1100MPa grade high-strength steel plate resistant to acidic media corrosion and its production method

By adding elements such as Cu, Cr, and Al to high-strength steel and employing a specific heat treatment process to form a martensitic structure, the problem of failure of high-strength wear-resistant steel under acidic media is solved, achieving comprehensive performance of high strength, wear resistance, and corrosion resistance.

CN118326252BActive Publication Date: 2026-11-17BAOSHAN IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310039787.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-12
Publication Date
2026-11-17
Estimated Expiration
2043-01-12

AI Technical Summary

Technical Problem

Existing high-strength wear-resistant steels fail rapidly under acidic corrosive media and cannot simultaneously meet the performance requirements of wear resistance and acid corrosion resistance.

Method used

By designing a reasonable composition and adding elements such as Cu, Cr, and Al, combined with a specific heat treatment process, a martensitic structure is formed, which improves the acid corrosion resistance of the steel plate while maintaining high strength and hardness.

Benefits of technology

This achieves high strength, wear resistance, and corrosion resistance of steel plates in acidic media, extending equipment service life and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004050548810000101
    Figure BDA0004050548810000101
  • Figure BDA0004050548810000111
    Figure BDA0004050548810000111
  • Figure BDA0004050548810000112
    Figure BDA0004050548810000112
Patent Text Reader

Abstract

This invention discloses a 1100MPa-grade high-strength steel plate resistant to acidic media corrosion, containing Fe and unavoidable impurity elements, and further containing the following chemical elements in the following mass percentages: C: 0.12-0.18%, Si: 0.1-0.3%, Mn: 0.5-0.9%, Cu: 0.15-0.35%, Al: 0.015-0.15%, Cr: 0.5-1.0%, Sb: 0.04-0.12%, B: 0.001-0.003%; and one or two of Nb: 0.01-0.03% and Ti: 0.01-0.03%. Accordingly, this invention also discloses a method for manufacturing this 1100MPa-grade high-strength steel plate resistant to acidic media corrosion. The steel plate obtained using the technical solution of this invention possesses high strength, high hardness, and excellent resistance to acidic media corrosion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a steel plate and its manufacturing method, and more particularly to a high-strength steel plate and its manufacturing method. Background Technology

[0002] High-strength wear-resistant steel plates have a variety of applications. Currently, high-strength wear-resistant steel has been gradually upgraded from 345MPa ordinary carbon steel to 700MPa and 960MPa grades to improve wear resistance.

[0003] However, in some applications, high-strength wear-resistant steel still faces significant corrosion. For example, in acidic corrosive media, the material fails rapidly, and even areas without wear develop noticeable pitting, severely shortening the service life of the equipment.

[0004] Extensive research has been conducted in this field on improving the wear resistance of steel materials. However, there is little research on how to simultaneously address the issues of wear resistance and acid corrosion resistance.

[0005] For example, Chinese patent document CN103146997A, published on June 12, 2013, entitled "A Low-Alloy High-Toughness Wear-Resistant Steel Plate and Its Manufacturing Method," achieves a hardness of 400-460 HBW and exhibits good wear resistance. However, this steel plate cannot meet the wear resistance requirements under acidic media.

[0006] For example, Chinese patent document CN108930001A, published on December 4, 2018, entitled "A High Hardness Wear-Resistant Steel Plate for Slurry Dredging and Its Production Method", discloses a wear-resistant steel plate that takes into account the corrosion problem in the seawater environment, but does not involve corrosion in acidic media.

[0007] For example, Chinese patent document with publication number CN102268613A and publication date of December 7, 2011, entitled "A Hot-rolled Steel Plate for Railway Freight Vehicles Resistant to Atmospheric Corrosion and Its Manufacturing Method", although it takes into account the corrosion of acidic media, its yield strength is only at the level of 450MPa, which cannot meet the functional requirements of wear resistance.

[0008] As can be seen, there is currently a lack of a steel grade that can achieve both high strength and wear resistance, as well as resistance to corrosion from acidic media. Summary of the Invention

[0009] One of the objectives of this invention is to provide a 1100MPa grade high-strength steel plate resistant to acidic media corrosion. Through reasonable composition design and reasonable process design, it not only has wear resistance but also acidic media corrosion resistance, thus making it widely applicable to mining material transportation, domestic waste treatment equipment, and various chemical fields with acidic media corrosion characteristics.

[0010] To achieve the above objectives, the present invention provides a 1100MPa grade high-strength steel plate resistant to acidic media corrosion, which contains Fe and unavoidable impurity elements, and also contains the following chemical elements in the following mass percentages:

[0011] C: 0.12-0.18%, Si: 0.1-0.3%, Mn: 0.5-0.9%, Cu: 0.15-0.35%, Al: 0.015-0.15%, Cr: 0.5-1.0%, Sb: 0.04-0.12%, B: 0.001-0.003%; and one or both of Nb: 0.01-0.03% and Ti: 0.01-0.03%.

[0012] Accordingly, the present invention also provides a high-strength steel plate resistant to acidic media corrosion at a pressure of 1100 MPa, wherein the mass percentage content of each chemical element is as follows:

[0013] C: 0.12-0.18%, Si: 0.1-0.3%, Mn: 0.5-0.9%, Cu: 0.15-0.35%, Al: 0.015-0.15%, Cr: 0.5-1.0%, Sb: 0.04-0.12%, B: 0.001-0.003%; and one or both of Nb: 0.01-0.03% and Ti: 0.01-0.03%; the balance being Fe and unavoidable impurity elements.

[0014] The design principles of each chemical element in the 1100MPa grade acid-resistant high-strength steel plate described in this invention are as follows:

[0015] Carbon (C) is the cheapest strengthening element in steel and can significantly improve the strength of steel plates. However, excessive C is detrimental to the weldability, toughness, and plasticity of steel plates. Therefore, this invention limits its content to 0.12-0.18%.

[0016] Si is a deoxidizing element, a solid solution strengthening element, and a commonly used corrosion-resistant element in atmospheric corrosion-resistant steels. In steel, Si replaces Fe atoms through substitution, hindering dislocation movement and thus achieving solid solution strengthening. Simultaneously, Si can reduce the diffusion coefficient of C in ferrite, increase carbon activity, inhibit carbide formation, and suppress the precipitation of coarse carbides at defects, thereby improving toughness. However, excessive Si promotes graphitization of C, which is detrimental to toughness, surface quality, and weldability. Therefore, this invention limits its content to 0.1-0.3%.

[0017] Mn enhances yield strength through solid solution strengthening, reduces elongation, significantly lowers the phase transformation temperature of steel, and refines the microstructure, making it an important strengthening and toughening element. However, excessive Mn content increases hardenability, leading to deterioration in weldability and weld heat-affected zone toughness, and increasing costs. Therefore, this invention controls its content to 0.5-0.9%.

[0018] Cu has solid solution and precipitation strengthening effects. At higher content, it exhibits a secondary hardening effect during tempering at appropriate temperatures, thereby increasing strength. Simultaneously, Cu is also an element that improves corrosion resistance. Its electrochemical potential is higher than that of Fe. Adding an appropriate amount of Cu not only helps increase the self-corrosion potential of the steel plate, reducing the corrosion rate, but also promotes the densification and stabilization of the rust layer on the steel surface, thus improving corrosion resistance. Especially in acidic media, Cu combines with residual S in the steel to form a Cu₂S protective film, mitigating corrosion in acidic environments. Therefore, in this invention, to ensure the effect of Cu, its content is not less than 0.15%. Excessive Cu content causes cracks in the steel billet during heating and hot rolling, deteriorating surface properties; therefore, the upper limit is limited to 0.35%.

[0019] Al is typically added to steel as a deoxidizer during the steelmaking process. Trace amounts of Al also help refine grains and improve the strength and toughness of the steel. Adding appropriate amounts of Al increases the corrosion potential of the steel, which helps inhibit corrosion. In this invention, the formation and aggregation of complex nanoscale oxides containing Al and Si in the inner rust layer can increase the charge-mass transfer resistance, thereby inhibiting the corrosion process. In particular, appropriate amounts of Al combined with Cr can improve corrosion resistance in acidic media. However, Al reduces austenite stability and austenite undercooling, causing rapid growth of new phase nuclei, thus reducing hardenability and increasing the critical quenching rate. Simultaneously, as a ferrite-forming element, excessive Al reduces the strength of the steel plate and increases the brittleness of ferrite, leading to a decrease in steel toughness. Therefore, this invention limits its content to 0.015-0.15%.

[0020] In steel, Cr forms a continuous solid solution with Fe, resulting in solid solution strengthening. It also forms various types of carbides with C, such as M3C, M7C3, and M... 23C6 and other compounds produce a secondary strengthening effect; simultaneously, Cr shrinks the austenite region, reduces the diffusion rate of C in austenite, lowers the critical cooling rate, and improves the hardenability and tempering stability of the steel plate. Therefore, wear-resistant steels typically have a certain amount of Cr added to achieve high strength and hardenability. Furthermore, in this invention, the addition of Cr primarily improves corrosion resistance in acidic media. Cr has a significant effect on improving the passivation ability of steel, promoting the formation of a dense passivation film or protective rust layer on the steel surface, and forming FeCr2O4 with good anti-corrosion function within the rust layer. Its enrichment within the rust layer effectively improves the selective permeability of the rust layer to corrosive media; simultaneously, the addition of Cr effectively increases the self-corrosion potential of the steel, inhibiting corrosion, thereby effectively reducing the promoting effect of corrosion on material failure during the abrasion process and improving corrosion and wear resistance. In particular, the combination of Cr and Cu improves resistance to acidic media corrosion. Furthermore, high-strength steel contains a high amount of carbon (C), which forms a supersaturated solid solution after heat treatment. While this improves strength and hardness, it also deteriorates corrosion resistance. Therefore, the addition of an appropriate amount of chromium (Cr) compensates for the reduced corrosion resistance caused by C. Thus, its content in this invention shall not be less than 0.5%. On the other hand, high Cr content is detrimental to toughness and increases welding difficulty, so its content is limited to 0.5-1.0%.

[0021] In this invention, Sb can combine with Cu in steel to form a Cu2Sb film on the surface, which has the effect of inhibiting sulfuric acid corrosion. However, excessive addition of Sb will worsen the hot brittleness of Cu-containing steel, leading to the formation of network cracks on the surface of the billet and strip. Based on this, this invention limits its addition range to 0.04-0.12%.

[0022] Boron has good hardenability, which improves the hardness of steel plates. However, excessive boron content is detrimental to welding. Therefore, this invention controls its content to be within the range of 0.001-0.003%.

[0023] Nitrogen (Nb) is a strong nitride-carbide-forming element, capable of combining with carbon and nitrogen in steel to form intermediate phases such as NbC, Nb(CN), and NbN. The resulting fine carbide particles refine the microstructure and produce precipitation strengthening, significantly improving the strength of the steel plate. Furthermore, Nb inhibits the expansion of austenite interfaces, raising the recrystallization temperature of steel and enabling rolling in the non-recrystallization zone at higher temperatures. Therefore, adding an appropriate amount of Nb to steel is beneficial for strength improvement. The carbonitrides formed by Nb can pin austenite grain boundaries during austenitization, inhibiting abnormal austenite grain growth and improving the toughness of the steel plate after quenching. However, excessive Nb is detrimental to welding, and it readily forms brittle metallic hydrides with hydrogen. These hydrides exhibit significant differences in ductility and toughness compared to the matrix, and their bonding strength with the matrix is ​​also poor, leading to delayed cracking. Therefore, this invention controls its content to 0.01-0.03%.

[0024] Ti inhibits austenite grain growth during slab reheating and ferrite grain growth during recrystallization controlled rolling, thus improving steel toughness. Furthermore, Ti preferentially combines with nitrogen (N) in the steel, reducing the amount of AlN. However, excessively high Ti content is detrimental to low-temperature impact toughness. Therefore, this invention controls its content to 0.01-0.03%.

[0025] Furthermore, in the 1100MPa grade acid-resistant high-strength steel plate described in this invention, the mass percentage content of Cr, Cu, and Al satisfies the following relationship: Cr + 0.82Cu + 2.89Al ≥ 1.0.

[0026] Furthermore, in the 1100MPa grade acid-resistant high-strength steel plate described in this invention, the mass percentage content of Cu, Cr, Al and Sb satisfies the following relationship: Cu + 1.22Cr + 3.53Al + 10Sb ≥ 2.0.

[0027] As mentioned above, the key to this invention lies in solving the problem of high-strength steel's poor corrosion resistance and short service life in acidic environments. Although high-strength steel possesses high strength and hardness, it, like ordinary carbon steel, is susceptible to corrosion in acidic environments, leading to premature failure of structural components. This invention, combining the failure mechanisms of steel materials in acidic environments, effectively improves corrosion resistance by incorporating various corrosion-resistant elements such as Cu, Sb, Cr, and Al while maintaining high strength and hardness.

[0028] The addition of Cu and Cr increases the matrix potential, and Cu combines with S in the steel to improve corrosion resistance in acidic media. The combination of Cr and Al in a specific ratio also benefits corrosion resistance in acidic media. Besides Al, the addition of Cr and Cu also increases strength; in addition to solid solution strengthening, Cu can also disperse and precipitate in the steel matrix, thus increasing strength. Sb combines with Cu to form Cu₂Sb during corrosion, effectively reducing the corrosion rate. This invention maximizes the synergistic effect of the above elements through the following elemental relationships: Cr + 0.82Cu + 2.89Al ≥ 1.0, Cu + 1.22Cr + 3.53Al + 10Sb ≥ 2.0, thereby improving corrosion resistance in acidic media environments.

[0029] Furthermore, the 1100MPa grade acid-resistant high-strength steel plate of the present invention also contains at least one of the following chemical elements in mass percentage:

[0030] Mo: 0.02-0.05%;

[0031] W: 0.01-0.5%;

[0032] RE+V: 0.02-0.12%;

[0033] Ca: 0.001-0.01%.

[0034] Mo can exist in steel in solid solution, resulting in solid solution strengthening. In addition, Mo improves the hardenability of the matrix, thereby increasing the strength of the steel plate. During quenching heat treatment, Mo promotes the formation of martensite, exhibiting phase transformation strengthening and dislocation strengthening effects. Simultaneously, Mo increases the solubility of Nb, V, and Ti, promoting precipitation strengthening. Furthermore, the addition of Mo improves the corrosion product film structure, enhancing the steel's resistance to pitting and crevice corrosion. Furthermore, Mo's combination with Cr in the steel is beneficial for improving corrosion resistance in acidic environments. However, higher Mo content is detrimental to weldability and increases cost. Therefore, this invention limits its content to 0.02-0.05%.

[0035] In this invention, W forms carbides in steel, resulting in secondary strengthening and solid solution strengthening effects, and during overaging, it suppresses the segregation of impurity atoms and non-metallic inclusions at grain boundaries, thereby improving fracture toughness. Based on this, its content is controlled at 0.01-0.5%.

[0036] The addition of rare earth elements (RE) is beneficial to improving corrosion resistance. RE forms RE compounds, RE / Fe intermetallic compounds, and dissolved rare earth elements in steel, which hydrolyze in the thin corrosion film and precipitate at the cathodic site with a high pH value, thus playing a role in corrosion inhibition. V is also a strong carbonitride forming element, which can precipitate during phase transformation. In steel, it has solid solution strengthening and carbonitride precipitation strengthening effects, and increases tempering stability, thereby improving strength. Based on this, the total amount of V is controlled at 0.02-0.12%.

[0037] In this invention, the purpose of adding Ca is to change the shape of sulfides, suppress the hot brittleness of S, and improve toughness.

[0038] Furthermore, in the 1100MPa grade acid-resistant high-strength steel plate of the present invention, when it contains Mo, the mass percentage content of Cu, Cr, Mo, Al and Sb satisfies the following relationship: Cu + 1.22Cr + 3.53Al + 0.66Mo + 10Sb ≥ 2.0.

[0039] When Mo is present, this invention utilizes the combination of Cr, Al, and Mo to significantly improve corrosion resistance in acidic media environments. As mentioned above, even without Mo, the equation Cu + 1.22Cr + 3.53Al + 10Sb ≥ 2.0 still holds true. The difference lies in the fact that, compared to adding Mo, without adding Mo, the contents of Al and Cr need to be significantly increased.

[0040] Furthermore, in the unavoidable impurity elements of the 1100MPa grade acid-resistant high-strength steel plate described in this invention: P≤0.018%, N≤0.005%, S≤0.01%.

[0041] The unavoidable impurities in this invention are mainly P, S and N, and it is desirable that their content be as low as possible.

[0042] Phosphorus (P) is a major corrosion-resistant element in traditional atmospheric corrosion-resistant steels, promoting the formation of a protective rust layer and effectively improving the steel's atmospheric corrosion resistance. However, during abrasion, the formation of this rust layer accelerates material wear and weight loss, reducing wear resistance. Furthermore, the presence of P easily leads to segregation, reducing the steel's toughness and plasticity, and making the steel plate brittle and affecting its toughness. Therefore, the P content in steel should be minimized. However, excessively low P control requirements increase alloy costs and steelmaking difficulty. Therefore, this invention controls the P content to below 0.018%.

[0043] Although sulfur (S) can improve the yield strength of steel, it easily forms manganese sulfide, a plastic inclusion, with Mn during solidification, which is detrimental to transverse plasticity and toughness. When volatile organic compounds (V) are present, fine MnS will promote the precipitation of fine VN, which serves as a nucleation site for intragranular ferrite (IGF), refining the ferrite-pearlite structure and improving strength and toughness. However, the presence of sulfur will worsen the atmospheric corrosion resistance of steel and make the steel plate brittle, reducing the low-temperature toughness of the steel. Therefore, its content should be controlled below 0.01%.

[0044] Although nitrogen (N) can form nitrides with Nb, V, and Ti in steel, and these fine precipitates act as grain boundaries, refining austenite grains, and the precipitated nitrides also have a precipitation strengthening effect, higher levels of N in steel readily combine with Al to form AlN, significantly increasing the amount of nitrides in the steel. When AlN exists independently as a non-metallic inclusion in steel, it disrupts the continuity of the steel matrix, especially when the Al content is high, resulting in a larger quantity of AlN and a more aggregated distribution, which is even more detrimental. Furthermore, higher levels of N tend to accumulate at defects, worsening low-temperature impact toughness. Therefore, this invention controls N as an impurity element, limiting the N content to below 0.005%.

[0045] Furthermore, the microstructure of the 1100MPa grade acid-resistant high-strength steel plate described in this invention is martensitic. This microstructure ensures the high hardness of the steel plate.

[0046] Furthermore, the thickness of the 1100MPa grade acid-resistant high-strength steel plate described in this invention is 3-20mm.

[0047] Furthermore, the 1100MPa grade acid-resistant high-strength steel plate of the present invention has a yield strength ≥960MPa, tensile strength ≥1100MPa, elongation ≥15%, hardness of 370-430HBW, and impact energy value at -40℃ ≥60J; its relative corrosion rate compared to ordinary carbon steel is less than 20%.

[0048] Accordingly, another objective of the present invention is to provide a method for manufacturing a high-strength steel plate with an 1100MPa grade resistant to acidic media corrosion. This manufacturing method, combined with the composition design system described above, can achieve a comprehensive performance of high-strength steel plate with excellent wear resistance and acidic media corrosion resistance.

[0049] To achieve the above objectives, this invention proposes a method for manufacturing a high-strength steel plate resistant to acidic media corrosion at a pressure of 1100 MPa, comprising the following steps:

[0050] (1) Smelting and casting;

[0051] (2) Reheating of the slab;

[0052] (3) Rough rolling and finish rolling, laminar flow cooling, coiling;

[0053] (4) Heat treatment: The quenching temperature is 820-845℃, the holding time is (1.5~2)×steel plate thickness t, and then water quenched to room temperature with a cooling rate ≥60℃ / s; The tempering temperature is 230-270℃, the holding time is (2~3)×steel plate thickness t, and shall not be less than 10min; the unit parameter of t is mm, and the unit parameter of holding time is min.

[0054] In this invention, offline heat treatment can be used. The quenching temperature directly affects the grain size of the subsequent martensite structure, and thus the toughness of the steel plate. Excessively high quenching temperatures can coarsen the austenite grains, resulting in a large martensite structure and deteriorated toughness after quenching. Conversely, excessively low quenching temperatures lead to incomplete austenitization, preventing the formation of a fully martensitic structure and negatively impacting toughness. The quenching holding time also exhibits a similar effect on quenching performance. Excessively long holding times result in coarse grains, increased energy consumption, and higher costs, while insufficient holding times lead to incomplete austenitization, resulting in insufficient hardness and strength after quenching.

[0055] To achieve outstanding low-temperature toughness, this invention employs a critical zone quenching process for steel plates. The critical zone quenching microstructure contains undissolved acicular ferrite. While this undissolved acicular ferrite reduces strength to some extent, it reaches its strength limit before martensite under external force, allowing cracks to initiate and propagate within it first, absorbing energy and thus improving toughness. Therefore, controlling the quenching temperature between -5°C and +20°C above Ac3, i.e., between 820-845°C, yields better low-temperature toughness.

[0056] This invention involves tempering steel plates within the temperature range of 230-270℃. The tempering process primarily aims to reduce and eliminate quenching stress, improve toughness and flexibility. Excessively high tempering temperatures can lead to excessive reductions in the strength and hardness of the steel plate, failing to meet design requirements and increasing costs. The tempering holding time begins from the core of the steel plate reaching the set temperature and is 2-3 times the plate thickness (mm) in minutes, but must not be less than 10 minutes.

[0057] Furthermore, in step (2) of the manufacturing method described in this invention, the heating temperature is ≥1230℃ and the heat soaking time is ≥40min.

[0058] Considering that trace amounts of Ti and / or Nb are added to the steel grade of this invention, in order to ensure that its carbonitrides are fully dissolved, the preferred heating temperature is controlled above 1230°C and the holding time is 2 hours, wherein the soaking and holding time is not less than 40 minutes.

[0059] In addition, the billet can be hot-charged into the furnace after casting. That is, after confirming that there are no quality problems on the surface of the billet, it can be directly transported from the casting area to the heating furnace through the roller conveyor for heating and heat preservation, thereby reducing energy consumption. If it cannot be hot-charged, the cast billet must be placed in the heat preservation pit for slow cooling after casting. The heat preservation pit can be removed and air-cooled after the temperature drops below 200°C.

[0060] Furthermore, in step (3) of the manufacturing method described in this invention, the finishing rolling temperature is controlled to be ≥880℃.

[0061] The steel grade of this invention undergoes offline heat treatment after rolling, therefore there are no special requirements for the rolling temperature of the cast billet. However, to reduce rolling load, it is preferable to use the highest possible final rolling and coiling temperature. Since the α→γ transformation point of the steel grade of this invention is approximately 827℃, a final rolling temperature of 880℃ or higher is recommended to ensure rolling in the complete austenitic region, thereby achieving low and stable rolling load, which is beneficial for obtaining high-quality sheet shape in subsequent processes.

[0062] Of course, when the steel plate is thicker, the final rolling temperature can be appropriately reduced, but it is best not to go below 860℃.

[0063] Furthermore, in step (3) of the manufacturing method described in this invention, the deformation ratio in the roughing stage is greater than 80%; and the reduction rate in the last pass of finishing rolling is ≥16%.

[0064] The rolling process in this invention is divided into two stages: roughing and finishing. To obtain a fine initial austenite grain size, the billet undergoes a large reduction during the roughing stage, with a deformation ratio (i.e., total reduction rate) exceeding 80%. Furthermore, to achieve a fine grain size and good plate shape, the reduction rate in the final finishing pass is controlled to be no less than 16%.

[0065] Furthermore, in step (3) of the manufacturing method described in this invention, the winding temperature is controlled to be 620-680°C.

[0066] After rolling, the steel coil is cooled to between 620-680℃ by laminar flow cooling before coiling because: if the coiling temperature is too high, the cooling rate will be too low, resulting in coarse grains in the steel coil, which is also detrimental to the coiling machine; if the coiling temperature is too low, bainite structure is easily formed, which increases the strength of the steel plate and increases the difficulty of subsequent uncoiling and straightening.

[0067] The 1100MPa grade acid-resistant high-strength steel plate described in this invention has the following advantages and beneficial effects:

[0068] The 1100MPa grade acid-resistant high-strength steel plate of this invention is based on C-Mn with the addition of small amounts of Nb, Ti microalloying elements and Sb, Cu, Cr and Al. While ensuring high strength and high hardness, it achieves excellent corrosion resistance under acidic corrosive media. Thus, the steel plate is both wear-resistant and corrosion-resistant under acidic corrosive media, effectively extending the service life of equipment and reducing costs.

[0069] The 1100MPa grade acid-resistant high-strength steel plate described in this invention has good low-temperature impact toughness and cold bending performance, which can meet the requirements of subsequent processing and use.

[0070] The 1100MPa grade acid-resistant high-strength steel plate of the present invention has excellent low-temperature toughness and corrosion resistance, significantly improving the corrosion resistance of high-strength steel plates in acidic corrosive media. Its corrosion resistance is more than 5 times that of ordinary carbon steel, and its relative corrosion rate is less than 20%.

[0071] The manufacturing method of the 1100MPa grade acid-resistant high-strength steel plate described in this invention is simple and reduces production difficulty and cost. Detailed Implementation

[0072] The following will further explain and illustrate the 1100MPa grade acid-resistant high-strength steel plate and its manufacturing method described in this invention with reference to specific embodiments. However, this explanation and illustration do not constitute an improper limitation on the technical solution of this invention.

[0073] Examples 1-16 and Comparative Examples 1-3

[0074] The 1100MPa grade acid-resistant high-strength steel plates described in Examples 1-16 of this invention are prepared using the following steps:

[0075] (1) Deep desulfurization of molten iron → combined blowing at the top and bottom of the converter → ladle refining → continuous casting; the mass percentage of each element in the billet is shown in Table 1.

[0076] (2) Slab reheating: heating temperature ≥1230℃, holding time ≥2h (the heating of slab in the heating furnace is divided into: preheating section, heating section and heat soaking and holding section, and the holding time refers to the total time of slab in the heating furnace), heat soaking and holding time ≥40min;

[0077] (3) Roughing and finishing: Control the finishing rolling temperature to ≥880℃; the deformation ratio (i.e., the total reduction rate of roughing) to be greater than 80%; the reduction rate of the last pass of finishing rolling to be ≥16%;

[0078] (4) Winding after laminar flow cooling: Control the winding temperature to 620-680℃;

[0079] (5) Uncoiling → Straightening → Cutting;

[0080] (6) Offline heat treatment: The quenching temperature is 820-845℃, the holding time is (1.5~2)×steel plate thickness t, and then water quenched to room temperature with a cooling rate ≥60℃ / s; The tempering temperature is 230-270℃, the holding time is (2~3)×steel plate thickness t, and shall not be less than 10min; the unit parameter of t is mm, and the unit parameter of holding time is min;

[0081] (7) Finishing.

[0082] It should be noted that although the manufacturing methods and steps of Comparative Examples 1-3 are basically the same as those of the embodiments of the present invention, their component ratios and specific process parameters do not conform to the present invention.

[0083] Table 1 lists the mass percentage of each chemical element in the steel plates of Examples 1-16 and the comparative steel plates of Comparative Examples 1-3.

[0084] Table 1. (wt%, balance Fe and other unavoidable impurities besides P, S, and N)

[0085]

[0086]

[0087] Note: In Table 1, I represents Cr + 0.82Cu + 2.89Al. In the examples without Mo, M represents Cu + 1.22Cr + 3.53Al + 10Sb. In the examples containing Mo, M represents Cu + 1.22Cr + 3.53Al + 0.66Mo + 10Sb.

[0088] Table 2 lists the specific process parameters for the steel plates of Examples 1-16 and the comparative steel plates of Comparative Examples 1-3.

[0089] Table 2.

[0090]

[0091] Samples of the steel plates from Examples 1-16 and the comparative steel plates from Comparative Examples 1-3, obtained through the above-described process steps, were taken for mechanical property testing and corrosion resistance testing. The test results are listed in Table 3. The relevant testing methods are as follows:

[0092] (1) Tensile property test: A transverse sample was taken from the steel plate and processed into a JIS13A specimen. Tensile tests were conducted at room temperature on an SCL185 tensile testing machine according to GB / T228.1-2021 Metallic materials, tensile testing—Part 1: Tensile testing at room temperature. The speed was 4 mm / min before yielding and 48 mm / min after yielding. The yield strength Rp0.2 of the steel plate was measured (when yielding is not obvious, R is used as the reference). eH (alternative), tensile strength R m Elongation A50.

[0093] (2) Low-temperature impact toughness test: Under an ambient temperature of -40℃, transverse samples were taken at 1 / 4 of the steel plate thickness and tested according to GB / T 229 "Charpy Impact Test Method for Metallic Materials". The average KV2 impact value of the standard sample at -40℃ was obtained. Among them, the 8mm steel plate used a 7.5*10*55mm impact sample, and the corresponding impact energy value was reduced accordingly. The full-size impact energy was 63J. Examples 1 and 2 involve steel plates with a thickness of less than 6mm, which were not subjected to impact tests, so no data is available.

[0094] (3) Hardness test: A 60*60mm hardness sample was machined from the steel plate, and 0.5mm of the sample surface was removed by grinding on a grinding machine. The hardness was tested using a BRIN400D Brinell hardness tester according to the hardness test method GB / T 231.1-2009. Test conditions: 10 / 3000.

[0095] (4) The acid resistance of the sample was tested in a 10% H2SO4 + 3.5% NaCl solution at a temperature of 23±2℃ for a test period of 24h. The relative corrosion rate was obtained by comparing it with Q345B.

[0096] Table 3 lists the performance test results of the steel plates of Examples 1-16 and the comparative steel plates of Comparative Examples 1-3.

[0097] Table 3.

[0098]

[0099] As can be seen from Table 3, the steel plates of Examples 1-16 of this invention all have a yield strength greater than 960 MPa, a tensile strength greater than 1100 MPa, an elongation greater than 15%, a hardness greater than 390 HBW, and an impact energy value of ≥60 J at -40℃; their relative corrosion rate compared to ordinary carbon steel is less than 20%. However, the elongation, low-temperature toughness, and resistance to acidic media corrosion of Comparative Examples 1-3 cannot reach the performance of this invention.

[0100] In summary, it can be seen that the steel plate manufactured using the technical solution of the present invention has high strength, high hardness, and excellent resistance to acidic media corrosion.

[0101] It should be noted that the combination of the technical features in this case is not limited to the combination methods described in the claims of this case or the combination methods described in the specific embodiments. All technical features described in this case can be freely combined or combined in any way, unless they contradict each other.

[0102] It should also be noted that the embodiments listed above are merely specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and similar changes or modifications made thereto are those that can be directly derived or easily conceived by those skilled in the art from the content disclosed in the present invention, and should all fall within the protection scope of the present invention.

Claims

1. A high-strength steel plate resistant to acidic media corrosion at 1100MPa, containing Fe and unavoidable impurity elements, characterized in that... It also contains the following chemical elements in the following mass percentages: C: 0.12-0.18%, Si: 0.1-0.3%, Mn: 0.5-0.9%, Cu: 0.15-0.35%, Al: 0.015-0.15%, Cr: 0.5-1.0%, Sb: 0.04-0.12%, B: 0.001-0.003%; and one or two of Nb: 0.01-0.03% and Ti: 0.01-0.03%; wherein the mass percentage content of Cu, Cr, Al and Sb satisfies the relationship: Cu + 1.22Cr + 3.53Al + 10Sb ≥ 2.

0.

2. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1, characterized in that, Its mass percentage content of each chemical element is as follows: C: 0.12-0.18%, Si: 0.1-0.3%, Mn: 0.5-0.9%, Cu: 0.15-0.35%, Al: 0.015-0.15%, Cr: 0.5-1.0%, Sb: 0.04-0.12%, B: 0.001-0.003%; and one or both of Nb: 0.01-0.03% and Ti: 0.01-0.03%; the balance being Fe and unavoidable impurity elements.

3. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, The mass percentages of Cr, Cu, and Al satisfy the following relationship: Cr + 0.82Cu + 2.89Al ≥ 1.

0.

4. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, It also contains at least one of the following chemical elements in the following mass percentages: Mo: 0.02-0.05%; W:0.01-0.5%; RE+V: 0.02-0.12%; Ca: 0.001-0.01%.

5. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 4, characterized in that, When it contains Mo, the mass percentage content of Cu, Cr, Mo, Al and Sb satisfies the following relationship: Cu + 1.22Cr + 3.53Al + 0.66Mo + 10Sb ≥ 2.

0.

6. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, Among unavoidable impurity elements: P≤0.018%, N≤0.005%, S≤0.01%.

7. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, Its microstructure is martensite.

8. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, Its thickness ranges from 3 to 20 mm.

9. The 1100MPa grade acid-resistant high-strength steel plate as described in claim 1 or 2, characterized in that, Its yield strength is ≥960MPa, tensile strength is ≥1100MPa, elongation is ≥15%, hardness is 370-430HBW, and impact energy at -40℃ is ≥60J.

10. The method for manufacturing a 1100MPa grade acid-resistant high-strength steel plate according to any one of claims 1-9, characterized in that, It includes the following steps: (1) Smelting and casting; (2) Reheating of the slab; (3) Rough rolling and finish rolling, laminar flow cooling, coiling; (4) Heat treatment: The quenching temperature is 820-845℃, the holding time is (1.5~2)×steel plate thickness t, and then water quenched to room temperature with a cooling rate ≥60℃ / s; The tempering temperature is 230-270℃, the holding time is (2~3)×steel plate thickness t, and shall not be less than 10min; the unit parameter of t is mm, and the unit parameter of holding time is min.

11. The manufacturing method as described in claim 10, characterized in that, In step (2), the heating temperature is ≥1230℃ and the heat preservation time is ≥40min.

12. The manufacturing method as described in claim 10, characterized in that, In step (3), the finishing rolling temperature is controlled to be ≥880℃.

13. The manufacturing method as described in claim 10, characterized in that, In step (3), the deformation ratio in the roughing stage is greater than 80%; the reduction rate in the last pass of finishing rolling is ≥16%.

14. The manufacturing method as described in claim 10, characterized in that, In step (3), the winding temperature is controlled to be 620-680℃.

Citation Information

Patent Citations

  • A hot-rolled steel plate resistant to atmospheric corrosion for railway freight cars and its manufacturing method

    CN102268613A

  • Low-alloy high-toughness wear resistant steel plate and manufacturing method thereof

    CN103146997A

  • High-hardness wear-resistant corrosion-resistant steel plate for slurry dredging and production method thereof

    CN108930001A

  • Cold-rolled steel resistant to low-temperature acid dew point corrosion and manufacturing method thereof

    CN112575269A

  • Ultra-fine grained high-strength steel plate with 1100 mpa-grade yield strength and production method thereof

    WO2019222988A1