A cable jacket containing a composite flame retardant and a charging pile cable and a preparation method thereof

By using a composite flame retardant compounded with amidinourea phosphate, decabromide diphenyl ether, and tribromide neopentyl alcohol in the charging pile cable, combining polyvinyl chloride and filler to form a high-performance cable jacket, the charging pile cable is solved. The problem of fire risk during high-power charging achieves higher safety and wear resistance.

CN118325253BActive Publication Date: 2024-11-05GUANGDONG XINLIWAN CABLE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410505162.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-05
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing charging pile cables are prone to electrical accidents during high-power charging, and existing flame retardant materials are difficult to meet their flame retardant needs.

Method used

Compound flame retardant is made of amidinourea phosphate, decabromide diphenyl ether, tribromide neopentyl alcohol, and combined with polyvinyl chloride, filler, and composite additives to form a high-performance cable jacket to improve the charging pile cable Flame retardant performance.

Benefits of technology

It significantly improves the safety of charging pile cables, reduces fire risks, and is not prone to flammability in electrical accidents, improving the wear resistance and life of the cable.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of charging pile cables, and specifically discloses a cable jacket containing a composite flame retardant, a charging pile cable and a preparation method thereof, wherein the cable jacket containing the composite flame retardant is made of a composite resin; the composite resin comprises the following components by mass: 100 parts of polyvinyl chloride; 6-8 parts of filler; 4.6-5.2 parts of composite flame retardant; 60.5-65.7 parts of composite auxiliary agent; the composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol. The present invention has the advantage of further improving the flame retardant performance of the charging pile cable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of charging pile cables, and in particular to a cable jacket containing a composite flame retardant and a charging pile cable and a preparation method thereof. Background Art

[0002] A cable is a device composed of several wires used for transmitting electrical energy or signals. With the rapid development of new energy vehicles, charging piles have also developed rapidly. Charging piles are energy replenishment devices that provide power for new energy vehicles. Therefore, charging piles need to be connected to power sources or cars through cables to achieve the transmission of electrical energy to replenish power for new energy vehicles.

[0003] In order to facilitate the use of new energy vehicles, they need to be charged quickly. The battery capacity of new energy vehicles is large. Therefore, in the process of charging new energy vehicles, more electric energy is transmitted in the cable. When a large amount of electric energy is transmitted, once an electrical accident such as short circuit or overload occurs, it is easy to quickly cause a fire. Therefore, the charging pile cable needs to have good flame retardant properties to ensure the safety of the charging pile facilities.

[0004] Cables mainly protect wires by wrapping cable jackets on the surface of several wires. By improving the flame retardant properties of cable jackets, the fire resistance of cables can be effectively improved. Existing cable jackets are mainly made of plastic and rubber, so that the cable jackets have good wear resistance to better protect the wires in the cable. By adding flame retardants to plastic, rubber and other materials, the flame retardant properties of the cable jacket can be improved to a certain extent. However, the charging pile cable has a large amount of power transmission. Once an electrical accident occurs, a large amount of heat will be generated instantly. The flame retardant properties of existing flame retardant plastics and rubbers are still difficult to meet the flame retardant requirements of charging pile cables. Therefore, there is still room for improvement. Summary of the invention

[0005] In order to further improve the flame retardant performance of charging pile cables, the present application provides a cable jacket containing a composite flame retardant and a charging pile cable and a preparation method thereof.

[0006] In a first aspect, the present application provides a cable jacket containing a composite flame retardant, which adopts the following technical solution:

[0007] A cable jacket containing a composite flame retardant, made of a composite resin;

[0008] The composite resin comprises the following components in parts by weight:

[0009] 100 parts of polyvinyl chloride;

[0010] 6-8 parts of filler;

[0011] Composite flame retardant 4.6-5.2 parts;

[0012] Composite additives 60.5-65.7 parts;

[0013] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0014] By adopting the above technical scheme, by specifically selecting a composite flame retardant formed by compounding guanyl urea phosphate, decabromodiphenyl ether, and tribromoneopentyl alcohol, the composite flame retardant can be added to polyvinyl chloride to significantly improve the flame retardant properties of polyvinyl chloride. The prepared cable jacket can greatly improve the safety of the charging pile cable, and electrical accidents in the process of high-power charging are not likely to cause the charging pile cable to burn, which can effectively reduce the risk of fire.

[0015] Preferably, the mass ratio of the guanyl phosphate urea, decabromodiphenyl ether and tribromoneopentyl alcohol is 1.3-1.5:2.6-2.8:0.7-0.9.

[0016] By adopting the above technical scheme and specifically selecting the mass ratio of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentanol, the coordination effect of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentanol is better, thereby further improving the flame retardant properties of polyvinyl chloride and making the prepared charging pile cable safer.

[0017] Preferably, the composite auxiliary agent includes a compound of a plasticizer, a lubricant and a heat stabilizer.

[0018] By adopting the above technical scheme, by adding plasticizers, lubricants and heat stabilizers, the processing performance of polyvinyl chloride is improved, and the dispersion effect of the composite flame retardant in polyvinyl chloride is better, thereby improving the flame retardant performance of polyvinyl chloride.

[0019] Preferably, the plasticizer is dibutyl phthalate, the lubricant is barium stearate, and the heat stabilizer is butyl tin mercaptan.

[0020] By adopting the above technical scheme, by specifically selecting dibutyl phthalate as the plasticizer, barium stearate as the lubricant, and butyl tin mercaptan as the heat stabilizer, the processing performance of polyvinyl chloride can be better improved, and the effect of the composite flame retardant on improving the flame retardant properties of polyvinyl chloride can be better improved.

[0021] Preferably, the mass ratio of the plasticizer, lubricant and heat stabilizer is 60-65:0.2-0.3:0.3-0.4.

[0022] By adopting the above technical solution and specifically selecting the mass ratio of the plasticizer, lubricant and heat stabilizer, the processing performance of polyvinyl chloride can be further improved, thereby achieving higher economic value.

[0023] Preferably, the filler is calcium carbonate whisker.

[0024] By adopting the above technical solution and adding calcium carbonate whiskers, the physical properties of polyvinyl chloride are improved, which better protects the wires in the charging pile cable and prolongs the life of the charging pile cable.

[0025] In a second aspect, the present application provides a charging pile cable, which adopts the following technical solution:

[0026] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant which wraps the plurality of electric wires. The cable jacket containing a composite flame retardant is a cable jacket containing a composite flame retardant made of the composite resin mentioned above.

[0027] By adopting the above technical solution, the charging pile cable has good wear resistance and is not easy to be damaged. In addition, the charging pile cable has good flame retardant properties and is not easy to burn in the event of an electrical accident. It can effectively reduce the probability of fire and has high safety performance.

[0028] In a third aspect, the present application provides a method for preparing a charging pile cable, which adopts the following technical solution:

[0029] A method for preparing a charging pile cable comprises the following steps:

[0030] Step 1), bundling and fixing a plurality of electric wires to form an electric wire bundle;

[0031] Step 2), hot-melt extrude the above-mentioned composite resin onto the surface of the wire bundle to form a cable jacket containing a composite flame retardant that wraps the wire bundle, cool, and reel to obtain a charging pile cable.

[0032] By adopting the above technical solution, the process difficulty of the charging pile cable production process is relatively low, and it has a high economic value. The produced charging pile cable has high flame retardant performance, good safety performance and better quality.

[0033] In summary, this application has the following beneficial effects:

[0034] 1. Since the composite flame retardant is formed by specifically selecting guanyl urea phosphate, decabromodiphenyl ether, and tribromoneopentyl alcohol, the composite flame retardant can significantly improve the flame retardant properties of polyvinyl chloride after being added to polyvinyl chloride. The prepared cable jacket can greatly improve the safety of the charging pile cable, and electrical accidents during high-power charging are not likely to cause the charging pile cable to burn, which can effectively reduce the risk of fire.

[0035] 2. In the present application, it is preferred to specifically select the mass ratio of guanyl urea phosphate, decabromodiphenyl ether, and tribromoneopentyl alcohol so that the coordination effect of guanyl urea phosphate, decabromodiphenyl ether, and tribromoneopentyl alcohol is better, thereby further improving the flame retardant properties of polyvinyl chloride and making the obtained charging pile cable safer.

[0036] 3. In the present application, it is preferred to add plasticizers, lubricants and heat stabilizers to improve the processing performance of polyvinyl chloride, and to make the dispersion effect of the composite flame retardant in polyvinyl chloride better, thereby improving the flame retardant performance of polyvinyl chloride. DETAILED DESCRIPTION

[0037] The present application is further described in detail below with reference to the embodiments.

[0038] Example 1

[0039] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires.

[0040] The jacket of the cable containing composite flame retardant is made of composite resin.

[0041] Composite resins include the following components:

[0042] Polyvinyl chloride, filler, composite flame retardant, composite additive.

[0043] Polyvinyl chloride was purchased from Sinopec, model: S-700.

[0044] The filler is calcium carbonate whisker, purchased from Shijiazhuang Mayue Building Materials Co., Ltd., 325 mesh.

[0045] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0046] Phosphate guanyl urea was purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., CAS No.: 17675-60-4.

[0047] Decabromodiphenyl ether was purchased from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 1163-19-5.

[0048] Tribromoneopentyl alcohol was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd., CAS number: 1522-92-5.

[0049] The composite additive is a compound of plasticizer, lubricant and heat stabilizer.

[0050] The plasticizer is dibutyl phthalate, purchased from Jinan Shanhai Chemical Technology Co., Ltd., CAS No.: 84-74-2.

[0051] The lubricant is barium stearate, purchased from Shandong Guangshen Electronic Technology Co., Ltd., CAS No.: 6865-35-6.

[0052] The heat stabilizer is butyl tin mercaptan, purchased from Hubei Shineng Chemical Technology Co., Ltd., CAS No.: 26410-42-4.

[0053] The preparation method of composite resin is as follows:

[0054] Step 01), 100kg polyvinyl chloride, 6kg calcium carbonate whisker, 1.3kg guanyl phosphate urea, 2.6kg decabromodiphenyl ether, 0.7kg tribromoneopentyl alcohol, 60kg dibutyl phthalate, 0.2kg barium stearate, 0.3kg butyl tin mercaptan are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, to obtain a premix.

[0055] Step 02), the premix is ​​put into a twin-screw extruder for extrusion granulation, the processing temperatures of the twin-screw extruder zones I-XI are set to: 150°C, 150°C, 160°C, 170°C, 180°C, 180°C, 180°C, 190°C, 190°C, 190°C, the main screw speed is 60r / min, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a composite resin.

[0056] The preparation method of the charging pile cable is as follows:

[0057] Step 1), several electric wires are arranged in parallel, and then tied and fixed with copper wire to form a wire bundle.

[0058] Step 2), putting the composite resin into a cable extruder, and hot-melt-extrude the composite resin onto the surface of the wire bundle through the cable extruder to form a cable jacket containing a composite flame retardant that wraps the wire bundle. The extrusion temperature is 200°C, the extrusion speed is 2mm / s, and the mixture is naturally cooled and rolled up to obtain a charging pile cable.

[0059] Example 2

[0060] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires.

[0061] The jacket of the cable containing composite flame retardant is made of composite resin.

[0062] Composite resins include the following components:

[0063] Polyvinyl chloride, filler, composite flame retardant, composite additive.

[0064] Polyvinyl chloride was purchased from Sinopec, model: S-700.

[0065] The filler is calcium carbonate whisker, purchased from Shijiazhuang Mayue Building Materials Co., Ltd., 325 mesh.

[0066] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0067] Phosphate guanyl urea was purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., CAS No.: 17675-60-4.

[0068] Decabromodiphenyl ether was purchased from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 1163-19-5.

[0069] Tribromoneopentyl alcohol was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd., CAS number: 1522-92-5.

[0070] The composite additive is a compound of plasticizer, lubricant and heat stabilizer.

[0071] The plasticizer is dibutyl phthalate, purchased from Jinan Shanhai Chemical Technology Co., Ltd., CAS No.: 84-74-2.

[0072] The lubricant is barium stearate, purchased from Shandong Guangshen Electronic Technology Co., Ltd., CAS No.: 6865-35-6.

[0073] The heat stabilizer is butyl tin mercaptan, purchased from Hubei Shineng Chemical Technology Co., Ltd., CAS No.: 26410-42-4.

[0074] The preparation method of composite resin is as follows:

[0075] Step 01), 100kg polyvinyl chloride, 7kg calcium carbonate whisker, 1.4kg guanyl phosphate urea, 2.7kg decabromodiphenyl ether, 0.8kg tribromoneopentyl alcohol, 62.5kg dibutyl phthalate, 0.25kg barium stearate, 0.35kg butyl tin mercaptan are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, and obtaining a premix.

[0076] Step 02), the premix is ​​put into a twin-screw extruder for extrusion granulation, the processing temperatures of the twin-screw extruder zones I-XI are set to: 150°C, 150°C, 160°C, 170°C, 180°C, 180°C, 180°C, 190°C, 190°C, 190°C, the main screw speed is 60r / min, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a composite resin.

[0077] The preparation method of the charging pile cable is as follows:

[0078] Step 1), several electric wires are arranged in parallel, and then tied and fixed with copper wire to form a wire bundle.

[0079] Step 2), putting the composite resin into a cable extruder, and hot-melt-extrude the composite resin onto the surface of the wire bundle through the cable extruder to form a cable jacket containing a composite flame retardant that wraps the wire bundle. The extrusion temperature is 200°C, the extrusion speed is 2mm / s, and the mixture is naturally cooled and rolled up to obtain a charging pile cable.

[0080] Example 3

[0081] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires.

[0082] The jacket of the cable containing composite flame retardant is made of composite resin.

[0083] Composite resins include the following components:

[0084] Polyvinyl chloride, filler, composite flame retardant, composite additive.

[0085] Polyvinyl chloride was purchased from Sinopec, model: S-700.

[0086] The filler is calcium carbonate whisker, purchased from Shijiazhuang Mayue Building Materials Co., Ltd., 325 mesh.

[0087] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0088] Phosphate guanyl urea was purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., CAS No.: 17675-60-4.

[0089] Decabromodiphenyl ether was purchased from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 1163-19-5.

[0090] Tribromoneopentyl alcohol was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd., CAS number: 1522-92-5.

[0091] The composite additive is a compound of plasticizer, lubricant and heat stabilizer.

[0092] The plasticizer is dibutyl phthalate, purchased from Jinan Shanhai Chemical Technology Co., Ltd., CAS No.: 84-74-2.

[0093] The lubricant is barium stearate, purchased from Shandong Guangshen Electronic Technology Co., Ltd., CAS No.: 6865-35-6.

[0094] The heat stabilizer is butyl tin mercaptan, purchased from Hubei Shineng Chemical Technology Co., Ltd., CAS No.: 26410-42-4.

[0095] The preparation method of composite resin is as follows:

[0096] Step 01), 100kg polyvinyl chloride, 8kg calcium carbonate whisker, 1.5kg guanyl phosphate urea, 2.8kg decabromodiphenyl ether, 0.9kg tribromoneopentyl alcohol, 65kg dibutyl phthalate, 0.3kg barium stearate, 0.4kg butyl tin mercaptan are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, to obtain a premix.

[0097] Step 02), the premix is ​​put into a twin-screw extruder for extrusion granulation, the processing temperatures of the twin-screw extruder zones I-XI are set to: 150°C, 150°C, 160°C, 170°C, 180°C, 180°C, 180°C, 190°C, 190°C, 190°C, the main screw speed is 60r / min, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a composite resin.

[0098] The preparation method of the charging pile cable is as follows:

[0099] Step 1), several electric wires are arranged in parallel, and then tied and fixed with copper wire to form a wire bundle.

[0100] Step 2), putting the composite resin into a cable extruder, and hot-melt-extrude the composite resin onto the surface of the wire bundle through the cable extruder to form a cable jacket containing a composite flame retardant that wraps the wire bundle. The extrusion temperature is 200°C, the extrusion speed is 2mm / s, and the mixture is naturally cooled and rolled up to obtain a charging pile cable.

[0101] Example 4

[0102] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires.

[0103] The jacket of the cable containing composite flame retardant is made of composite resin.

[0104] Composite resins include the following components:

[0105] Polyvinyl chloride, filler, composite flame retardant, composite additive.

[0106] Polyvinyl chloride was purchased from Sinopec, model: S-700.

[0107] The filler is calcium carbonate whisker, purchased from Shijiazhuang Mayue Building Materials Co., Ltd., 325 mesh.

[0108] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0109] Phosphate guanyl urea was purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., CAS No.: 17675-60-4.

[0110] Decabromodiphenyl ether was purchased from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 1163-19-5.

[0111] Tribromoneopentyl alcohol was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd., CAS number: 1522-92-5.

[0112] The composite additive is a compound of plasticizer, lubricant and heat stabilizer.

[0113] The plasticizer is dibutyl phthalate, purchased from Jinan Shanhai Chemical Technology Co., Ltd., CAS No.: 84-74-2.

[0114] The lubricant is barium stearate, purchased from Shandong Guangshen Electronic Technology Co., Ltd., CAS No.: 6865-35-6.

[0115] The heat stabilizer is butyl tin mercaptan, purchased from Hubei Shineng Chemical Technology Co., Ltd., CAS No.: 26410-42-4.

[0116] The preparation method of composite resin is as follows:

[0117] Step 01), 100kg polyvinyl chloride, 7kg calcium carbonate whisker, 0.4kg guanyl phosphate urea, 3.2kg decabromodiphenyl ether, 1.3kg tribromoneopentyl alcohol, 62.5kg dibutyl phthalate, 0.25kg barium stearate, 0.35kg butyl tin mercaptan are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, and obtaining a premix.

[0118] Step 02), the premix is ​​put into a twin-screw extruder for extrusion granulation, the processing temperatures of the twin-screw extruder zones I-XI are set to: 150°C, 150°C, 160°C, 170°C, 180°C, 180°C, 180°C, 190°C, 190°C, 190°C, the main screw speed is 60r / min, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a composite resin.

[0119] The preparation method of the charging pile cable is as follows:

[0120] Step 1), several electric wires are arranged in parallel, and then tied and fixed with copper wire to form a wire bundle.

[0121] Step 2), putting the composite resin into a cable extruder, and hot-melt-extrude the composite resin onto the surface of the wire bundle through the cable extruder to form a cable jacket containing a composite flame retardant that wraps the wire bundle. The extrusion temperature is 200°C, the extrusion speed is 2mm / s, and the mixture is naturally cooled and rolled up to obtain a charging pile cable.

[0122] Example 5

[0123] A charging pile cable comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires.

[0124] The jacket of the cable containing composite flame retardant is made of composite resin.

[0125] Composite resins include the following components:

[0126] Polyvinyl chloride, filler, composite flame retardant, composite additive.

[0127] Polyvinyl chloride was purchased from Sinopec, model: S-700.

[0128] The filler is calcium carbonate whisker, purchased from Shijiazhuang Mayue Building Materials Co., Ltd., 325 mesh.

[0129] The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0130] Phosphate guanyl urea was purchased from Zhengzhou Shengyu Chemical Products Co., Ltd., CAS No.: 17675-60-4.

[0131] Decabromodiphenyl ether was purchased from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 1163-19-5.

[0132] Tribromoneopentyl alcohol was purchased from Wuhan Jixinyibang Biotechnology Co., Ltd., CAS number: 1522-92-5.

[0133] The composite additive is a compound of plasticizer, lubricant and heat stabilizer.

[0134] The plasticizer is dibutyl phthalate, purchased from Jinan Shanhai Chemical Technology Co., Ltd., CAS No.: 84-74-2.

[0135] The lubricant is barium stearate, purchased from Shandong Guangshen Electronic Technology Co., Ltd., CAS No.: 6865-35-6.

[0136] The heat stabilizer is butyl tin mercaptan, purchased from Hubei Shineng Chemical Technology Co., Ltd., CAS No.: 26410-42-4.

[0137] The preparation method of composite resin is as follows:

[0138] Step 01), 100kg polyvinyl chloride, 7kg calcium carbonate whisker, 0.9kg guanyl phosphate urea, 2.2kg decabromodiphenyl ether, 1.8kg tribromoneopentyl alcohol, 62.5kg dibutyl phthalate, 0.25kg barium stearate, 0.35kg butyl tin mercaptan are put into a stirring tank, the speed is 120r / min, stirring for 5min, mixing evenly, and obtaining a premix.

[0139] Step 02), the premix is ​​put into a twin-screw extruder for extrusion granulation, the processing temperatures of the twin-screw extruder zones I-XI are set to: 150°C, 150°C, 160°C, 170°C, 180°C, 180°C, 180°C, 190°C, 190°C, 190°C, the main screw speed is 60r / min, the water tank temperature is 25°C during the cooling process, and underwater granulation is performed to obtain a composite resin.

[0140] The preparation method of the charging pile cable is as follows:

[0141] Step 1), several electric wires are arranged in parallel, and then tied and fixed with copper wire to form a wire bundle.

[0142] Step 2), putting the composite resin into a cable extruder, and hot-melt-extrude the composite resin onto the surface of the wire bundle through the cable extruder to form a cable jacket containing a composite flame retardant that wraps the wire bundle. The extrusion temperature is 200°C, the extrusion speed is 2mm / s, and the mixture is naturally cooled and rolled up to obtain a charging pile cable.

[0143] Comparative Example 1

[0144] A charging pile cable, compared with embodiment 2, the only difference is:

[0145] In the composite resin, ammonium dihydrogen phosphate was used to replace guanyl urea phosphate in equal amounts.

[0146] Ammonium dihydrogen phosphate was purchased from Suzhou Bogerui Chemical Technology Co., Ltd.

[0147] Comparative Example 2

[0148] A charging pile cable, compared with embodiment 2, the only difference is:

[0149] In the composite resin, triphenyl phosphate was used to replace decabromodiphenyl ether in equal amounts.

[0150] Triphenyl phosphate was purchased from Dongguan Zhenming Chemical Co., Ltd.

[0151] Comparative Example 3

[0152] A charging pile cable, compared with embodiment 2, the only difference is:

[0153] In the composite resin, diethylaluminum hypophosphite was used in equal amounts to replace tribromoneopentyl alcohol.

[0154] Diethyl aluminum hypophosphite was purchased from Guangzhou Yinyuan New Materials Co., Ltd.

[0155] Comparative Example 4

[0156] A charging pile cable, compared with embodiment 2, the only difference is:

[0157] In the composite resin, ammonium dihydrogen phosphate was used to replace guanyl urea phosphate in an equal amount, triphenyl phosphate was used to replace decabromodiphenyl ether in an equal amount, and diethylaluminum hypophosphite was used to replace tribromoneopentyl alcohol in an equal amount.

[0158] Ammonium dihydrogen phosphate was purchased from Suzhou Bogerui Chemical Technology Co., Ltd.

[0159] Triphenyl phosphate was purchased from Dongguan Zhenming Chemical Co., Ltd.

[0160] Diethyl aluminum hypophosphite was purchased from Guangzhou Yinyuan New Materials Co., Ltd.

[0161] Experiment 1

[0162] According to GB / T2408-2021 "Determination of combustion performance of plastics - horizontal and vertical methods", the flame retardant properties of the samples made of the composite resins of the embodiments and comparative examples were tested. The vertical method was used for testing.

[0163] The specific test data of Experiment 1 are shown in Table 1.

[0164] Table 1

[0165] Flame retardant grade Afterflame time(s) Example 1 V-0 1.3 Example 2 V-0 1.1 Example 3 V-0 1.7 Example 4 V-0 8.9 Example 5 V-0 8.1 Comparative Example 1 V-1 22.9 Comparative Example 2 V-1 23.4 Comparative Example 3 V-1 21.8 Comparative Example 4 V-1 24.5

[0166] According to the data comparison in Table 1, the flame retardant properties of the composite resins in each embodiment are significantly higher than those of the composite resins in each comparative example. It can be seen that when the composite flame retardant is specifically compounded with guanyl urea phosphate, decabromodiphenyl ether, and tribromoneopentyl alcohol, the flame retardant properties of polyvinyl chloride can be effectively and significantly further improved, and the prepared charging pile cable has higher safety performance and higher economic value.

[0167] Although flame retardants were added to the comparative examples, the flame retardant properties decreased due to the destruction of the special matching system of guanidine urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol.

[0168] The flame retardant grade of Example 1-3 is the same as that of Example 4-5, but the afterflame time of Example 1-3 is significantly shorter than that of Example 4-5. It can be seen that when guanyl phosphate urea, decabromodiphenyl ether, and tribromoneopentyl alcohol are compounded in a specific proportion, the flame retardant properties of polyvinyl chloride can be significantly further improved, and the burning time can be greatly shortened, thereby further improving the safety performance of the charging pile cable.

[0169] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A cable jacket containing a composite flame retardant, characterized in that: Made of composite resin; The composite resin comprises the following components in parts by weight: 100 parts of polyvinyl chloride; 6-8 parts of filler; Composite flame retardant 4.6-5.2 parts; Composite additives 60.5-65.7 parts; The composite flame retardant is a compound of guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol; The mass ratio of the guanyl urea phosphate, decabromodiphenyl ether and tribromoneopentyl alcohol is 1.3-1.5:2.6-2.8:0.7-0.

9.

2. The cable jacket containing a composite flame retardant according to claim 1, characterized in that: The composite auxiliary agent comprises a compound of a plasticizer, a lubricant and a heat stabilizer.

3. The cable jacket containing a composite flame retardant according to claim 2, characterized in that: The plasticizer is dibutyl phthalate, the lubricant is barium stearate, and the heat stabilizer is butyl tin mercaptan.

4. The cable jacket containing a composite flame retardant according to claim 3, characterized in that: The mass ratio of the plasticizer, lubricant and heat stabilizer is 60-65: 0.2-0.3:0.3-0.4。 5. The cable jacket containing a composite flame retardant according to claim 1, characterized in that: The filler is calcium carbonate whisker.

6. A charging pile cable, characterized in that: The invention comprises a plurality of electric wires and a cable jacket containing a composite flame retardant and wrapping the plurality of electric wires, wherein the cable jacket containing a composite flame retardant is a cable jacket containing a composite flame retardant made of the composite resin described in any one of claims 1-5.

7. A method for preparing a charging pile cable, characterized in that: The following steps are involved: Step 1), bundling and fixing a plurality of electric wires to form an electric wire bundle; Step 2), hot-melt extrude the composite resin described in any one of claims 1-5 onto the surface of the wire bundle to form a cable jacket containing a composite flame retardant that wraps the wire bundle, cool, and reel to obtain a charging pile cable.