A preparation method of high-strength adhesive for PVC pipes
By using multiple cross-linked polyurethane cross-linking agents of sulfonate and silicone in PVC pipe adhesives, combined with maleic anhydride-modified chlorinated polyvinyl chloride resin, the problem of insufficient bonding performance and strength of PVC pipes is solved. The preparation of high-strength, environmentally friendly and non-toxic adhesive is achieved, and is suitable for various pipeline leakage problems.
Patent Information
- Application Number
- CN202410358286.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Existing adhesives for PVC pipes have poor bonding performance and strength, and traditional adhesives often contain toxic and volatile substances, which affect the environment and human health.
A multi-crosslinked polyurethane cross-linking agent containing sulfonate and organic silicon is used to enhance the electrostatic force between molecules and organic silicon to improve corrosion resistance. It is combined with maleic anhydride modified chlorinated polyvinyl chloride resin and Multiple cross-linked polyurethane emulsion forms a high-strength adhesive to enhance the bonding performance and corrosion resistance of PVC pipes.
It realizes the preparation of high-strength adhesive for PVC pipes, solves the problem of insufficient bonding performance and strength, and ensures environmentally friendly and non-toxic characteristics. It is widely applicable to the leakage problem of PVC pipes and other pipes.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a method for preparing a high-strength adhesive for PVC pipes. Background Art
[0002] Polyvinyl chloride (PVC) is widely available and easy to process. Its products have excellent corrosion resistance and certain mechanical strength. In addition to its application in daily products, it has also been widely used in chemical anti-corrosion. For example, PVC pipes are a new type of building material and are increasingly widely used in building drainage and sewage treatment. However, most of them are currently formed by welding, which will greatly reduce the strength of PVC products, and the pressure-bearing capacity of PVC pipes themselves is relatively low. During the installation process, improper construction methods and poor coordination between pipes and fittings often cause leakage or seepage in the completed PVC pipelines, which cannot meet the acceptance requirements. There are usually two solutions: one is to remove the leaking part of the pipeline and reinstall it; the other is to use adhesives for anti-leakage treatment. The former is time-consuming and labor-intensive and has a large economic loss, while the latter is easy to construct. Therefore, suitable adhesives can be used to enhance the weld area or the entire exterior of the product.
[0003] Among synthetic adhesives, when acrylic adhesives are used to bond PVC materials, the organic volatile content of acrylic adhesives is low and the bonding is strong. However, when used to bond PVC pipes, the initial adhesion is low and the bonding strength is poor due to the smooth surface of PVC pipes. Modified perchlorethylene adhesives have a structure similar to polyvinyl chloride and are a good PVC bonding material. However, the solvents used in this adhesive, such as cyclohexanone, benzene, toluene, chlorinated hydrocarbons, etc., are all toxic volatile substances that will cause harm to workers and the surrounding environment. The price of polyvinyl acetate adhesives It is cheap and easy to produce, uses water as the dispersion medium, is safe and non-toxic, and does not pollute the environment. However, when used for bonding PVC pipes, the bonding strength is poor due to its relatively smooth surface. The urethane polar bonds, ester bonds, ether bonds, urea bonds, etc. in the polyurethane adhesives in the prior art have good bonding properties to a variety of materials, and have the characteristics of good wettability, high initial bonding strength, non-toxicity, and no pollution. However, PVC pipes have a wide range of application scenarios and will lose their bonding properties under various harsh conditions. Therefore, they need to be modified to meet more application fields of PVC pipes.
[0004] The present invention synthesizes a polyurethane crosslinking agent containing sulfonate and organosilicon. The sulfonate can increase the electrostatic force between molecules and adsorb the relatively polar molecules of the polyurethane molecular chain on the bonding interface. The organosilicon has good corrosion resistance. The addition of multiple crosslinking agents makes the structure denser and the penetration of small molecules is difficult, thereby improving the corrosion resistance and mechanical strength of the adhesive. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a high-strength adhesive for PVC pipes, which solves the problems of poor bonding performance and strength of the existing adhesive for PVC pipes and is environmentally friendly and non-toxic.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A method for preparing a high-strength adhesive for PVC pipes. The adhesive comprises the following components in parts by weight: 100 parts of perchlorethylene resin, 5-25 parts of maleic anhydride modified chlorinated polyvinyl chloride resin, 2-10 parts of multi-crosslinked polyurethane emulsion, 15-25 parts of alkyd resin, 15-30 parts of plasticizer dibutyl phthalate, 200-300 parts of mixed solvent, and 600-700 parts of light calcium carbonate.
[0008] The preparation method is as follows: add weighed perchlorethylene resin, maleic anhydride modified chlorinated polyvinyl chloride resin and mixed solvent into a dissolving tank, stir to make the resin fully swell and dissolve, then add multi-crosslinked polyurethane emulsion, alkyd resin, plasticizer dibutyl phthalate, stir evenly, add light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0009] Furthermore, the mixed solvent is prepared by uniformly mixing butyl acetate and acetone in a ratio of 1 g: (1.2-1.5) g.
[0010] Further, the preparation method of the multi-crosslinked polyurethane emulsion is:
[0011] (1) Add 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and N,N-dimethylformamide to a reaction flask, stir evenly, then add potassium carbonate and sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, stir to react, and after the reaction is completed, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate. The preparation reaction formula is as follows:
[0012]
[0013] (2) Add sodium bis(allyloxytetramethyldisiloxane sulfonate) and ethanol to the reaction flask, stir evenly, then add tris(hydroxymethylaminomethane) and a catalyst, stir to react, and after the reaction is completed, concentrate and separate by column chromatography to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker. The preparation reaction formula is as follows:
[0014]
[0015] (3) Add polyester diol to a reaction bottle equipped with a condenser, perform vacuum dehydration at 100-110°C for 1-2 hours, add isophorone diisocyanate, sodium polyhydroxysulfonate-based silicone crosslinker and dibutyltin dilaurate, react at 70-80°C for 2-5 hours, cool to 40-50°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 10-20 minutes, and perform vacuum distillation to obtain a multi-crosslinked polyurethane emulsion.
[0016] Furthermore, in step (1), the ratio of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, potassium carbonate, and sodium 3-allyloxy-2-hydroxy-1-propanesulfonate is 1 mol: (2.2-2.5) mol: (2-2.1) mol.
[0017] Furthermore, in step (1), the reaction temperature is 80-100° C. and the reaction time is 5-10 h.
[0018] Furthermore, in step (2), the catalyst is any one of benzyltriethylammonium chloride, benzyltrimethylammonium chloride and tetrabutylammonium bromide.
[0019] Furthermore, in step (2), the ratio of sodium bis(allyloxytetramethyldisiloxane sulfonate), tris(hydroxymethylaminomethane) and the catalyst is 1 mol: (2.05-2.2) mol: (0.001-0.003) mol.
[0020] Furthermore, in step (2), the reaction temperature is 60-75° C. and the reaction time is 8-16 h.
[0021] Furthermore, in step (3), the ratio of polyester diol, isophorone diisocyanate, sodium polyhydroxysulfonate-based silicone crosslinking agent, and dibutyltin dilaurate is (0.4-0.5) mol: 1 mol: (0.1-0.3) mol: (0.0015-0.0025) mol.
[0022] By adopting the above technical solution, the beneficial effects of the present invention are:
[0023] The invention firstly reacts 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 3-allyloxy-2-hydroxy-1-propanesulfonate sodium under the action of potassium carbonate to obtain bisallyloxytetramethyldisiloxane sodium sulfonate, then uses the alkenyl group of the sulfonate to react with the amino group of trishydroxymethylaminomethane to obtain a polyhydroxysulfonate sodium-based organosilicon crosslinking agent, then polymerizes with polyester polyol and isophorone diisocyanate to obtain a multi-crosslinked polyurethane emulsion, and finally evenly mixes with perchlorethylene resin, maleic anhydride-modified chlorinated polyvinyl chloride resin and the like to obtain a high-strength adhesive for PVC pipes.
[0024] Maleic anhydride modified chlorinated polyvinyl chloride resin is the product of the reaction of chlorinated polyvinyl chloride resin with maleic anhydride. Its structural formula is very similar to polyvinyl chloride. Polyurethane and maleic anhydride modified chlorinated polyvinyl chloride resin have good compatibility. According to the principle of "like dissolves like", good compatibility enhances the adsorption between molecules, which is beneficial to the mutual diffusion and penetration of polyurethane on the bonding interface, making the interface between polyurethane and PVC material disappear. At the same time, it can form a cross-linked network structure with multi-cross-linked polyurethane emulsion, making the molecular chain blocked and difficult to move, thereby generating more ordered urea groups, carbamates and hydrogen bonds, so that a stronger force is formed between the polyurethane adhesive and the PVC substrate, and the wettability on PVC is gradually improved, forming a more solid bond with the PVC material.
[0025] The more densely and evenly the sodium sulfonate hydrophilic groups in the multi-cross-linked polyurethane emulsion are distributed on the latex surface, the more the Coulomb force and intermolecular force between the particles increase. Under the action of high-speed shear force, it is easier to form uniform particles. The smaller the particle size, the smaller the gap between the particles, and the more difficult the particle movement, which increases the viscosity of the emulsion and improves the overall performance. The polar groups such as urea and carbamate in the polyurethane structure can form hydrogen bonds with the sodium sulfonate groups. At the same time, the increase in the degree of cross-linking between polyurethane and PVC makes the film structure denser, the penetration of small molecules is difficult, the destructive power of the acid environment on the urethane bond is weakened, and the silicone has good corrosion resistance, which improves the mechanical properties and acid resistance of the adhesive.
[0026] The adhesive prepared by the present invention is not only widely used in PVC pipes, but can also quickly block leakage on PVC pipes and can also block leakage at the junction of PVC pipes and cement floors. It can also solve the water leakage and sealing problems of other pipes at present. Since the added filler is a polar material, the adhesive is also suitable for solving the water leakage problem of the sewer pipe system in the kitchen and bathroom, and has a wide range of applications. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Preparation of maleic anhydride modified chlorinated polyvinyl chloride resin: add 20g chlorinated polyvinyl chloride resin and 50mL acetone into a reaction flask, swell at 25°C for 1h, add 20g maleic anhydride and 1g ammonium persulfate, react at 80°C for 2h, filter, and dry to obtain maleic anhydride modified chlorinated polyvinyl chloride resin.
[0029] 1,3-Bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, CAS number is 2362-10-9.
[0030] Sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, CAS number is 52556-42-0.
[0031] Tris(hydroxymethyl)aminomethane, CAS number is 77-86-1.
[0032] Example 1
[0033] (1) Add 25 mmol of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 100 mL of N,N-dimethylformamide to a reaction flask, stir evenly, then add 57.5 mmol of potassium carbonate and 51.5 mmol of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, react at 90°C for 8 h, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate.
[0034] (2) Add 18 mmol sodium bis(allyloxytetramethyldisiloxane)sulfonate and 180 mL ethanol to a reaction flask, stir evenly, then add 38.7 mmol tris(hydroxymethyl)aminomethane and 0.036 mmol benzyltriethylammonium chloride, react at 65° C. for 12 h, concentrate, and separate by column chromatography using a mobile system with a volume ratio of methanol to dichloromethane of 1:10 to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker.
[0035] (3) Add 4.5 mmol of polyester diol into a reaction bottle equipped with a condenser, vacuum dehydrate at 105°C for 2 h, add 10 mmol of isophorone diisocyanate, 1 mmol of sodium polyhydroxysulfonate-based silicone crosslinker and 0.02 mmol of dibutyltin dilaurate, react at 75°C for 4 h, cool to 45°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 15 min, and distill under reduced pressure to obtain a multi-crosslinked polyurethane emulsion.
[0036] Example 2
[0037] (1) Add 40 mmol of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 120 mL of N,N-dimethylformamide into a reaction flask, stir evenly, then add 88 mmol of potassium carbonate and 80 mmol of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, react at 100°C for 5 h, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate.
[0038] (2) Add 32 mmol sodium bis(allyloxytetramethyldisiloxane)sulfonate and 256 mL ethanol to a reaction flask, stir evenly, then add 65.6 mmol tris(hydroxymethyl)aminomethane and 0.032 mmol benzyltrimethylammonium chloride, react at 75° C. for 8 h, concentrate, and separate by column chromatography using a mobile system with a volume ratio of methanol to dichloromethane of 1:10 to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker.
[0039] (3) Add 4 mmol of polyester diol into a reaction bottle equipped with a condenser, vacuum dehydrate at 110°C for 1 h, add 10 mmol of isophorone diisocyanate, 1.5 mmol of sodium polyhydroxysulfonate-based silicone crosslinker and 0.015 mmol of dibutyltin dilaurate, react at 80°C for 2 h, cool to 50°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 10 min, and distill under reduced pressure to obtain a multi-crosslinked polyurethane emulsion.
[0040] Example 3
[0041] (1) Add 15 mmol of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 75 mL of N,N-dimethylformamide to a reaction flask, stir evenly, then add 37.5 mmol of potassium carbonate and 31.5 mmol of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, react at 80°C for 10 h, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate.
[0042] (2) Add 13 mmol sodium bis(allyloxytetramethyldisiloxane)sulfonate and 156 mL ethanol to a reaction flask, stir evenly, then add 28.6 mmol tris(hydroxymethyl)aminomethane and 0.039 mmol tetrabutylammonium bromide, react at 60° C. for 16 h, concentrate, and separate by column chromatography using a mobile system with a volume ratio of methanol to dichloromethane of 1:10 to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker.
[0043] (3) Add 5 mmol of polyester diol into a reaction bottle equipped with a condenser, vacuum dehydrate at 100°C for 2 h, add 10 mmol of isophorone diisocyanate, 2 mmol of sodium polyhydroxysulfonate-based silicone crosslinker and 0.025 mmol of dibutyltin dilaurate, react at 70°C for 5 h, cool to 50°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 20 min, and distill under reduced pressure to obtain a multi-crosslinked polyurethane emulsion.
[0044] Example 4
[0045] (1) Add 24 mmol of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 108 mL of N,N-dimethylformamide to a reaction flask, stir evenly, then add 56.4 mmol of potassium carbonate and 49.2 mmol of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, react at 95°C for 9 h, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate.
[0046] (2) Add 16 mmol sodium bis(allyloxytetramethyldisiloxane)sulfonate and 176 mL ethanol to a reaction flask, stir evenly, then add 34.4 mmol tris(hydroxymethyl)aminomethane and 0.04 mmol benzyltriethylammonium chloride, react at 70° C. for 15 h, concentrate, and separate by column chromatography using a mobile system with a volume ratio of methanol to dichloromethane of 1:10 to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker.
[0047] (3) Add 5 mmol of polyester diol into a reaction bottle equipped with a condenser, vacuum dehydrate at 105°C for 2 h, add 10 mmol of isophorone diisocyanate, 2.5 mmol of sodium polyhydroxysulfonate-based silicone crosslinker and 0.02 mmol of dibutyltin dilaurate, react at 80°C for 4 h, cool to 45°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 15 min, and distill under reduced pressure to obtain a multi-crosslinked polyurethane emulsion.
[0048] Example 5
[0049] (1) Add 10 mmol of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and 35 mL of N,N-dimethylformamide to a reaction flask, stir evenly, then add 24 mmol of potassium carbonate and 21 mmol of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, react at 85°C for 8 h, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate.
[0050] (2) Add 8 mmol sodium bis(allyloxytetramethyldisiloxane)sulfonate and 72 mL ethanol to a reaction flask, stir evenly, then add 17.2 mmol tris(hydroxymethyl)aminomethane and 0.024 mmol benzyltrimethylammonium chloride, react at 70° C. for 16 h, concentrate, and separate by column chromatography using a mobile system with a volume ratio of methanol to dichloromethane of 1:10 to obtain a polyhydroxy sodium sulfonate-based organosilicon crosslinker.
[0051] (3) Add 4.5 mmol of polyester diol into a reaction bottle equipped with a condenser, vacuum dehydrate at 110°C for 2 h, add 10 mmol of isophorone diisocyanate, 3 mmol of sodium polyhydroxysulfonate-based silicone crosslinker and 0.02 mmol of dibutyltin dilaurate, react at 80°C for 4 h, cool to 40°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 20 min, and distill under reduced pressure to obtain a multi-crosslinked polyurethane emulsion.
[0052] Average particle size test: The prepared multi-cross-linked polyurethane emulsion was diluted 500 times with deionized water, and when the system became transparent, the average particle size of the emulsion was tested with a laser particle size analyzer at 25°C.
[0053] Emulsion viscosity test: The prepared multi-cross-linked polyurethane emulsion was diluted 500 times with deionized water, and the viscosity of the emulsion was tested at 25°C using a rotational viscometer. The rotation speed was set to 750 r / min, and the average value was obtained by measuring three times.
[0054]
[0055] It can be seen from the test results in the above table that with the increase of the content of polyhydroxy sodium sulfonate-based silicone crosslinking agent, the particle size of the multi-crosslinked polyurethane emulsion gradually decreases and the viscosity gradually increases. After 500 times of dilution with deionized water, the particle size of the polyurethane emulsion in Example 5 is 32.6nm and the viscosity is 245.6mPa·s. This is because the polyhydroxy sodium sulfonate-based silicone crosslinking agent contains sodium sulfonate hydrophilic monomers. With the increase of the sulfonic acid group content, the hydrophilicity of the emulsion particles is stronger, the volume of the hydrated particles is larger, and the polyurethane emulsion is more stable. At the same time, the more dense and uniform the distribution of the sodium sulfonate hydrophilic groups on the latex surface is, the Coulomb force and intermolecular force between the particles are continuous. Under the action of high-speed shear force, it is easier to form uniform particles. The smaller the particle size, the smaller the gap between the particles, and the more difficult the particle movement is, the greater the viscosity of the emulsion is, and the comprehensive performance is excellent.
[0056] Example 6
[0057] Add 100g of perchlorethylene resin, 5g of maleic anhydride-modified chlorinated polyvinyl chloride resin, 80g of butyl acetate and 120g of acetone into a dissolving tank, stir to fully swell and dissolve the resin, then add 2g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 20g of alkyd resin, and 25g of plasticizer dibutyl phthalate, stir evenly, add 650g of light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0058] Example 7
[0059] Add 100g of perchlorethylene resin, 10g of maleic anhydride-modified chlorinated polyvinyl chloride resin, 120g of butyl acetate and 180g of acetone into the dissolution tank, stir to fully swell and dissolve the resin, then add 4g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 15g of alkyd resin, and 30g of plasticizer dibutyl phthalate, stir evenly, add 700g of light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0060] Example 8
[0061] Add 100g of perchlorethylene resin, 15g of maleic anhydride-modified chlorinated polyvinyl chloride resin, 100g of butyl acetate and 130g of acetone into the dissolution tank, stir to fully swell and dissolve the resin, then add 6g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 25g of alkyd resin, and 15g of plasticizer dibutyl phthalate, stir evenly, add 600g of light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0062] Example 9
[0063] Add 100g of perchlorethylene resin, 20g of maleic anhydride-modified chlorinated polyvinyl chloride resin, 90g of butyl acetate and 135g of acetone into a dissolving tank, stir to fully swell and dissolve the resin, then add 8g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 25g of alkyd resin, and 25g of plasticizer dibutyl phthalate, stir evenly, add 660g of light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0064] Example 10
[0065] Add 100g of perchlorethylene resin, 25g of maleic anhydride-modified chlorinated polyvinyl chloride resin, 110g of butyl acetate and 132g of acetone into a dissolving tank, stir to fully swell and dissolve the resin, then add 10g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 15g of alkyd resin, and 20g of plasticizer dibutyl phthalate, stir evenly, add 650g of light calcium carbonate, stir until fine and uniform, and obtain a high-strength adhesive for PVC pipes.
[0066] Comparative Example 1
[0067] Add 100 g of perchlorethylene resin, 80 g of butyl acetate and 120 g of acetone into the dissolution tank, stir to make the resin fully swell and dissolve, then add 2 g of multi-crosslinked polyurethane emulsion (prepared in Example 5), 20 g of alkyd resin, and 25 g of plasticizer dibutyl phthalate, stir evenly, add 650 g of light calcium carbonate, stir until fine and uniform, and obtain an adhesive.
[0068] Comparative Example 2
[0069] Add 100g of perchlorethylene resin, 5g of maleic anhydride modified chlorinated polyvinyl chloride resin, 80g of butyl acetate and 120g of acetone into the dissolution tank, stir to make the resin fully swell and dissolve, then add 20g of alkyd resin and 25g of plasticizer dibutyl phthalate, stir evenly, then add 650g of light calcium carbonate, stir until fine and uniform, to obtain an adhesive.
[0070] Comparative Example 3
[0071] Add 100g of perchlorethylene resin, 80g of butyl acetate and 120g of acetone into the dissolution tank, stir to make the resin fully swell and dissolve, then add 20g of alkyd resin and 25g of plasticizer dibutyl phthalate, stir evenly, add 650g of light calcium carbonate, stir until fine and uniform, and obtain the adhesive.
[0072] Initial adhesion and glass strength test: An electronic tensile tester was used to evenly apply the prepared adhesive on the surface of two pieces of PVC (130mm×30mm) with a brush. After activation at 70°C for 5 minutes, the two pieces of PVC were bonded under a pressure of 1.5MPa. The initial adhesion was measured after 5 minutes of bonding, and the final peel strength was measured after 24 hours.
[0073]
[0074] Generally speaking, the peel strength of the material with good bonding performance is higher; it can be seen from the test results in the above table that with the increase of the content of maleic anhydride modified chlorinated polyvinyl chloride resin and multi-crosslinked polyurethane emulsion, the peel strength of the adhesive to the PVC substrate is gradually enhanced, the initial adhesion of Example 10 is 4.42N / mm, the final peel strength is 12.76N / mm, and the bonding performance is good; this is because on the one hand, the increase in the content of sodium sulfonate hydrophilic groups in the polyurethane emulsion introduces more charges into the molecules, the Coulomb attraction between ions increases, the bonding force is enhanced, and at the same time, the increase in the molecular polarity of polar groups such as urea bonds, urethane bonds, and ionic bonds in the polyurethane structure can improve the bonding strength; on the other hand, maleic anhydride modified chlorinated polyvinyl chloride resin has good compatibility with PVC and polyurethane, and can form a cross-linked network structure with the multi-crosslinked polyurethane emulsion, so that the molecular chain is blocked and difficult to move, thereby generating more ordered urea groups, urethanes and hydrogen bonds, so that a stronger force is formed between the polyurethane adhesive and the PVC substrate, and the wettability on the PVC is gradually improved.
[0075] Comparative Example 1 does not contain maleic anhydride-modified chlorinated polyvinyl chloride resin, resulting in poor compatibility between the polyurethane and the PVC matrix in the adhesive and low peel strength; Comparative Example 2 does not contain a multi-crosslinked polyurethane emulsion, and a cross-linked network structure is not formed, and its final peel strength is only 4.21 N / mm; Comparative Example 3 does not add maleic anhydride-modified chlorinated polyvinyl chloride resin and multi-crosslinked polyurethane emulsion, and its bonding performance is the worst.
[0076] Preparation of adhesive film: Weigh a certain amount of adhesive and pour it onto a polytetrafluoroethylene plate, allowing it to spread naturally into a film. Leave it at room temperature for 12 hours, and then place it in a vacuum drying oven at 65°C for 24 hours.
[0077] Tensile strength test: The film was tested at 25°C using an electronic universal material testing machine with a tensile rate of 200 mm / min.
[0078] Acid resistance test: After the film is immersed in a 5% H2SO4 solution at 25°C for 7 days, it is taken out and the tensile properties are tested.
[0079]
[0080] From the test results in the above table, it can be seen that with the increase of the content of maleic anhydride modified chlorinated polyvinyl chloride resin and multi-crosslinked polyurethane emulsion, the tensile strength of the film is significantly improved. This is because the polar groups such as urea and carbamate in the polyurethane structure can form hydrogen bonds with the sodium sulfonate group. At the same time, the increase in the degree of crosslinking between polyurethane and PVC makes the film structure denser, the penetration of small molecules is difficult, the destructive power of the acid environment on the urethane bond is weakened, and the silicone has good corrosion resistance, which improves the mechanical properties and acid resistance of the adhesive.
[0081] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a high-strength adhesive for PVC pipes, characterized in that: The adhesive comprises the following components in parts by weight: 100 parts of perchlorethylene resin, 5-25 parts of maleic anhydride modified chlorinated polyvinyl chloride resin, 2-10 parts of multi-crosslinked polyurethane emulsion, 15-25 parts of alkyd resin, 15-30 parts of plasticizer dibutyl phthalate, 200-300 parts of mixed solvent, and 600-700 parts of light calcium carbonate; The preparation method comprises: adding weighed perchlorethylene resin, maleic anhydride modified chlorinated polyvinyl chloride resin and mixed solvent into a dissolving tank, stirring to fully swell and dissolve the resin, then adding multi-crosslinked polyurethane emulsion, alkyd resin and plasticizer dibutyl phthalate, stirring evenly, adding light calcium carbonate, stirring until fine and even, and obtaining a high-strength adhesive for PVC pipes; The preparation method of the multi-crosslinked polyurethane emulsion is: (1) Add 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane and N,N-dimethylformamide to a reaction flask, stir evenly, then add potassium carbonate and sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, stir to react, and after the reaction is completed, cool to room temperature, filter, concentrate the filtrate, and dry to obtain sodium bis(allyloxytetramethyldisiloxanesulfonate; (2) adding sodium bis(allyloxytetramethyldisiloxane)sulfonate and ethanol to a reaction flask, stirring evenly, adding tris(hydroxymethyl)aminomethane and a catalyst, stirring to react, and after the reaction is completed, concentrating, separating by column chromatography, and obtaining a polyhydroxy sodium sulfonate-based organosilicon crosslinking agent; (3) Add polyester diol to a reaction bottle equipped with a condenser, perform vacuum dehydration at 100-110°C for 1-2 hours, add isophorone diisocyanate, sodium polyhydroxysulfonate-based silicone crosslinker and dibutyltin dilaurate, react at 70-80°C for 2-5 hours, cool to 40-50°C, add triethylamine for neutralization, disperse in distilled water at high speed shear for 10-20 minutes, and perform vacuum distillation to obtain a multi-crosslinked polyurethane emulsion.
2. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: The mixed solvent is prepared by uniformly mixing butyl acetate and acetone in a ratio of 1 g: (1.2-1.5) g.
3. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: In the step (1), the ratio of 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisiloxane, potassium carbonate and sodium 3-allyloxy-2-hydroxy-1-propanesulfonate is 1 mol: (2.2-2.5) mol: (2-2.1) mol.
4. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: In the step (1), the reaction temperature is 80-100° C. and the reaction time is 5-10 h.
5. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: The catalyst in step (2) is any one of benzyltriethylammonium chloride, benzyltrimethylammonium chloride and tetrabutylammonium bromide.
6. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: In the step (2), the ratio of sodium bis(allyloxytetramethyldisiloxanesulfonate), tris(hydroxymethylaminomethane) and the catalyst is 1 mol: (2.05-2.2) mol: (0.001-0.003) mol.
7. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: In the step (2), the reaction temperature is 60-75° C. and the reaction time is 8-16 h.
8. The method for preparing a high-strength adhesive for PVC pipes according to claim 1, characterized in that: In the step (3), the ratio of polyester diol, isophorone diisocyanate, sodium polyhydroxysulfonate-based silicone crosslinking agent, and dibutyltin dilaurate is (0.4-0.5) mol: 1 mol: (0.1-0.3) mol: (0.0015-0.0025) mol.