Flame retardant silicone rubber, preparation method thereof and liquid plug

By using specific combinations of flame retardants and platinum complexes in silicone rubber, the flammability problem of silicone rubber under high temperature flame is solved, and its flame retardant and mechanical properties are improved, meeting the needs of flame retardant and mechanical modification. , suitable for applications in complex environments.

CN118325342BActive Publication Date: 2024-11-08NINGBO DEAN PHOTOVOLTAIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410590242.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-13
Publication Date
2024-11-08
Estimated Expiration
2044-05-13

AI Technical Summary

Technical Problem

Existing silicone rubbers are flammable under high temperature flames, the mechanical properties of the flame retardant are degraded after adding the flame retardant, and the flame retardant effect is uneven, making it difficult to meet the needs of flame retardant and mechanical modification.

Method used

Using vinyl-terminated dimethyl methyl vinyl, silane-modified silica, magnesium hydroxide, aluminum hydroxide, octphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyl dimethyl The flame retardant composed of silazane combines platinum complex and vulcanizing agent to improve the flame retardant and mechanical properties of silicone rubber through modification treatment and synergistic action.

Benefits of technology

It achieves excellent flame retardant properties, good compatibility and dispersion of flame retardant silicone rubber, improves its anti-sintering and mechanical properties at high temperatures, and is suitable for electrical appliances, power waterproofing and fire protection in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004837043250000011
    Figure HDA0004837043250000011
  • Figure HDA0004837043250000012
    Figure HDA0004837043250000012
  • Figure HDA0004837043250000021
    Figure HDA0004837043250000021
Patent Text Reader

Abstract

The present application relates to the technical field of silicone rubber preparation, and in particular to a flame retardant silicone rubber, a preparation method thereof and a liquid plug. A flame retardant silicone rubber, by mass, the raw materials for preparation include: 30-55 parts of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 5-15 parts of silane-modified silica, 40-55 parts of flame retardant, 0.06-0.08 parts of platinum complex, 0.5-1 parts of vulcanizing agent, 1.5-3.5 parts of hydroxyl-terminated polydimethylsiloxane, and 1-2 parts of stearate. The flame retardant in the flame retardant silicone rubber prepared in the present application has excellent flame retardant properties, and has good compatibility and good dispersibility in the silicone rubber matrix. The prepared flame retardant silicone rubber has high flame retardant properties and excellent mechanical properties, so that it has a wide range of application prospects in various electrical appliances, power waterproofing and fire protection fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of silicone rubber preparation, and in particular to a flame retardant silicone rubber and a preparation method thereof and a liquid plug. Background Art

[0002] Silicone rubber has excellent properties such as high and low temperature resistance, insulation, and weather resistance. After years of development and utilization, it has been widely used in many fields such as medical and health, aerospace, wire and cable, and automotive industry. However, silicone rubber itself is flammable and will continue to burn once ignited, which seriously limits the application scope of silicone rubber. Although adding flame retardants to silicone rubber will enhance the flame retardant properties of silicone rubber, the addition of flame retardants often affects the mechanical properties of silicone rubber, resulting in a significant decrease in mechanical properties. Therefore, flame retardancy and mechanical modification of silicone rubber are particularly important.

[0003] Silicone rubber is a composite material composed of polysiloxane, reinforcing fillers, crosslinking agents, catalysts and other additives. Due to the high bond energy of Si-O bonds, it has good thermal stability. In addition, when burning under high-temperature flames, Si-O bonds will be transformed into continuous, insulating network-like SiO2 ash covering the surface, thereby effectively preventing further ablation of the substrate. Organic or inorganic flame retardants, such as phosphate esters and phosphazene organic flame retardants, and inorganic flame retardants such as magnesium hydroxide and aluminum hydroxide, are compounded into silicone rubber. The biggest problem with this type of flame retardant during application is that it cannot be evenly dispersed, and obvious ablation unevenness occurs during the ablation process, resulting in an unsatisfactory overall flame retardant effect.

[0004] Therefore, there is an urgent need to develop a flame retardant silicone rubber with good flame retardancy and good mechanical properties to meet market demand. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present application provides a flame retardant silicone rubber and a preparation method thereof and a liquid plug.

[0006] In a first aspect, the present application provides a flame retardant silicone rubber, which adopts the following technical solution:

[0007] A flame retardant silicone rubber, the preparation raw materials of which include, by weight: 30-55 parts of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 5-15 parts of silane-modified silica, 40-55 parts of flame retardant, 0.06-0.08 parts of platinum complex, 0.5-1 parts of vulcanizing agent, 1.5-3.5 parts of hydroxyl-terminated polydimethylsiloxane, 1-2 parts of stearate, wherein the flame retardant is composed of magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane.

[0008] By adopting the above technical scheme, the vinyl-terminated dimethyl methyl vinyl plays the main structural component of the silicone rubber matrix, and has good flexibility and rubber properties. The addition of silane-modified silica to silicone rubber can improve the compatibility of silicone rubber with flame retardants, and at the same time increase the anti-aging and mechanical properties of silicone rubber. Flame retardants are key components for improving the flame retardant properties of silicone rubber. The combination of magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane has good flame retardant, smoke suppression and filling effects. Platinum complexes can improve the heat resistance of silicone rubber at high temperatures, and the combination with nitrogen elements can enhance the flame retardant properties of silicone rubber. Vulcanizers and hydroxyl-terminated polydimethylsiloxane play the role of cross-linking silicone rubber, improving the mechanical properties and stability of silicone rubber. Stearate is used to improve the processing properties and formability of silicone rubber. The synergistic effect between the components makes the flame-retardant silicone rubber finally prepared have improved comprehensive performance, which is suitable for applications in various electrical appliances, power waterproofing and fire protection fields.

[0009] Preferably, the preparation method of the flame retardant is: according to the mass fractions, magnesium hydroxide, aluminum hydroxide and octaphenyl cage silsesquioxane are added to the reactor respectively and stirred evenly, then isopropyl glycidyl ether is added, the temperature is raised to 85-90°C, after mixing evenly, hexamethyldisilazane is finally added and stirred for 20-30 minutes to obtain the flame retardant.

[0010] By adopting the above technical scheme, flame retardants are essential for the performance of flame retardant silicone rubber. The flame retardant is composed of magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane. These flame retardants have flame retardant, smoke suppression and filling functions, and play a role in comprehensively improving the flame retardant and mechanical properties of silicone rubber by cooperating with each other. Magnesium hydroxide and aluminum hydroxide, as excellent flame retardants, help to improve the flame retardant properties of silicone rubber. However, they are easy to agglomerate in organic systems, affecting the dispersibility. Therefore, by adding isopropyl glycidyl ether and hexamethyldisilazane for modification during the preparation process, the dispersibility of magnesium hydroxide and aluminum hydroxide can be improved, so that they are more evenly dispersed in silicone rubber, and at the same time, they can further cross-link with the silicone rubber system to enhance the stability of the cross-linked macromolecular structure, thereby improving the flame retardant and mechanical properties of silicone rubber.

[0011] Preferably, the mass ratio of the magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane is (10-12):(28-30):(5-7):(0.2-0.3):(0.8-1.2), and the particle sizes of the magnesium hydroxide and aluminum hydroxide are both 1-3 μm.

[0012] By adopting the above technical scheme, in the present application, the mass fraction ratio of flame retardants such as magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane is (10-12): (28-30): (5-7): (0.2-0.3): (0.8-1.2), which is conducive to achieving the synergistic effect between these flame retardants and improving the overall performance of flame retardant silicone rubber. Magnesium hydroxide and aluminum hydroxide often agglomerate in organic systems, and after modification with isopropyl glycidyl ether and hexamethyldisilazane, it is conducive to enhancing the dispersibility and compatibility of these flame retardants in the silicone rubber system. Isopropyl glycidyl ether, as a substance with flexibility and molecular coupling effect, cooperates with the role of hexamethyldisilazane as an efficient coupling agent and modifier, which can better promote the dispersion and cross-linking reaction of flame retardants, improve the stability of the silicone rubber system, and thus improve the flame retardant properties and mechanical properties of flame retardant silicone rubber. In addition, the particle sizes of magnesium hydroxide and aluminum hydroxide are both 1-3μm, which is conducive to increasing the surface area of ​​the flame retardant, enhancing its contact area with the silicone rubber matrix, and further improving the flame retardant effect. In general, by reasonably selecting the ratio and particle size range of the flame retardant, and improving its dispersibility and compatibility through modification, the synergistic effect between flame retardants can be achieved in flame retardant silicone rubber, improving the flame retardant performance and mechanical properties of the material, making it more suitable for application requirements in various complex environments.

[0013] Preferably, the silane-modified silica is at least one of 3-aminopropyltrimethoxysilane-modified silica, γ-methacryloxypropyltrimethoxysilane-modified silica, and γ-mercaptopropyltriethoxysilane-modified silica; the average particle size D50 of the silane-modified silica is ≤2 μm; the oil absorption value of the silane-modified silica is 60-80 mL / 100 g; the bulk density of the silane-modified silica is 0.5-0.6 g / cm 3 .

[0014] By adopting the above technical scheme, silane-modified silica plays a role in improving the compatibility with silicone rubber in this application. This silane-modified silica uses different types of silanes, including 3-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, etc. Through the modification of these silanes, the compatibility of silane and silicone rubber can be promoted, so that the silicone rubber material has more stable mechanical properties. In addition, the average particle size D50 of the silane-modified silica is ≤2μm and the oil absorption value is 60-80mL / 100g. These characterization parameters also affect the compatibility and performance of silane-modified silica with silicone rubber. A smaller average particle size is conducive to improving the uniform dispersion of the filler, while the oil absorption value affects the surface activity and colloidal stability of the filler.

[0015] Preferably, the platinum complex is a platinum complex containing a nitrogen-containing ligand, and the nitrogen-containing ligand is one of tetramethylethylenediamine and benzotriazole.

[0016] By adopting the above technical solution, the nitrogen-containing ligand of the platinum complex in this application adopts one of tetramethylethylenediamine and benzotriazole, and these nitrogen-containing ligands can enhance the anti-sintering performance of platinum at high temperatures. Platinum itself has flame retardancy, and nitrogen also has certain flame retardancy, so the combination of nitrogen-containing ligands and platinum ligands can further enhance the flame retardancy of the platinum complex. At the same time, the nitrogen-containing ligand can also enhance the stability and catalytic performance of the complex.

[0017] Preferably, the platinum element in the platinum-gold complex is 80-100 ppm by mass.

[0018] By adopting the above technical scheme, the platinum complex is combined with the platinum ligand through the nitrogen-containing ligand, which enhances the anti-sintering performance of platinum at high temperature. At the same time, platinum itself has good flame retardant properties, and the flame retardant effect can be further improved after combining with nitrogen. In the preparation process of flame-retardant silicone rubber, the platinum complex plays a catalytic role in silicone rubber, enhances the performance of the flame retardant, and improves the flame retardant properties of silicone rubber. The addition of platinum complex can promote the cross-linking reaction in the silicone rubber system and improve the stability of the cross-linked macromolecular structure of the silicone rubber system, thereby producing a synergistic effect with other flame retardants and further improving the overall performance of flame-retardant silicone rubber. In general, by reasonably proportioning and adding platinum complex as a flame retardant, the flame retardant properties of flame-retardant silicone rubber can be effectively improved, and the anti-sintering performance of silicone rubber materials in high temperature environments can be enhanced, which meets the requirements for flame retardant material performance in various electrical appliances, power waterproofing and fire protection fields.

[0019] Preferably, the vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane.

[0020] Preferably, the stearate is at least one of zinc stearate, magnesium stearate and calcium stearate.

[0021] In a second aspect, the present application provides a method for preparing a flame retardant silicone rubber, using the following technical solution:

[0022] As a general technical concept, the present application also provides a method for preparing the flame retardant silicone rubber, comprising the following steps:

[0023] S91, according to the mass parts, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), silane-modified silica and flame retardant are mixed and added into a kneader for heating and kneading, the kneading temperature is 105-115° C., the kneading time is 4-5 hours, and a mixture A is obtained;

[0024] S92, adding the platinum complex to the mixture A according to the parts by mass, and kneading to obtain a mixture B;

[0025] S93, mixing hydroxyl-terminated polydimethylsiloxane and stearate according to parts by mass to prepare a mixture C;

[0026] S94, adding mixture C and a vulcanizing agent to mixture B according to parts by mass, and kneading to obtain mixture D;

[0027] S95. Place the mixture D in a flat vulcanizer for vulcanization. The vulcanization process is as follows: temperature 155-165° C., vulcanization time 20-30 min, to obtain a flame retardant silicone rubber.

[0028] In a third aspect, the present application provides a liquid plug, which adopts the following technical solution:

[0029] The liquid plug is made of the flame retardant silicone rubber material. The flame retardant grade of the liquid plug is V-0 according to ANSI / UL-94-1985 standard. The tensile strength of the liquid plug is 6.8-7.7 MPa, and the oxygen index of the liquid plug is 34-39%.

[0030] In summary, the present application includes at least one of the following beneficial technical effects:

[0031] 1. Excellent flame retardant properties: The flame retardant is composed of magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane. It has flame retardant, smoke suppression and filling functions, and can effectively improve the flame retardant properties of flame retardant silicone rubber to meet the application needs in various fields.

[0032] 2. Good compatibility and dispersibility: The flame retardant has good compatibility and dispersibility with the silicone rubber matrix, and can be more evenly dispersed into the silicone rubber system through the modifier, promoting the cross-linking reaction and improving the overall performance of the silicone rubber.

[0033] 3. Synergistic effect improves performance: Platinum complex enhances the anti-sintering performance at high temperature, and forms a synergistic effect with other flame retardants to jointly improve the flame retardant and mechanical properties of silicone rubber, providing better protection for silicone rubber materials in complex environments.

[0034] 4. Stable mechanical properties: Silane modification treatment improves the compatibility between silica and silicone rubber, making the silicone rubber material have more stable mechanical properties and improving the overall performance of silicone rubber. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A top view of the liquid plug prepared in Example 3;

[0036] Figure 2 A front view of the liquid plug prepared in Example 3;

[0037] Figure 3 A cross-sectional view of the liquid plug prepared in Example 3; DETAILED DESCRIPTION

[0038] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0039] Preparation Example 1 Preparation of flame retardant

[0040] The preparation method of the flame retardant is as follows: according to the mass proportions, 1.0 kg of magnesium hydroxide, 2.8 kg of aluminum hydroxide and 0.5 kg of octaphenyl cage silsesquioxane are added to the reactor respectively and stirred evenly, then 0.02 kg of isopropyl glycidyl ether is added, the temperature is raised to 85° C., after mixing evenly, 0.08 kg of hexamethyldisilazane is finally added and stirred for 20 minutes to obtain the flame retardant, wherein the particle sizes of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm.

[0041] Preparation Example 2 Preparation of flame retardant

[0042] The preparation method of the flame retardant is as follows: according to the mass proportions, 1.2 kg of magnesium hydroxide, 3.0 kg of aluminum hydroxide and 0.7 kg of octaphenyl cage silsesquioxane are added to a reactor and stirred evenly, 0.03 kg of isopropyl glycidyl ether is added, the temperature is raised to 90° C., after mixing evenly, 0.12 kg of hexamethyldisilazane is finally added and stirred for 30 minutes to obtain a flame retardant, wherein the particle sizes of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm.

[0043] Preparation Example 3 Preparation of flame retardant

[0044] The preparation method of the flame retardant is as follows: according to the mass proportions, 1.1 kg of magnesium hydroxide, 2.9 kg of aluminum hydroxide and 0.6 kg of octaphenyl cage silsesquioxane are added to the reactor respectively and stirred evenly, then 0.025 kg of isopropyl glycidyl ether is added, the temperature is raised to 88° C., after mixing evenly, 0.1 kg of hexamethyldisilazane is finally added and stirred for 25 minutes to obtain the flame retardant, wherein the particle sizes of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm.

[0045] Preparation of comparative example 1: Preparation of flame retardant

[0046] The preparation method of the flame retardant is as follows: according to the mass fraction, 4.6 kg of magnesium hydroxide is added into the reactor and stirred evenly, then 0.025 kg of isopropyl glycidyl ether is added, the temperature is raised to 88° C., after mixing evenly, 0.1 kg of hexamethyldisilazane is added and stirred for 25 minutes to obtain the flame retardant, wherein the particle size of the magnesium hydroxide and aluminum hydroxide are both 1-3 μm.

[0047] Preparation of comparative example 2: Preparation of flame retardant

[0048] The preparation method of the flame retardant is as follows: according to the mass fraction, 4.6 kg of aluminum hydroxide is added to the reactor and stirred evenly, then 0.025 kg of isopropyl glycidyl ether is added, the temperature is raised to 88° C., after mixing evenly, 0.1 kg of hexamethyldisilazane is added and stirred for 25 minutes to obtain the flame retardant, and the particle size of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm.

[0049] Preparation of comparative example 3: Preparation of flame retardant

[0050] The preparation method of the flame retardant is as follows: according to the mass fraction, 4.6 kg of octaphenyl cage silsesquioxane is added into the reactor and stirred evenly, then 0.025 kg of isopropyl glycidyl ether is added, the temperature is raised to 88 ° C, and after mixing evenly, 0.1 kg of hexamethyldisilazane is added and stirred for 25 minutes to obtain the flame retardant, and the particle size of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm.

[0051] Example 1

[0052] A flame retardant silicone rubber, prepared by raw materials including, by weight: 3.0 kg of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 0.5 kg of silane-modified silica, 4.0 kg of flame retardant, 0.006 kg of platinum complex, 0.05 kg of 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, 0.15 kg of hydroxyl-terminated polydimethylsiloxane, and 0.1 kg of magnesium stearate, wherein the flame retardant is the flame retardant prepared in Preparation Example 1; the silane-modified silica is 3-aminopropyltrimethoxysilane-modified silica, the average particle size D50 of which is 2 μm, the oil absorption value of which is 60 mL / 100 g, and the bulk density of which is 0.6 g / cm 3 The platinum complex is a platinum complex containing tetramethylethylenediamine, wherein the platinum element is 80 ppm by mass.

[0053] The method for preparing the flame retardant silicone rubber comprises the following steps:

[0054] S91. According to the mass fractions, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), silane-modified silica and flame retardant are mixed and added into a kneader for heating and kneading. The kneading temperature is 105° C. and the kneading time is 5 h to obtain a mixture A.

[0055] S92, adding the platinum complex to the mixture A according to the parts by mass, and kneading to obtain a mixture B;

[0056] S93, mixing hydroxyl-terminated polydimethylsiloxane and magnesium stearate according to parts by mass to obtain a mixture C;

[0057] S94. Add mixture C and 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane to mixture B according to their weight parts, and knead to obtain mixture D;

[0058] S95. Place the mixture D in a flat vulcanizer for vulcanization. The vulcanization process is as follows: temperature 155° C., vulcanization time 30 min, to obtain a flame retardant silicone rubber.

[0059] Example 2

[0060] A flame retardant silicone rubber, prepared from raw materials including, by weight: 5.5 kg of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 1.5 kg of silane-modified silica, 5.5 kg of flame retardant, 0.008 kg of platinum complex, 0.1 kg of 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, 0.35 kg of hydroxyl-terminated polydimethylsiloxane, and 0.2 kg of calcium stearate, wherein the flame retardant is the flame retardant prepared in Preparation Example 2; the silane-modified silica is γ-methacryloxypropyltrimethoxysilane-modified silica, the average particle size D50 of which is 0.8 μm, the oil absorption value of which is 80 mL / 100 g, and the bulk density of which is 0.5 g / cm 3 The platinum complex is a platinum complex containing benzotriazole, wherein the platinum element is 100 ppm by mass.

[0061] The method for preparing the flame retardant silicone rubber comprises the following steps:

[0062] S91, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), silane-modified silica and flame retardant are mixed according to their weight parts, added into a kneader, and heated and kneaded at a kneading temperature of 115° C. for a kneading time of 4 h to obtain a mixture A;

[0063] S92, adding the platinum complex to the mixture A according to the parts by mass, and kneading to obtain a mixture B;

[0064] S93, mixing hydroxyl-terminated polydimethylsiloxane and calcium stearate according to parts by mass to obtain a mixture C;

[0065] S94. Add mixture C and 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane to mixture B according to their weight parts, and knead to obtain mixture D;

[0066] S95. Place the mixture D in a flat vulcanizer for vulcanization. The vulcanization process is as follows: temperature 165° C., vulcanization time 20 min, to obtain a flame retardant silicone rubber.

[0067] Example 3

[0068] A flame retardant silicone rubber, prepared from raw materials including, by weight: 4 kg of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 1 kg of silane-modified silica, 5 kg of flame retardant, 0.007 kg of platinum complex, 0.08 kg of 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane, 0.27 kg of hydroxyl-terminated polydimethylsiloxane, and 0.15 kg of zinc stearate, wherein the flame retardant is the flame retardant prepared in Preparation Example 3; the silane-modified silica is γ-mercaptopropyltriethoxysilane-modified silica, the average particle size D50 of which is 1.2 μm, the oil absorption value of which is 71 mL / 100 g, and the bulk density of which is 0.56 g / cm 3 The platinum complex is a platinum complex containing benzotriazole, wherein the platinum element accounts for 90 ppm by mass.

[0069] The method for preparing the flame retardant silicone rubber comprises the following steps:

[0070] S91. According to the mass fractions, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), silane-modified silica and flame retardant were mixed and added into a kneader for heating and kneading. The kneading temperature was 110° C. and the kneading time was 4.2 h to obtain a mixture A.

[0071] S92, adding the platinum complex to the mixture A according to the parts by mass, and kneading to obtain a mixture B;

[0072] S93, mixing hydroxyl-terminated polydimethylsiloxane and zinc stearate according to parts by mass to prepare a mixture C;

[0073] S94. Add mixture C and 2,5-dimethyl-2,5-di-tert-butyl peroxyhexane to mixture B according to their weight parts, and knead to obtain mixture D;

[0074] S95. Place the mixture D in a flat vulcanizer for vulcanization. The vulcanization process is as follows: temperature 160° C., vulcanization time 25 min, to obtain a flame retardant silicone rubber.

[0075] The flame retardant silicone rubber liquid plug is processed into a liquid plug, and its structure is shown in the figure Figure 1 , Figure 2 , Figure 3 shown.

[0076] Comparative Example 1

[0077] The same as Example 3, except that: the flame retardant is the flame retardant prepared in Comparative Example 1.

[0078] Comparative Example 2

[0079] The same as Example 3, except that: the flame retardant is the flame retardant prepared in Comparative Example 2.

[0080] Comparative Example 3

[0081] The same as Example 3, except that: the flame retardant is the flame retardant prepared in Comparative Example 3.

[0082] Comparative Example 4

[0083] The same as Example 3, except that an equal amount of tetramethyl divinyl disiloxane platinum complex (90 ppm by mass of platinum element) is used instead of the platinum gold complex.

[0084] Comparative Example 5

[0085] The same as Example 3, except that an equal amount of silicon dioxide with an average particle size D50 of 1.2 μm is used instead of the silane-modified silicon dioxide.

[0086] Performance testing

[0087] The flame retardant silicone rubbers prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were sampled and processed into test strips for testing. The test results are shown in Table 1.

[0088] Flame retardant test: refer to the test method in ANSI / UL-94-1985, vertical burning test according to 94V-0, 94V-1, 94V-2, the test strip thickness is 1mm;

[0089] The tensile strength and elongation at break were tested according to standard GB / T528-2009, with a tensile rate of 50 mm / min;

[0090] Oxygen index The oxygen index of the test material is determined in accordance with GB / T 2406-1993.

[0091] Table 1 Performance test

[0092] project Tensile strength / MPa Elongation at break / % Flame retardant grade Oxygen index / % Example 1 6.8 423 V-0 34 Example 2 7.7 465 V-0 39 Example 3 7.1 446 V-0 36 Comparative Example 1 6.3 398 V-1 32 Comparative Example 2 6.4 402 V-1 31 Comparative Example 3 6.5 412 V-2 26 Comparative Example 4 6.6 387 V-0 31 Comparative Example 5 5.7 363 V-0 34

[0093] Analyzing the data in Table 1, we can see that:

[0094] 1) The flame retardant silicone rubber prepared in Examples 1 to 3 has a high flame retardant grade and good mechanical properties. This indicates that the flame retardant in the flame retardant silicone rubber prepared in this application has excellent flame retardant properties, good compatibility and good dispersibility in the silicone rubber matrix, and the prepared flame retardant silicone rubber has high flame retardant properties and excellent mechanical properties, which makes it have a wide range of application prospects in various electrical appliances, power waterproofing and fire protection fields.

[0095] 2) A comparative analysis of the properties of the flame retardant silicone rubber prepared in combination with Example 3 and Comparative Examples 1 to 3 shows that the flame retardant prepared in the preparation example, which consists of magnesium hydroxide, aluminum hydroxide, octaphenyl cage silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane in a mass ratio of 11:29:6:0.25:1, can improve the flame retardant properties and mechanical properties of the flame retardant silicone rubber by utilizing the synergistic effect therebetween.

[0096] 3) The performance comparison analysis of the flame retardant silicone rubber prepared in Example 3 and Comparative Example 4 shows that the nitrogen-containing ligand of the platinum complex in this application uses benzotriazole, and the nitrogen-containing ligand can enhance the anti-sintering performance of platinum at high temperatures. Platinum itself has flame retardancy, and nitrogen also has certain flame retardancy, so the combination of nitrogen-containing ligands and platinum ligands can further enhance the flame retardancy of the platinum complex.

[0097] 4) The comparative analysis of the performance of the flame retardant silicone rubber prepared in Example 3 and Comparative Example 5 shows that the use of silane-modified silica in the present application plays a role in improving the compatibility with silicone rubber, and can further enhance the mechanical properties and stability of the flame retardant silicone rubber.

[0098] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.

Claims

1. A flame retardant silicone rubber, characterized in that: The raw materials for preparation include, by weight: 30-55 parts of vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), 5-15 parts of silane-modified silica, 40-55 parts of flame retardant, 0.06-0.08 parts of platinum complex, 0.5-1 parts of vulcanizing agent, 1.5-3.5 parts of hydroxyl-terminated polydimethylsiloxane, and 1-2 parts of stearate; the preparation method of the flame retardant is: according to the weight parts, respectively, magnesium hydroxide, aluminum hydroxide and octaphenyl cage-shaped silsesquioxane are added to the reactor and stirred evenly, then isopropyl glycidyl ether is added, the temperature is raised to 85-90°C, after mixing evenly, hexamethyldisilazane is finally added and stirred for 20-30 minutes to obtain the flame retardant, the magnesium hydroxide, aluminum hydroxide, octaphenyl The mass ratio of cage-shaped silsesquioxane, isopropyl glycidyl ether and hexamethyldisilazane is (10-12):(28-30):(5-7):(0.2-0.3):(0.8-1.2), the particle sizes of the magnesium hydroxide and the aluminum hydroxide are both 1-3 μm; the silane-modified silica is at least one of 3-aminopropyltrimethoxysilane-modified silica, γ-methacryloxypropyltrimethoxysilane-modified silica, and γ-mercaptopropyltriethoxysilane-modified silica; the average particle size D50 of the silane-modified silica is ≤2 μm; the oil absorption value of the silane-modified silica is 60-80 mL / 100 g; the bulk density of the silane-modified silica is 0.5-0.6 g / cm 3 ; The platinum complex is a platinum complex containing a nitrogen ligand, and the nitrogen ligand is one of tetramethylethylenediamine and benzotriazole; The method for preparing the flame retardant silicone rubber comprises the following steps: S91, according to the mass parts, vinyl-terminated dimethyl methyl vinyl (siloxane and polysiloxane), silane-modified silica and flame retardant are mixed and added into a kneader for heating and kneading, the kneading temperature is 105-115° C., the kneading time is 4-5 hours, and a mixture A is obtained; S92, adding the platinum complex to the mixture A according to the parts by mass, and kneading to obtain a mixture B; S93, mixing hydroxyl-terminated polydimethylsiloxane and stearate according to parts by mass to prepare a mixture C; S94, adding mixture C and a vulcanizing agent to mixture B according to parts by mass, and kneading to obtain mixture D; S95. Place the mixture D in a flat vulcanizer for vulcanization. The vulcanization process is as follows: temperature 155-165° C., vulcanization time 20-30 min, to obtain a flame retardant silicone rubber.

2. The flame retardant silicone rubber according to claim 1, characterized in that: The mass fraction of platinum element in the platinum-gold complex is 80-100 ppm.

3. The flame retardant silicone rubber according to claim 1, characterized in that: The vulcanizing agent is 2,5-dimethyl-2,5-di-tert-butyl peroxide hexane.

4. The flame retardant silicone rubber according to claim 1, characterized in that: The stearate is at least one of zinc stearate, magnesium stearate and calcium stearate.

5. A liquid plug, characterized in that: The liquid plug is made of the flame retardant silicone rubber according to any one of claims 1 to 4, and the flame retardant grade of the liquid plug is V-0 according to ANSI / UL-94-1985 standard; the tensile strength of the liquid plug is 6.8-7.7 MPa, and the oxygen index of the liquid plug is 34-39%.