. A higher oxidation temperature helps the diffusion of aluminum atoms in the oil casing matrix, reduces its concentration, distributes it more evenly, and transforms it to the Fe3Al phase, which helps to further improve the high-temperature oxidation resistance and corrosion resistance of the manufactured oil casing.
[0013] Furthermore, the sealing process is as follows: applying the sealant to the surface of the oil casing after aluminum coating, drying, and curing to form a sealing coating; the coating thickness of the sealant is 10 to 20 μm.
[0014] Furthermore, the sealant includes the following components by mass: 10 to 20 parts of alkenyl hydrogen-containing polydimethylsiloxane, 20 to 30 parts of aminosilazane, 5 to 10 parts of 3-aminopropyltriethoxysilane, 6 to 10 parts of 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, 0.18 to 0.30 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 20% to 40%.
[0015] Further, aminosilazane is prepared by the following process:
[0016] Under the protection of nitrogen atmosphere, phenyldichlorocyclodisilazane and n-hexane are mixed, amino group is introduced, and the mixture is stirred to react for 60 to 90 minutes; the mixture is filtered and distilled to obtain aminosilazane.
[0017] Further, the ratio of phenyldichlorocyclodisilazane to n-hexane is (5-10) g / 100 mL;
[0018] The ammonia flow rate is 0.35~0.50L / min.
[0019] Further, phenyldichlorocyclodisilazane is prepared by the following process:
[0020] Mix diphenyldichlorosilane and N,N′-bis(chlorodimethylsilyl)tetramethylcyclodisilazane, raise the temperature to 320-380°C, and keep the temperature to react for 10 hours; cool naturally, and extract with toluene and n-octane to obtain phenyldichlorocyclodisilazane.
[0021] Furthermore, the molar ratio of diphenyldichlorosilane to N,N′-bis(chlorodimethylsilyl)tetramethylcyclodisilazane is (2.1-4.2):1.
[0022] With the increase of reaction temperature and molar ratio, the product phenyldichlorocyclodisilazane changes from 1,3-bis(diphenylchlorosilyl)-2,2,4,4-tetramethylcyclodisilazane to 1,3-bis(diphenylchlorosilyl)-2,2,4,4-tetraphenylcyclodisilazane.
[0023] Furthermore, the drying process conditions are: drying temperature 55-60°C, humidity 40%-50%RH, and drying time 30-60min.
[0024] Furthermore, the curing process conditions are: ultraviolet irradiation for 20 to 25 minutes, the distance between the sealing coating and the light source is 3 cm, and the wavelength of the light source is 185 to 254 nm.
[0025] In the above technical scheme, due to the long-term high temperature of oxidation in the aluminum coating process, the iron element diffuses outward and the aluminum element diffuses inward, so that the molten aluminum on the surface of the aluminum film is continuously consumed, and the mass fraction of aluminum in the aluminum-poor area is reduced, which cannot provide sufficient chlorine elements for the continuous growth of aluminum oxide, so that it is stretched by the nearby aluminum oxide to form holes, which will have a negative impact on the corrosion resistance of the oil casing. Therefore, it needs to be sealed. By applying the sealant, it enters the holes of the oxide film and solidifies and seals it. The low surface energy and good wettability of silicone make it have good leveling properties and easier to enter the pores, which helps to reduce shrinkage cavities, orange peel and other undesirable phenomena, and can effectively increase the diffusion path of the corrosive medium, thereby reducing the corrosion rate and improving the corrosion resistance of the oil casing.
[0026] After the sealant is applied, it is first subjected to wet heat conversion. The Si-H in alkenyl hydrogenated polydimethylsiloxane and Si-NH in aminosilazane are hydroxylated. 3-aminopropyltriethoxysilane is hydrolyzed to generate silanol groups. Si-OH undergoes dehydration and polycondensation on the surface of the oxide film to initially form a Si-O-Si cross-linked structure, fix the sealant components on the surface of the oil casing, and remove the solvent. In addition, aminosilazane and 3-aminopropyltriethoxysilane contain primary amine groups, which provide alkalinity for the system, promote the generation of silanol groups, transform them into silicon oxide structures, and improve the density of the closed coating. The amine groups in the system make the sealant have better adhesion on the surface and pores of the oxide film, and improve the bonding between the closed coating and the substrate.
[0027] After UV irradiation, Si-CH3 in the sealant system breaks and oxidizes to form Si-O bonds, which promotes the inorganicization of the sealant coating and increases the surface silicon oxide content, which helps to strengthen the oxide film formed after aluminum coating and reduce its porosity. Under the action of photoinitiator and UV irradiation, the alkenyl hydrogen-containing polydimethylsiloxane in the sealant and the alkenyl in 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane undergo free radical polymerization, increasing the crosslinking degree of the system, while strengthening the oxide film and sealing the holes, increasing the organic content in the system. Aminosilazane is obtained by ammonolysis of phenyldichlorocyclodisilazane, which converts Si-Cl bonds into Si-NH bonds, can enhance the adhesion between the sealant and the oxide film, increase the density of the coating, and make the surface of the closed coating have better corrosion resistance. In combination with 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, the cyclodisilazane structure is introduced into the system, which can improve the adhesion and high temperature resistance of the closed coating; at the same time, the organic groups such as methyl, methylene, and phenyl are coordinated to increase the diffusion path of the medium, the surface energy of the closed coating is low, and the water contact angle is increased, so that it has excellent hydrophobicity, can effectively resist the invasion of corrosive ions, reduce the contact between the corrosive medium and the oil casing, and improve its heat corrosion resistance.
[0028] Further, the steel billet comprises the following mass components: carbon C: 0.22% to 0.29%, chromium Cr: 0.15% to 0.80%, silicon Si: 0.17% to 0.37%, manganese Mn: 0.35% to 0.75%, titanium Ti: 0.07% to 0.15%, vanadium V: ≤0.01%, sulfur S: 0.015% to 0.030%, molybdenum Mo: 0.15% to 0.30%, nickel Ni: ≤0.030%, copper Cu: ≤0.10%, phosphorus P: ≤0.02%, nitrogen N: ≤0.01%, calcium Ca: 0.025% to 0.085%, rare earth RE: 120 to 160ppm; the balance is iron Fe;
[0029] The rare earth element is one or more of cerium, lanthanum, neodymium and yttrium.
[0030] Further, the material is heated to 1200-1280°C, kept warm for 4-7 hours and then perforated; the perforation temperature is 1150-1200°C.
[0031] Furthermore, the process conditions of the heat treatment are: quenching: quenching temperature 900-920°C, holding time 60-80min, water quenching;
[0032] Tempering: Tempering temperature 480 ~ 520 ℃, insulation time 60 ~ 80min.
[0033] In the above technical scheme, carbon is the most effective element to improve the strength and hardenability of steel, and the carbon content is controlled at 0.17% to 0.35% to prevent quenching deformation and cracking. Manganese and silicon are economical elements to improve the strength of steel, which can effectively improve the hardness and strength of oil casing; manganese is a good deoxidation and desulfurization element, which can avoid the formation of FeS at the grain boundary, reduce the hot brittleness of steel, and improve its hot processing performance; the sulfur content is controlled at 0.015% to 0.030%, and it forms MnS with a higher melting point with manganese, which can improve the mechanical properties of steel. Chromium and molybdenum can increase the hardenability of steel and improve the mechanical properties, corrosion resistance and wear resistance of steel. Titanium is an austenite stabilizing element, which can form stable titanium carbide with carbon, thereby reducing the solubility of carbon in steel, effectively stabilizing the austenite phase, and preventing austenite from transforming into a non-austenite phase at high temperature or during cooling. Vanadium can refine the grains of steel, improve the toughness of steel, and improve its thermal sensitivity; it can also improve the tempering stability of martensite. Steel contains a small amount of calcium, which has a strong deoxidizing ability, has a good deterioration promoting effect on inclusions in steel, and can reduce the segregation of sulfur in the grain boundaries, reduce the brittleness of steel, and improve its resistance to thermal cracking. Steel contains rare earth, which has the effect of desulfurization and degassing. At the same time, the fine particles generated by the reaction of rare earth and liquid metal have the effect of accelerating solidification nucleation, which can refine the grains of high-silicon cast steel, limit dendrite segregation, and effectively improve mechanical properties and wear resistance.
[0034] Quenching promotes austenitization of steel, water quenching forms martensite structure, and the original austenite grains are refined. In the tempering heat treatment, with the increase of temperature and time, martensite decomposes and refines, carbides precipitate, and play a role in solid solution strengthening, which can effectively improve the tensile strength of oil casing. The ratio of the above components is conducive to the formation and stabilization of the grain structure of steel after heat treatment, so that the produced oil casing exhibits excellent comprehensive mechanical properties.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] The invention describes a preparation process for a high-strength, corrosion-resistant oil casing, which is formed by heating, piercing, rolling and heat treating a steel billet; and aluminum coating and sealing the surface of the billet to obtain an oil casing with high-strength, corrosion-resistant performance. Aluminum coating includes plating, hot-dip aluminum and high-temperature oxidation, forming a corrosion-resistant oxide film on the surface of the oil casing, and plugging the holes with an organic silicon sealant containing cyclodisilazane, which can effectively improve its heat corrosion resistance. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] In the following specific embodiment, the steel billet includes the following mass components: carbon C: 0.25%, chromium Cr: 0.66%, silicon Si: 0.20%, manganese Mn: 0.45%, titanium Ti: 0.10%, vanadium V: 0.008%, sulfur S: 0.018%, molybdenum Mo: 0.19%, nickel Ni: 0.011%, copper Cu: 0.05%, phosphorus P: 0.009%, nitrogen N: 0.009%, calcium Ca: 0.029%, rare earth cerium Ce: 142ppm; the balance is iron Fe;
[0039] Alkenyl hydrogenated polydimethylsiloxane: CAS NO: 104780-63-4, from Gaide Chemical;
[0040] The photoinitiator is 2,2-dimethoxy-2-phenylacetophenone;
[0041] The size of the billet is 300.00mm×21.50mm;
[0042] The size of the oil casing is 193.68mm×12.70mm, the minimum diameter is 165.40mm, and the minimum length is 152mm.
[0043] Embodiment 1: A process for preparing a high-strength corrosion-resistant oil casing comprises the following processes:
[0044] S1. Take the steel billet, heat it to 1200℃, keep it warm for 7h, then punch it, the punching temperature is 1150℃, and form a rough tube; roll it to get a rough tube; sizing, straightening, and heat treatment. The process conditions of heat treatment are: quenching: quenching temperature 900℃, holding time 80min, water quenching; tempering: tempering temperature 480℃, holding time 80min, and get oil casing;
[0045] S2, aluminum coating, the process is as follows: auxiliary plating: put the oil casing in a 95℃ auxiliary plating solution, auxiliary plating for 12 minutes, take it out, dry it at 78℃ for 100 minutes, and form a salt film; the auxiliary plating solution includes the following mass components: 15g / L potassium fluoride, 2.0g / L sodium fluoride, 1.4g / L calcium chloride, 5.2g / L tin chloride, 6g / L zinc chloride, 1.2g / L sodium chloride, 1.5g / L potassium chloride, 1.0g / L potassium fluorozirconate, and the solvent is water;
[0046] Hot-dip aluminum: Place the oil casing in 720℃ molten aluminum, hot dip for 180s, take it out, water cool, wash, dry, and form an aluminum film;
[0047] Oxidation: Place at 750℃ for 4 hours to form an oxide film;
[0048] S3, sealing, the process is as follows: apply the sealant to the surface of the oil casing after aluminum coating, the coating thickness of the sealant is 12μm, dry, the drying process conditions are: drying temperature 55℃, humidity 40%RH, time 60min; curing, the curing process conditions are: ultraviolet irradiation 20min, the distance between the sealing coating and the light source is 3cm, the wavelength of the light source is 185nm, and the sealing coating is formed; 20℃, 35%RH, stand for 24h, and obtain high-strength corrosion-resistant oil casing; the sealant includes the following mass components: 10 parts of alkenyl hydrogen-containing polydimethylsiloxane, 30 parts of aminosilazane, 10 parts of 3-aminopropyltriethoxysilane, 6 parts of 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, 0.18 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 30%;
[0049] Aminosilazane is prepared by the following process: under the protection of nitrogen atmosphere, phenyldichlorocyclodisilazane and n-hexane are mixed, amino group is introduced, and the reaction is stirred for 60 minutes; suction filtration and distillation are performed to obtain aminosilazane; the ratio of phenyldichlorocyclodisilazane to n-hexane is 5g / 100mL; the flow rate of ammonia is 0.35L / min;
[0050] Phenyldichlorocyclodisilazane is prepared by the following process: diphenyldichlorosilane and N,N'-bis(chlorodimethylsilyl)tetramethylcyclodisilazane are mixed, the temperature is raised to 320°C, and the reaction is kept at this temperature for 10 hours; the mixture is naturally cooled, and phenyldichlorocyclodisilazane is obtained by extraction with toluene and n-octane; the molar ratio of diphenyldichlorosilane to N,N'-bis(chlorodimethylsilyl)tetramethylcyclodisilazane is 2.1:1.
[0051] Embodiment 2: A process for preparing a high-strength corrosion-resistant oil casing comprises the following processes:
[0052] S1. Take the steel billet, heat it to 1240℃, keep it warm for 5h, then punch it, the punching temperature is 1180℃, and form a rough tube; roll it to get a rough tube; sizing, straightening, and heat treatment. The process conditions of heat treatment are: quenching: quenching temperature 910℃, holding time 70min, water quenching; tempering: tempering temperature 500℃, holding time 70min, and get oil casing;
[0053] S2, aluminum coating, the process is as follows: auxiliary plating: put the oil casing in a 98℃ auxiliary plating solution, assist plating for 10 minutes, take it out, dry it at 80℃ for 80 minutes to form a salt film; the auxiliary plating solution includes the following mass components: 15g / L potassium fluoride, 1.6g / L sodium fluoride, 1.4g / L calcium chloride, 4.6g / L tin chloride, 5g / L zinc chloride, 1.1g / L sodium chloride, 1.0g / L potassium chloride, 1.3g / L potassium fluorozirconate, and the solvent is water;
[0054] Hot-dip aluminum: Place the oil casing in 730℃ molten aluminum, hot dip for 150s, take it out, water cool, wash, dry, and form an aluminum film;
[0055] Oxidation: Place at 900℃ for 2h to form an oxide film;
[0056] S3, sealing, the process is as follows: apply the sealant to the surface of the oil casing after aluminum coating, the coating thickness of the sealant is 12μm, dry, the drying process conditions are: drying temperature 58℃, humidity 45%RH, time 45min; curing, the curing process conditions are: ultraviolet irradiation 22min, the distance between the sealing coating and the light source is 3cm, the wavelength of the light source is 185nm, and the sealing coating is formed; 22℃, 36%RH, stand for 24h, and obtain high-strength corrosion-resistant oil casing; the sealant includes the following mass components: 15 parts of alkenyl hydrogen-containing polydimethylsiloxane, 25 parts of aminosilazane, 7 parts of 3-aminopropyltriethoxysilane, 8 parts of 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, 0.24 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 20%;
[0057] Aminosilazane is prepared by the following process: under the protection of nitrogen atmosphere, phenyldichlorocyclodisilazane and n-hexane are mixed, amino group is introduced, and the reaction is stirred for 75 minutes; suction filtration and distillation are performed to obtain aminosilazane; the ratio of phenyldichlorocyclodisilazane to n-hexane is 5g / 100mL; the flow rate of ammonia is 0.42L / min;
[0058] Phenyldichlorocyclodisilazane is prepared by the following process: diphenyldichlorosilane and N,N'-bis(chlorodimethylsilyl)tetramethylcyclodisilazane are mixed, the temperature is raised to 380°C, and the reaction is kept at this temperature for 10 hours; the mixture is naturally cooled, and phenyldichlorocyclodisilazane is obtained by extraction with toluene and n-octane; the molar ratio of diphenyldichlorosilane to N,N'-bis(chlorodimethylsilyl)tetramethylcyclodisilazane is 4.1:1.
[0059] Embodiment 3: A process for preparing a high-strength corrosion-resistant oil casing comprises the following processes:
[0060] S1. Take the steel billet, heat it to 1280℃, keep it warm for 4h, then punch it, the punching temperature is 1200℃, and form a rough tube; roll it to get a rough tube; sizing, straightening, and heat treatment. The process conditions of heat treatment are: quenching: quenching temperature 920℃, holding time 60min, water quenching; tempering: tempering temperature 520℃, holding time 60min, and get oil casing;
[0061] S2, aluminum coating, the process is as follows: auxiliary plating: put the oil casing in a 100℃ auxiliary plating solution, assist plating for 9 minutes, take it out, dry it at 82℃ for 60 minutes, and form a salt film; the auxiliary plating solution includes the following mass components: 15g / L potassium fluoride, 1.2g / L sodium fluoride, 1.4g / L calcium chloride, 4.0g / L tin chloride, 4g / L zinc chloride, 1.0g / L sodium chloride, 0.5g / L potassium chloride, 1.6g / L potassium fluorozirconate, and the solvent is water;
[0062] Hot-dip aluminum: Place the oil casing in 740℃ molten aluminum, hot dip for 120s, take it out, water cool, wash, dry, and form an aluminum film;
[0063] Oxidation: Place at 1050℃ for 0.5h to form an oxide film;
[0064] S3, sealing, the process is as follows: apply the sealant to the surface of the oil casing after aluminum coating, the coating thickness of the sealant is 12μm, and dry, the drying process conditions are: drying temperature 60℃, humidity 40%RH, time length 30min; curing, the curing process conditions are: ultraviolet irradiation 25min, the distance between the sealing coating and the light source is 3cm, the wavelength of the light source is 254nm, and the sealing coating is formed; 25℃, 40%RH, stand for 24h, and obtain high-strength corrosion-resistant oil casing;
[0065] The sealant includes the following components by mass: 20 parts of alkenyl hydrogen-containing polydimethylsiloxane, 30 parts of aminosilazane, 10 parts of 3-aminopropyltriethoxysilane, 10 parts of 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, 0.3 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 20%;
[0066] Aminosilazane is prepared by the following process: under the protection of nitrogen atmosphere, phenyldichlorocyclodisilazane and n-hexane are mixed, amino group is introduced, and the reaction is stirred for 90 minutes; suction filtration and distillation are performed to obtain aminosilazane; the ratio of phenyldichlorocyclodisilazane to n-hexane is 5g / 100mL; the flow rate of ammonia is 0.50L / min;
[0067] Phenyldichlorocyclodisilazane is prepared by the following process: diphenyldichlorosilane and N,N′-bis(chlorodimethylsilyl)tetramethylcyclodisilazane are mixed, the temperature is raised to 380°C, and the reaction is kept at this temperature for 10 hours; the mixture is naturally cooled, and phenyldichlorocyclodisilazane is obtained by extraction with toluene and n-octane; the molar ratio of diphenyldichlorosilane to N,N′-bis(chlorodimethylsilyl)tetramethylcyclodisilazane is 4.2:1.
[0068] Comparative Example 1: A preparation process for a high-strength corrosion-resistant oil casing, comprising the following processes:
[0069] S1-S2 are the same as in Example 1;
[0070] S3. Sealing. The process is as follows: apply the sealant to the surface of the oil casing after aluminum coating, the coating thickness of the sealant is 12μm, and dry. The drying process conditions are: drying temperature 55℃, humidity 40%RH, and time 60min; curing. The curing process conditions are: ultraviolet irradiation for 20min, the distance between the sealing coating and the light source is 3cm, the wavelength of the light source is 185nm, and a sealing coating is formed; 20℃, 35%RH, stand for 24h, and obtain high-strength corrosion-resistant oil casing; the sealant includes the following mass components: 10 parts of alkenyl hydrogen-containing polydimethylsiloxane, 10 parts of 3-aminopropyltriethoxysilane, 0.02 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 30%.
[0071] Comparative Example 2: A preparation process for a high-strength corrosion-resistant oil casing, comprising the following processes:
[0072] S1-S2 are the same as in Example 1;
[0073] S3. Sealing. The process is as follows: apply the sealant to the surface of the oil casing after aluminum coating, the coating thickness of the sealant is 12μm, and dry. The drying process conditions are: drying temperature 55℃, humidity 40%RH, and time 60min; curing. The curing process conditions are: ultraviolet irradiation for 20min, the distance between the sealing coating and the light source is 3cm, the wavelength of the light source is 185nm, and a sealing coating is formed; 20℃, 35%RH, stand for 24h, and obtain high-strength corrosion-resistant oil casing; the sealant is a mixture of alkenyl hydrogenated polydimethylsiloxane with a solid content of 30% and a photoinitiator, and the solvent is n-butyl ether; the photoinitiator is 0.3% of the mass of alkenyl hydrogenated polydimethylsiloxane.
[0074] Comparative Example 3: A preparation process for a high-strength corrosion-resistant oil casing, comprising the following processes:
[0075] S1-S2 are the same as in Example 1;
[0076] S3. Sealing. The process is as follows: apply the sealant to the surface of the oil casing after aluminum coating. The coating thickness of the sealant is 12μm. Dry. The drying process conditions are: drying temperature 55℃, humidity 40%RH, time 60min; 20℃, 35%RH, standing for 24h to obtain high-strength corrosion-resistant oil casing. The sealant is a 30% solid content 3-aminopropyltriethoxysilane / n-butyl ether solution, and the solvent is n-butyl ether.
[0077] Comparative Example 4:
[0078] S1. Take the steel billet and heat it to 1200℃, keep it warm for 7h and then pierce it. The piercing temperature is 1150℃ to form a rough tube; roll it to get a rough tube; sizing, straightening and heat treatment. The process conditions of heat treatment are: quenching: quenching temperature 900℃, holding time 80min, water quenching; tempering: tempering temperature 700℃, holding time 80min, and get oil casing.
[0079] Comparative Example 5: S1 is the same as Example 1, and an oil casing is obtained;
[0080] The steel billet includes the following mass components: carbon C: 0.25%, chromium Cr: 0.85%, silicon Si: 0.20%, manganese Mn: 0.87%, titanium sulfur S: 0.005%, molybdenum Mo: 0.16%, nickel Ni: 0.06%, phosphorus P: 0.009%, nitrogen N: 0.009%, calcium Ca: 0.029%; the balance is iron Fe.
[0081] Experiment: Take the oil casing and high-strength corrosion-resistant oil casing obtained in Examples 1-3 and Comparative Examples 1-5, prepare samples, test their properties respectively and record the test results:
[0082] 1. Experiments on oil casing:
[0083] Tensile performance test: Taking ASTM A370 as the reference standard, a universal testing machine was used to conduct tensile performance tests;
[0084] Impact performance test: Taking ASTM A370 as the reference standard, the sample was subjected to room temperature impact test on a drop weight test machine. The sample was a V-notch impact specimen with a size of 10mm×7.5mmmm×55mm.
[0085] 2. Experiments on high-strength corrosion-resistant oil casing:
[0086] Corrosion resistance test: The electrochemical performance of the sample was tested using an electrochemical workstation. The experimental medium was 3.5wt% sodium chloride solution, a 10mm×10mm sample was used as the working electrode, saturated calomel was used as the reference electrode, and platinum was used as the auxiliary electrode. The experimental temperature was 25°C. The experiment was immersed in the corrosive medium for 24 hours. The scanning rate was 1mV / s, the scanning range was -0.3~1.6V, and the scanning frequency was 1×(10 -2 ~10 5 ) Hz;
[0087] Thermal corrosion performance test: Cover the surface of the sample with 2M corrosion solution (a mixed solution of sodium sulfate and potassium sulfate with a molar ratio of 7:3), place it in a 260℃ resistance furnace, and corrode for 4 hours; after the experiment, record the percentage of the sample corrosion area to the total area as the test index;
[0088] Adhesion test: GB / T 9286 is used as the reference standard to test the adhesion of the sample.
[0089] Table 1 shows the tensile and impact properties test results of the oil casing samples of Examples 1-3 and Comparative Examples 4-5:
[0090] Example 1 Example 2 Example 3 Comparative Example 4 Comparative Example 5 Tensile strength (MPa) 1393 1307 1172 792 815 Impact absorption energy (J) 97 103 117 138 84
[0091] Table 2 shows the corrosion resistance and adhesion test results of the high-strength corrosion-resistant oil casing samples of Examples 1-3 and Comparative Examples 1-3:
[0092] <![CDATA[Corrosion current density (A / cm 2 )]]> High temperature corrosion area (%) Adhesion Example 1 <![CDATA[1.74×10 -7 ]]> 0.1 Level 0 Example 2 <![CDATA[1.18×10 -7 ]]> No corrosion Level 0 Example 3 <![CDATA[8.96×10 -8 ]]> No corrosion Level 0 Comparative Example 1 <![CDATA[6.93×10 -7 ]]> 0.7 Level 0 Comparative Example 2 <![CDATA[1.49×10 -6 ]]> 3.3 Level 1 Comparative Example 3 <![CDATA[9.35×10 -7 ]]> 1.0 Level 1
[0093] According to the data in the above table, we can clearly draw the following conclusions:
[0094] The oil casing and high-strength corrosion-resistant oil casing obtained in Examples 1-3 are compared with the oil casing and high-strength corrosion-resistant oil casing obtained in Comparative Examples 1-5. The test results show that:
[0095] Compared with the comparative example, the oil casing and high-strength corrosion-resistant oil casing obtained in Examples 1-3 have more excellent tensile strength data and corrosion performance data, which fully demonstrates that the preparation and surface treatment of the oil casing in the present invention can improve its strength and corrosion resistance.
[0096] Compared with the high-strength corrosion-resistant oil casing obtained in Example 1, aminosilazane and 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane are not added to the sealant of Comparative Example 1; the sealant components are alkenyl hydrogen-containing polydimethylsiloxane, 3-aminopropyltriethoxysilane and photoinitiator; the sealant components of Comparative Example 2 are alkenyl hydrogen-containing polydimethylsiloxane and photoinitiator; the sealant component of Comparative Example 3 is 3-aminopropyltriethoxysilane. The high-strength corrosion-resistant oil casing obtained in Comparative Examples 1-3 have deteriorated corrosion current density, high-temperature corrosion area and adhesion data. It can be seen that the surface treatment process of the oil casing and the setting of the components used in the present invention can promote the improvement of its heat corrosion resistance and adhesion.
[0097] Compared with the oil casing obtained in Example 1, the heat treatment process in Comparative Example 4 is different; too high tempering temperature will lead to a large decomposition of martensite, aggregation and growth of carbides, resulting in a decrease in the strength of the oil casing. In Comparative Example 5, the composition ratio of the steel billet is different, and no rare earth element is added, which weakens the purification and fine grain strengthening effects on the melt, and the strength of the oil casing is reduced.
[0098] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0099] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A process for preparing high-strength corrosion-resistant oil casing, characterized in that: Including the following processes: The steel billet is heated and perforated in sequence to form a rough tube; Rolling to obtain rough pipe; Sizing, straightening and heat treatment to obtain oil casing; Aluminum coating and sealing to obtain high-strength and corrosion-resistant oil casing; The aluminum coating process includes the following steps: a. Plating assistance: Place the oil casing in a 95-100℃ plating assistance solution for 9-12 minutes, take it out, and dry it at 78-82℃ for 60-100 minutes to form a salt film; b. Hot-dip aluminum: Place the oil casing in molten aluminum at 720-740℃, hot-dip for 120-180s, take it out, water-cool, wash, and dry to form an aluminum film; c. Oxidation: Place at 750-1050℃ for 0.5-4h to form an oxide film; The sealing comprises the following process: applying a sealant to the surface of the oil casing after aluminum coating, drying, curing, and forming a sealing coating; the coating thickness of the sealant is 10-20 μm; the sealant comprises the following mass components: 10-20 parts of alkenyl hydrogen-containing polydimethylsiloxane, 20-30 parts of aminosilazane, 5-10 parts of 3-aminopropyltriethoxysilane, 6-10 parts of 1,1,3,N,N′-pentamethyl-3-vinylcyclodisilazane, 0.18-0.30 parts of photoinitiator, and the solvent is n-butyl ether; the solid content of the sealant is 20%-40%.
2. The process for preparing a high-strength corrosion-resistant oil casing according to claim 1, characterized in that: The aminosilazane is prepared by the following process: diphenyldichlorosilane and N,N′-bis(chlorodimethylsilyl)tetramethylcyclodisilazane are mixed, the temperature is raised to 320-380° C., and the temperature is kept for reaction for 10 hours to obtain phenyldichlorocyclodisilazane; under the protection of nitrogen atmosphere, phenyldichlorocyclodisilazane and n-hexane are mixed, amino groups are introduced, and the reaction is stirred for 60-90 minutes to obtain aminosilazane.
3. The process for preparing a high-strength corrosion-resistant oil casing according to claim 1, characterized in that: The drying process conditions are: drying temperature 55-60°C, humidity 40%-50%RH, and time 30-60min.
4. The process for preparing a high-strength corrosion-resistant oil casing according to claim 1, characterized in that: The curing process conditions are: ultraviolet irradiation for 20 to 25 minutes, the distance between the sealing coating and the light source is 3 cm, and the wavelength of the light source is 185 to 254 nm.
5. The process for preparing a high-strength corrosion-resistant oil casing according to claim 1, characterized in that: The steel billet includes the following mass components: C: 0.22%~0.29%, Cr: 0.15%~0.80%, Si: 0.17%~0.37%, Mn: 0.35%~0.75%, Ti: 0.07%~0.15%, V: ≤0.01%, S: 0.015%~0.030%, Mo: 0.15%~0.30%, nickel Ni: ≤0.030%, Cu: ≤0.10%, P: ≤0.02%, N: ≤0.01%, Ca: 0.025%~0.085%, RE: 120~160ppm; the balance is Fe.
6. The process for preparing a high-strength corrosion-resistant oil casing according to claim 1, characterized in that: The process conditions of the heat treatment are: quenching: quenching temperature 900-920°C, holding time 60-80min, water quenching; Tempering: Tempering temperature 480 ~ 520 ℃, insulation time 60 ~ 80min.
7. A high-strength, corrosion-resistant oil casing produced according to the production process according to any one of claims 1 to 6.