A large volume ultra-high performance concrete and its preparation process
By synthesizing amphoteric ether-type polycarboxylate water-reducing agents and using steel fibers and polypropylene fibers, the problem of cracks in large-volume concrete caused by uneven temperatures and the poor dispersion performance of polycarboxylate water-reducing agents has been solved, achieving high performance The preparation of concrete meets construction needs.
Patent Information
- Application Number
- CN202410380958.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-31
AI Technical Summary
During the construction process of large-volume concrete, the tensile stress caused by uneven temperature is too large and cracks are prone to occur. Moreover, the existing polycarboxylate superplasticizer has poor dispersion performance under high salt concentrations and cannot meet the construction needs of large-volume concrete.
By synthesizing amphoteric ether type polycarboxylate superplasticizer, introducing anionic and cationic groups to enhance its adsorption capacity and dispersion performance of cement particles, and combining steel fiber and polypropylene fiber to optimize the crack resistance and tensile properties of concrete.
It significantly improves the crack resistance of large-volume concrete, slows down the heat release rate of hydration reaction, reduces adiabatic temperature rise, enhances the mechanical properties and fluidity of concrete, and meets the construction requirements of large-volume concrete.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, in particular to a large-volume ultra-high performance concrete and a preparation process thereof. Background Art
[0002] Concrete is one of the main building materials in the construction industry and the most widely used artificial material in the world. The hydration reaction of concrete releases a large amount of heat. When the volume of the concrete structure is large, the heat is difficult to dissipate, which will lead to uneven spatial distribution of the internal temperature of the concrete after pouring. Usually, the temperature in the central area of the interior is high and the temperature in the boundary area is low. When the deformation of the structure due to temperature is constrained, including foundation constraints and mature concrete constraints, a large tensile stress will be generated. When the tensile stress exceeds the tensile strength of the concrete, large-volume concrete at an early age will produce surface cracks, deep cracks and even penetrating temperature cracks, which seriously affect the normal progress of concrete construction. Therefore, the development of a new type of large-volume ultra-high performance concrete has become a hot topic of current research.
[0003] If the early shrinkage cracks of concrete are not handled in time or are handled improperly, the deterioration of concrete will be accelerated, which will not only affect the appearance and use function of the building, but also pose a threat to the safety and durability of the structure. In practice, in addition to improving the steam curing efficiency and saving energy consumption by optimizing the steam curing system, the development of polycarboxylic acid water reducers that can effectively improve the comprehensive performance of concrete has become an important research field of concrete; in actual applications, the evaluation indicators of concrete are only the strength and slump of concrete, which results in the development process of concrete being mainly a process of continuous improvement of the strength grade and slump of concrete, while ignoring the problem of the volume stability of concrete, which also makes the production and application of water reducers only focus on the size of the water reduction rate The direct consequence of poor volume stability is the occurrence of cracks; due to the different contents of certain components and substances in concrete, there are also some compatibility problems between ordinary polycarboxylate water-reducing agents and concrete. The initial working performance of the benchmark mix concrete prepared with ordinary polycarboxylate water-reducing agents is acceptable, but the slump and expansion losses are large, the plasticity retention performance is poor, and it cannot meet the requirements of large-volume continuous pumping construction. In addition, the early adiabatic temperature rise of concrete is high, the autogenous shrinkage and drying shrinkage are large, and the crack resistance is poor; currently, polycarboxylate water-reducing agents are mainly anionic water-reducing agents, but the side chains of their "comb-type" molecules will curl in cement systems with high salt concentrations, especially calcium ions, and the adsorption on cement particles will slow down, thereby reducing their cement dispersibility.
[0004] The invention synthesizes molecular monomers of amphoteric groups through molecular design, polymerizes with polyoxyethylene ether long-chain monomers and maleic anhydride monomers, and introduces some anionic and cationic groups into the molecular chain of polycarboxylate water-reducing agent to synthesize amphoteric polycarboxylate water-reducing agent with higher performance, so that large-volume ultra-high performance concrete has obvious enhanced anti-cracking effect. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a large-volume ultra-high performance concrete and a preparation process thereof, thereby improving the problems of severe chemical shrinkage and poor dispersion performance of large-volume concrete.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A large-volume ultra-high performance concrete comprises the following components in parts by weight: 30-35 parts of cement, 10-15 parts of deionized water, 18-25 parts of crushed stone, 16-22 parts of quartz sand, 5-12 parts of fly ash, 3-6 parts of steel fiber, 2-5 parts of polypropylene fiber, 0.3-1.5 parts of amphoteric ether type polycarboxylate water reducer, 0.2-1 parts of hydration temperature rise inhibitor, and 0.1-0.5 parts of expansion agent.
[0008] The preparation process of large-volume ultra-high performance concrete is as follows: weigh the above-mentioned weight components of cement, crushed stone, quartz sand, fly ash, steel fiber and hydration temperature rise inhibitor, pour them into a concrete mixer and dry mix for 30-50 seconds. After mixing evenly, add deionized water and expansion agent, mix and stir for 6-10 minutes, then add amphoteric ether polycarboxylate water reducer and polypropylene fiber, stir for 10-20 minutes, and naturally cure after molding to obtain large-volume ultra-high performance concrete.
[0009] Preferably, the cement is low-heat silicate cement, and the expansion agent is calcium oxide expansion agent.
[0010] Preferably, the steel fiber is a copper-plated steel fiber with a diameter of 0.2-0.25 mm and a length of 10-15 mm.
[0011] Preferably, the preparation process of the amphoteric ether type polycarboxylate water reducer is:
[0012] (1) Add 2,3-epoxypropyldimethylamine and chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add sodium 2-chloroethane-1-sulfonate, stir to react, and after the reaction is completed, cool to room temperature, filter, wash with ether, and dry to obtain 2,3-epoxypropyl betaine intermediate. The preparation reaction formula is:
[0013]
[0014] (2) Add allyl polyoxyethylene ether and deionized water to a reaction flask equipped with a reflux condenser, stir evenly, then add 2,3-epoxypropyl betaine intermediate and sodium hydroxide aqueous solution, adjust the pH to 10-11, stir and react, add glacial acetic acid to neutralize after the reaction, concentrate and dry to obtain amphoteric allyl polyoxyethylene ether. The preparation reaction formula is as follows:
[0015]
[0016] (3) Add amphoteric allyl polyoxyethylene ether, maleic anhydride and deionized water to a reaction flask equipped with a reflux condenser and a dropping funnel, stir evenly, then drop acrylic acid and ammonium persulfate at the same time, react at 60-80°C for 2-5h, cool to 40-50°C, add sodium hydroxide aqueous solution to adjust the pH to 6-7, continue stirring for 10-20min, and obtain an amphoteric ether type polycarboxylic acid water reducer.
[0017] Preferably, in step (1), the ratio of 2,3-epoxypropyldimethylamine to sodium 2-chloroethane-1-sulfonate is 1 mol: (1.05-1.15) mol.
[0018] Preferably, in step (1), the reaction temperature is 45-60° C. and the reaction time is 48-72 h.
[0019] Preferably, in step (2), the ratio of allyl polyoxyethylene ether to 2,3-epoxypropyl betaine intermediate is 1 mol: (1.02-1.1) mol.
[0020] Preferably, the mass fraction of the sodium hydroxide aqueous solution in step (2) is 25-35%.
[0021] Preferably, in step (2), the reaction temperature is 40-55° C. and the reaction time is 3-8 h.
[0022] Preferably, in step (3), the ratio of the amphoteric allyl polyoxyethylene ether, maleic anhydride, acrylic acid, and ammonium persulfate is (0.3-0.45) mol: (0.1-0.3) mol: 1 mol: (0.03-0.05) mol.
[0023] By adopting the above technical solution, the beneficial effects of the present invention are:
[0024] The invention firstly conducts quaternization reaction on 2,3-epoxypropyl dimethylamine and sodium 2-chloroethane-1-sulfonate to obtain a 2,3-epoxypropyl betaine intermediate, then conducts epoxy ring-opening reaction with allyl polyoxyethylene ether to obtain amphoteric allyl polyoxyethylene ether, then polymerizes with maleic anhydride, acrylic acid and the like to obtain an amphoteric ether-type polycarboxylic acid water reducer, and finally compounded with cement, fly ash, fiber and the like to obtain large-volume ultra-high performance concrete.
[0025] Amphoteric ether polycarboxylate water-reducing agent contains cationic and anionic zwitterions. The anionic groups such as carboxyl and sulfonic acid groups on the main chain are fixed on the positively charged cement particles, resulting in strong adsorption; quaternary ammonium salt cations can be adsorbed on the surface of negatively charged cement particles, which enhances the steric hindrance effect, gradually increases the charge density, and enhances the electrostatic repulsion between cement particles; at the same time, the cross-linked polyoxyethylene ether side chains in the polycarboxylate water-reducing agent extend radially, have a strong steric hindrance effect, can effectively prevent the agglomeration of cement particles, improve the dispersibility and water reduction rate of cement particles, and show higher cement paste flow properties.
[0026] Amphoteric ether polycarboxylate water reducer has the dual superposition effect of steric hindrance and amphoteric charge attraction, which improves the steric hindrance effect between cement particles, fully disperses the cement particles that were originally bonded to each other, keeps them independent of each other, promotes the hydration of cement particles, fully stimulates the bonding effect of unit cement components, avoids concentrated heat release, and greatly improves the working performance and mechanical properties of concrete; amphoteric ether polycarboxylate water reducer can slow down the speed of early cement hydration, reduce the cracking tendency caused by temperature difference stress, avoid internal hydration heat release, and cause excessive temperature. When the hydration reaction is in progress, the cement paste is alkaline. The molecules of the polycarboxylate water-reducing agent contain sulfonic acid, carboxylic acid and other groups, which can adsorb and disperse the cement particles, thereby achieving a slow-release effect. In addition, the quaternary ammonium salt cations adsorbed on the surface of the negatively charged cement particles can inhibit the expansion of the soil, so that the polyoxyethylene ether side chain of the water-reducing agent will not react with the soil through intercalation, reducing the adsorption of the soil on the admixture and improving the tolerance of the polycarboxylate water-reducing agent to the soil. At the same time, the addition of the concrete hydration heat inhibitor has the effect of slowing down the heat release rate of the concrete hydration reaction.
[0027] By optimizing the selection of steel fibers, it is ensured that the concrete forms a good tensile strength during the period of shrinkage stress, providing sufficient resistance for the concrete to resist the shrinkage of components and avoid cracking; by adding polypropylene fibers, the heat release and temperature rise of cement hydration are used to stimulate the contraction of the fibers. The concrete matrix expands due to heat, and the fibers shrink in the opposite direction. The fiber retraction force is transmitted to the hardened slurry through interfacial bonding, and then micro-prestress is applied to the cementitious slurry on a "micro-meso" scale. The micro-prestress generated by countless evenly dispersed fibers is superimposed, forming a "macro" three-dimensional prestressing effect on the concrete as a whole, partially or completely offsetting the tensile stress generated by the internal and external temperature difference in the large-volume concrete during the construction stage, thereby improving the crack resistance of the large-volume concrete in the temperature rising and falling stages. DETAILED DESCRIPTION
[0028] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] Hydration temperature rise inhibitor: produced by Jiangsu Subote New Materials Co., Ltd., white powder, fineness (1.18mm sieve residue) ≦0.50%, total alkali content ≦0.60%, chloride ion content ≦0.05%.
[0030] Fly ash: Hubei Huadian Grade II fly ash, loss on ignition is 5.80%, density is 2-3g / cm 3 , bulk density 0.5-0.8kg / m 3 .
[0031] Allyl polyoxyethylene ether (APEG-2400), produced by Hai'an Petrochemical Co., Ltd., Jiangsu Province.
[0032] Preparation of 2,3-epoxypropyldimethylamine: Add 6 g of 3-dimethylamino-1,2-propylene glycol and 50 mL of toluene to a reaction flask, stir evenly, add 13.4 g of triphenylphosphine and 7.5 mL of diethyl azodicarboxylate, react at 110 ° C for 4 h, cool, and concentrate under reduced pressure to obtain 2,3-epoxypropyldimethylamine (structural formula: ).
[0033] Example 1
[0034] (1) Add 25 mmol of 2,3-epoxypropyldimethylamine and 100 mL of chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add 27.5 mmol of sodium 2-chloroethane-1-sulfonate, react at 55 °C for 64 h, cool to room temperature, filter, wash with ether, and dry to obtain 2,3-epoxypropyl betaine intermediate.
[0035] (2) Add 5 mmol of allyl polyoxyethylene ether 2400 and 15 mL of deionized water to a reaction flask equipped with a reflux condenser. After stirring evenly, add 5.3 mmol of 2,3-epoxypropyl betaine intermediate and 30% by mass sodium hydroxide aqueous solution to adjust the pH to 10. React at 50 °C for 7 h, add glacial acetic acid to neutralize, and concentrate to dryness to obtain amphoteric allyl polyoxyethylene ether.
[0036] (3) Add 3 mmol of amphoteric allyl polyoxyethylene ether, 2 mmol of maleic anhydride and 80 mL of deionized water to a reaction flask equipped with a reflux condenser and a dropping funnel. After stirring evenly, add 10 mmol of acrylic acid and 0.4 mmol of ammonium persulfate dropwise at the same time. React at 70 °C for 4 h, cool to 45 °C, add sodium hydroxide aqueous solution to adjust the pH to 7, and continue stirring for 15 min to obtain an amphoteric ether-type polycarboxylic acid water reducer.
[0037] Example 2
[0038] (1) Add 40 mmol of 2,3-epoxypropyldimethylamine and 120 mL of chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add 42 mmol of sodium 2-chloroethane-1-sulfonate, react at 45 °C for 72 h, cool to room temperature, filter, wash with ether, and dry to obtain a 2,3-epoxypropyl betaine intermediate.
[0039] (2) Add 3 mmol of allyl polyoxyethylene ether 2400 and 12 mL of deionized water to a reaction flask equipped with a reflux condenser. After stirring evenly, add 3.15 mmol of 2,3-epoxypropyl betaine intermediate and 25% by mass sodium hydroxide aqueous solution to adjust the pH to 11. React at 40 °C for 8 h, add glacial acetic acid to neutralize, and concentrate to dryness to obtain amphoteric allyl polyoxyethylene ether.
[0040] (3) To a reaction flask equipped with a reflux condenser and a dropping funnel, 3.3 mmol of amphoteric allyl polyoxyethylene ether, 2.5 mmol of maleic anhydride and 24 mL of deionized water were added, and after stirring evenly, 10 mmol of acrylic acid and 0.3 mmol of ammonium persulfate were added dropwise, and the mixture was reacted at 80 °C for 2 h. The temperature was lowered to 50 °C, and an aqueous sodium hydroxide solution was added to adjust the pH to 6. The mixture was stirred for 20 min to obtain an amphoteric ether-type polycarboxylic acid water reducer.
[0041] Example 3
[0042] (1) Add 15 mmol of 2,3-epoxypropyldimethylamine and 75 mL of chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add 17.25 mmol of sodium 2-chloroethane-1-sulfonate, react at 60 °C for 48 h, cool to room temperature, filter, wash with ether, and dry to obtain 2,3-epoxypropyl betaine intermediate.
[0043] (2) Add 2 mmol of allyl polyoxyethylene ether 2400 and 6 mL of deionized water to a reaction flask equipped with a reflux condenser. After stirring evenly, add 2.2 mmol of 2,3-epoxypropyl betaine intermediate and 35% by mass sodium hydroxide aqueous solution to adjust the pH to 10. React at 55 °C for 3 h, add glacial acetic acid to neutralize, and concentrate to dryness to obtain amphoteric allyl polyoxyethylene ether.
[0044] (3) To a reaction flask equipped with a reflux condenser and a dropping funnel, add 3.7 mmol of amphoteric allyl polyoxyethylene ether, 3 mmol of maleic anhydride and 100 mL of deionized water. After stirring evenly, add 10 mmol of acrylic acid and 0.5 mmol of ammonium persulfate dropwise at the same time. The mixture is reacted at 60 °C for 5 h, cooled to 40 °C, and sodium hydroxide aqueous solution is added to adjust the pH to 7. The mixture is stirred for 10 min to obtain an amphoteric ether-type polycarboxylic acid water reducer.
[0045] Example 4
[0046] (1) Add 22 mmol of 2,3-epoxypropyldimethylamine and 99 mL of chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add 25.3 mmol of sodium 2-chloroethane-1-sulfonate, react at 55 °C for 60 h, cool to room temperature, filter, wash with ether, and dry to obtain 2,3-epoxypropyl betaine intermediate.
[0047] (2) Add 8 mmol of allyl polyoxyethylene ether 2400 and 24 mL of deionized water to a reaction flask equipped with a reflux condenser. After stirring evenly, add 8.48 mmol of 2,3-epoxypropyl betaine intermediate and 30% by mass sodium hydroxide aqueous solution to adjust the pH to 11. React at 45 °C for 5 h, add glacial acetic acid to neutralize, and concentrate to dryness to obtain amphoteric allyl polyoxyethylene ether.
[0048] (3) To a reaction flask equipped with a reflux condenser and a dropping funnel, add 4.1 mmol of amphoteric allyl polyoxyethylene ether, 1.5 mmol of maleic anhydride and 90 mL of deionized water. After stirring evenly, add 10 mmol of acrylic acid and 0.45 mmol of ammonium persulfate dropwise at the same time. The mixture is reacted at 75 °C for 4 h. The temperature is lowered to 45 °C. An aqueous sodium hydroxide solution is added to adjust the pH to 7. The mixture is stirred for 15 min to obtain an amphoteric ether-type polycarboxylic acid water reducer.
[0049] Example 5
[0050] (1) Add 9 mmol of 2,3-epoxypropyldimethylamine and 45 mL of chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add 9.72 mmol of sodium 2-chloroethane-1-sulfonate, react at 55 °C for 72 h, cool to room temperature, filter, wash with ether, and dry to obtain 2,3-epoxypropyl betaine intermediate.
[0051] (2) Add 12 mmol of allyl polyoxyethylene ether 2400 and 36 mL of deionized water to a reaction flask equipped with a reflux condenser. After stirring evenly, add 12.6 mmol of 2,3-epoxypropyl betaine intermediate and 28% by mass sodium hydroxide aqueous solution to adjust the pH to 10. React at 50 °C for 6 h, add glacial acetic acid to neutralize, and concentrate to dryness to obtain amphoteric allyl polyoxyethylene ether.
[0052] (3) To a reaction flask equipped with a reflux condenser and a dropping funnel, add 4.5 mmol of amphoteric allyl polyoxyethylene ether, 2 mmol of maleic anhydride and 60 mL of deionized water, stir evenly, and then drop 10 mmol of acrylic acid and 0.3 mmol of ammonium persulfate. The mixture is reacted at 65 °C for 4 h, cooled to 40 °C, and sodium hydroxide aqueous solution is added to adjust the pH to 7. The mixture is stirred for 20 min to obtain an amphoteric ether-type polycarboxylic acid water reducer.
[0053] Comparative Example 1
[0054] (1) Add 5 mmol of allyl polyoxyethylene ether 2400 and 15 mL of deionized water to a reaction flask equipped with a reflux condenser, stir evenly, and then add 5.3 mmol of 2,3-epoxypropyltrimethylammonium chloride (structural formula: , CAS No. 3033-77-0) and 30% by mass sodium hydroxide aqueous solution to adjust the pH to 10, react at 50°C for 7h, add glacial acetic acid to neutralize, concentrate and dry to obtain cationic allyl polyoxyethylene ether.
[0055] (2) Add 3.5 mmol of cationic allyl polyoxyethylene ether, 2 mmol of maleic anhydride and 80 mL of deionized water to a reaction flask equipped with a reflux condenser and a dropping funnel. After stirring evenly, add 10 mmol of acrylic acid and 0.4 mmol of ammonium persulfate dropwise at the same time. React at 70 °C for 4 h, cool to 45 °C, add sodium hydroxide aqueous solution to adjust the pH to 7, and continue stirring for 15 min to obtain a cationic ether-type polycarboxylic acid water reducer.
[0056] Comparative Example 2
[0057] (1) Add 3.5 mmol of allyl polyoxyethylene ether 2400, 2 mmol of maleic anhydride and 80 mL of deionized water to a reaction flask equipped with a reflux condenser and a dropping funnel. After stirring evenly, add 10 mmol of acrylic acid and 0.4 mmol of ammonium persulfate dropwise at the same time. React at 70 °C for 4 h, cool to 45 °C, add sodium hydroxide aqueous solution to adjust the pH to 7, and continue stirring for 15 min to obtain an ether-type polycarboxylic acid water reducer.
[0058] Cement paste fluidity test: refer to GB8077-2000 "Concrete admixture homogeneity test method", weigh 300g cement and pour it into a wiped mixing pot, then place it on a cement paste mixer, add 5g of the ether-type polycarboxylate water-reducing agent prepared in the embodiment and the comparative example and 87g of water respectively, stir for 5min, and immediately inject the mixed slurry into a truncated cone circular mold placed on a horizontal glass plate, scrape it flat with a scraper, lift the truncated cone mold vertically and quickly, and let the cement paste flow on the glass plate. After 30s, use a ruler to measure the maximum diameters of the two directions perpendicular to each other of the flowing part, and take the average value as the flow value of the cement paste; then put it into a beaker, stir it again after 2h, repeat the operation, and measure the fluidity of the cement paste.
[0059] Table 1 Cement paste fluidity test
[0060] The fluidity of cement paste is also called the flowability of cement slurry. It is an indicator for evaluating the fluidity of cement slurry. It reflects the adaptability of cement and admixtures and has a great influence on the quality and performance of ready-mixed concrete. It can be seen from the test results in the above table that when the prepared amphoteric ether type polycarboxylate water reducer is dispersed in cement, the fluidity of cement paste is significantly improved with the increase of the content of amphoteric allyl polyoxyethylene ether. The initial cement paste fluidity in Example 4 reaches 326.8 mm, and the cement paste fluidity after 2 hours is 316.5 mm, indicating that the addition of water reducer effectively improves the fluidity of cement and no obvious flow loss occurs after 2 hours. This is because On the one hand, the cross-linked polyoxyethylene ethers in the polycarboxylic acid water-reducing agent have a strong steric hindrance effect. The anionic groups such as the carboxyl group and the sulfonic acid group on the main chain are fixed on the cement particles, resulting in strong adsorption. The side chains of the polyoxyethylene ether are suspended in the solution, which helps the side chains of the polyoxyethylene ether to extend radially and form a hydration film, which plays a role in water reduction, slowing down setting and preventing collapse. On the other hand, the increase in the cationic content enhances the steric hindrance effect and gradually increases the charge density. It is adsorbed on the surface of the negatively charged cement particles, the adsorption amount of the cement particles increases, the electrostatic repulsion between the cement particles continues to increase, the dispersion performance of the cement is improved, and the cement paste exhibits higher flow properties.
[0061] Comparative Example 1 does not contain sulfonic acid anion groups, and the adsorption of cement is easily saturated, resulting in poor dispersion performance of cement paste; Comparative Example 2 contains only carboxylic acid groups and polyoxyethylene ether long chains, and does not contain quaternary ammonium salt cations and sulfonic acid anions, which slows down its adsorption on cement particles, curls the side chains, and reduces the electrostatic repulsion and steric hindrance effects, affecting the dispersibility of the cement system.
[0062] Example 6
[0063] 32g of low-heat silicate cement, 20g of crushed stone, 16g of quartz sand, 10g of fly ash, 5g of copper-plated steel fiber with a diameter of 0.2mm and a length of 15mm, and 0.2g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 40s. After mixing evenly, 12g of deionized water and 0.25g of calcium oxide expansion agent were added, mixed and stirred for 8min, and then 0.3g of amphoteric ether type polycarboxylate water reducer (prepared in Example 4) and 3g of polypropylene fiber were added, stirred for 15min, and naturally cured after molding to obtain large-volume ultra-high performance concrete.
[0064] Example 7
[0065] 30g of low-heat silicate cement, 25g of crushed stone, 16g of quartz sand, 12g of fly ash, 3g of copper-plated steel fiber with a diameter of 0.25mm and a length of 10mm, and 0.4g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 50s. After mixing evenly, 10g of deionized water and 0.1g of calcium oxide expansion agent were added, mixed and stirred for 10min, and then 0.6g of amphoteric ether type polycarboxylate water reducer (prepared in Example 4) and 2g of polypropylene fiber were added, stirred for 20min, and naturally cured after molding to obtain large-volume ultra-high performance concrete.
[0066] Example 8
[0067] 35g of low-heat silicate cement, 18g of crushed stone, 22g of quartz sand, 12g of fly ash, 6g of copper-plated steel fiber with a diameter of 0.2mm and a length of 10mm, and 0.6g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 30s. After mixing evenly, 15g of deionized water and 0.5g of calcium oxide expansion agent were added, mixed and stirred for 6min, and then 0.9g of amphoteric ether type polycarboxylate water reducer (prepared in Example 4) and 2g of polypropylene fiber were added, stirred for 10min, and naturally cured after molding to obtain large-volume ultra-high performance concrete.
[0068] Example 9
[0069] 31g of low-heat silicate cement, 23g of crushed stone, 18g of quartz sand, 9g of fly ash, 5g of copper-plated steel fiber with a diameter of 0.23mm and a length of 12mm, and 0.8g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 35s. After mixing evenly, 15g of deionized water and 0.4g of calcium oxide expansion agent were added, mixed and stirred for 9min, and then 1.2g of amphoteric ether type polycarboxylate water reducer (prepared in Example 4) and 3g of polypropylene fiber were added, stirred for 16min, and naturally cured after molding to obtain large-volume ultra-high performance concrete.
[0070] Example 10
[0071] (4) 33 g of low-heat silicate cement, 22 g of crushed stone, 20 g of quartz sand, 12 g of fly ash, 5 g of copper-plated steel fiber with a diameter of 0.2 mm and a length of 14 mm, and 1 g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 45 seconds. After mixing evenly, 15 g of deionized water and 0.5 g of calcium oxide expansion agent were added and mixed and stirred for 8 minutes. Then, 1.5 g of amphoteric ether type polycarboxylate water reducer (prepared in Example 4) and 3 g of polypropylene fiber were added and stirred for 15 minutes. After molding, the mixture was naturally cured to obtain a large-volume ultra-high performance concrete.
[0072] Comparative Example 3
[0073] (3) 32 g of low-heat silicate cement, 20 g of crushed stone, 16 g of quartz sand, 10 g of fly ash, 5 g of copper-plated steel fiber with a diameter of 0.2 mm and a length of 15 mm, and 0.2 g of hydration temperature rise inhibitor were poured into a concrete mixer and dry-mixed for 4 min. After mixing evenly, 12 g of deionized water and 0.25 g of calcium oxide expansion agent were added and mixed and stirred for 8 min. Then, 0.3 g of cationic ether type polycarboxylate water reducer (prepared in Comparative Example 1) and 3 g of polypropylene fiber were added and stirred for 15 min. After molding, the mixture was naturally cured to obtain concrete.
[0074] Comparative Example 4
[0075] 32g of low-heat silicate cement, 20g of crushed stone, 16g of quartz sand, 10g of fly ash, 5g of copper-plated steel fiber with a diameter of 0.2mm and a length of 15mm and 0.2g of hydration temperature rise inhibitor were poured into a concrete mixer and dry mixed for 4 minutes. After mixing evenly, 12g of deionized water and 0.25g of calcium oxide expansion agent were added and mixed and stirred for 8 minutes. Then, 0.3g of polyether water reducer (prepared in Comparative Example 2) and 3g of polypropylene fiber were added and stirred for 15 minutes. After forming, natural curing was carried out to obtain concrete.
[0076] Comparative Example 5
[0077] 32g of low-heat Portland cement, 20g of crushed stone, 16g of quartz sand, 10g of fly ash, 5g of copper-plated steel fiber with a diameter of 0.2mm and a length of 15mm and 0.2g of hydration temperature rise inhibitor were poured into a concrete mixer and dry mixed for 4 minutes. After mixing evenly, 12g of deionized water and 0.25g of calcium oxide expansion agent were added and mixed for 8 minutes. Then, 3g of polypropylene fiber was added and stirred for 15 minutes. After forming, it was naturally cured to obtain concrete.
[0078] Adiabatic temperature rise test: Using an adiabatic temperature rise tester, the prepared concrete material is loaded into an adiabatic temperature rise mold for an adiabatic temperature rise test.
[0079] Concrete setting time test: Test in accordance with JCJ70-90 "Method for Determination of Mortar Setting Time".
[0080] Table 2 Adiabatic temperature rise and setting time test
[0081] It can be seen from the test results in the above table that with the increase of the content of the amphoteric ether polycarboxylate water-reducing agent, the adiabatic temperature rise of the concrete gradually decreases. The adiabatic temperature rise value between 3 days and 28 days in Example 9 only increases by 1.74°C, while the adiabatic temperature rise value of Comparative Example 5, in which no water-reducing agent is added, increases by 5.16°C, indicating that the hydration process of the cement in the example is delayed, the cracking tendency caused by the temperature difference stress is reduced, and the overall heat release process tends to be stable; this is because the amphoteric ether polycarboxylate water-reducing agent can slow down the early cement hydration speed, avoid internal hydration heat release, and cause the temperature to be too high. When the cement hydration reaction is in progress, the cement paste is alkaline. The molecules of the polycarboxylate water-reducing agent contain sulfonic acid, carboxylic acid and other groups, which can adsorb and disperse the cement particles, thereby achieving a slow-release effect. In addition, the quaternary ammonium salt cations adsorbed on the surface of the negatively charged cement particles can inhibit the expansion of the soil, so that the polyoxyethylene ether side chain of the water-reducing agent will not react with the soil through intercalation, reducing the adsorption of the soil on the admixture and improving the tolerance of the polycarboxylate water-reducing agent to the soil. At the same time, the addition of the concrete hydration heat inhibitor has the effect of slowing down the heat release rate of the concrete hydration reaction.
[0082] Compressive strength test: Tested in accordance with GB / T 31387-2015 "Reactive Powder Concrete" and GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0083] Tensile strength test: Tested in accordance with standard T / CECS 10107 "Technical Requirements for Ultra-High Performance Concrete (RPC)".
[0084] Elastic modulus test: Tested in accordance with GB / T 31387-2015 "Reactive Powder Concrete" and GB / T 50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0085] Table 3 Concrete mechanical properties test
[0086] It can be seen from the test results in the above table that with the increase of the content of amphoteric ether polycarboxylate water-reducing agent, the compressive strength, tensile strength and elastic modulus of concrete are significantly improved. This is because the polar groups in the amphoteric ether polycarboxylate water-reducing agent can effectively improve the solid-liquid surface tension of cement particles and the electrostatic repulsion between molecules, improve the steric hindrance effect between cement particles, fully disperse the cement particles that were originally bonded to each other, keep them independent of each other, promote the hydration of cement particles, fully stimulate the bonding effect of unit cement components, avoid concentrated heat release, and greatly improve the working performance and mechanical properties of concrete.
[0087] Slump and expansion test: refer to GBT 50080-2016 "Standard for test methods of performance of ordinary concrete mixtures" for testing.
[0088] Shrinkage test: Test in accordance with GB / T 50082-2009 "Standard for test methods of long-term performance and durability of ordinary concrete".
[0089] Table 4 Slump, expansion and total shrinkage test
[0090] Generally speaking, the greater the slump, the better the fluidity of the concrete, and the greater the expansion. This is because the concrete with a larger slump has smaller viscosity and internal friction, and is more likely to expand. It can be seen from the test results in the above table that the large-volume ultra-high performance concrete prepared by the present invention has good slump retention, which reduces the volume shrinkage of the concrete and makes its performance more superior.
[0091] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A large volume ultra-high performance concrete, characterized in that: The concrete comprises the following components in parts by weight: 30-35 parts of cement, 10-15 parts of deionized water, 18-25 parts of crushed stone, 16-22 parts of quartz sand, 5-12 parts of fly ash, 3-6 parts of steel fiber, 2-5 parts of polypropylene fiber, 0.3-1.5 parts of amphoteric ether type polycarboxylate water reducer, 0.2-1 parts of hydration temperature rise inhibitor, and 0.1-0.5 parts of expansion agent; The preparation process of the large-volume ultra-high performance concrete is as follows: weigh the above-mentioned weight components of cement, crushed stone, quartz sand, fly ash, steel fiber and hydration temperature rise inhibitor, pour them into a concrete mixer and dry mix them for 30-50 seconds, after mixing evenly, add deionized water and expansion agent, mix and stir for 6-10 minutes, then add amphoteric ether type polycarboxylate water reducer and polypropylene fiber, stir for 10-20 minutes, and naturally cure after forming to obtain a large-volume ultra-high performance concrete; The preparation process of the amphoteric ether type polycarboxylate water reducer is: (1) Add 2,3-epoxypropyldimethylamine and chloroform to a reaction flask equipped with a reflux condenser, stir evenly, then add sodium 2-chloroethane-1-sulfonate, stir to react, and after the reaction is completed, cool to room temperature, filter, wash with ether, and dry to obtain a 2,3-epoxypropyl betaine intermediate; (2) Add allyl polyoxyethylene ether and deionized water to a reaction flask equipped with a reflux condenser, stir evenly, add 2,3-epoxypropyl betaine intermediate and sodium hydroxide aqueous solution, adjust the pH to 10-11, stir to react, add glacial acetic acid to neutralize after the reaction is completed, concentrate and dry to obtain amphoteric allyl polyoxyethylene ether; (3) Add amphoteric allyl polyoxyethylene ether, maleic anhydride and deionized water to a reaction flask equipped with a reflux condenser and a dropping funnel, stir evenly, and then drop acrylic acid and ammonium persulfate at the same time, react at 60-80°C for 2-5h, cool to 40-50°C, add sodium hydroxide aqueous solution to adjust the pH to 6-7, and continue stirring for 10-20min to obtain an amphoteric ether type polycarboxylic acid water reducer; In the step (1), the ratio of 2,3-epoxypropyldimethylamine to sodium 2-chloroethane-1-sulfonate is 1 mol: (1.05-1.15) mol; In the step (2), the ratio of allyl polyoxyethylene ether to 2,3-epoxypropyl betaine intermediate is 1 mol: (1.02-1.1) mol; In the step (3), the ratio of the amphoteric allyl polyoxyethylene ether, maleic anhydride, acrylic acid and ammonium persulfate is (0.3-0.45) mol: (0.1-0.3) mol: 1 mol: (0.03-0.05) mol.
2. The large volume ultra-high performance concrete according to claim 1, characterized in that: The cement is low-heat silicate cement, and the expansion agent is calcium oxide expansion agent.
3. The large volume ultra-high performance concrete according to claim 1, characterized in that: The steel fiber is a copper-plated steel fiber with a diameter of 0.2-0.25 mm and a length of 10-15 mm.
4. The large volume ultra-high performance concrete according to claim 1, characterized in that: In the step (1), the reaction temperature is 45-60° C. and the reaction time is 48-72 h.
5. The large volume ultra-high performance concrete according to claim 1, characterized in that: The mass fraction of the sodium hydroxide aqueous solution in step (2) is 25-35%.
6. The large volume ultra-high performance concrete according to claim 1, characterized in that: In the step (2), the reaction temperature is 40-55° C. and the reaction time is 3-8 h.
Citation Information
Patent Citations
Preparation method and application for amphoteric polycarboxylate water reducer containing anions and cations
CN103992442A
Marine ultra-high performance concrete and preparation method thereof
CN110627453A
Low-temperature-rise and high-crack-resistance mass concrete as well as preparation method and application thereof
CN116768557A