Low dark current p on n-type mercury cadmium telluride device, preparation method and infrared detector
By establishing simulation models and performance testing experiments, we optimized the doping concentration and structural thickness of the p on n-type mercury cadmium telluride infrared detector, which solved the problem of difficult control of the dark current of the device and achieved high performance and low dark current infrared detection. device.
Patent Information
- Application Number
- CN202410749479.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The performance of existing p on n-type mercury cadmium telluride infrared detectors cannot meet the needs of technological development, and the doping concentration of the material structure layer and the device structure cannot be accurately controlled during the device preparation process, making it difficult to optimize the dark current.
By establishing a simulation model and conducting performance testing experiments, we can obtain the relationship between the p-type layer, n-type layer doping concentration and transition layer thickness and dark current, determine the doping concentration range and thickness range of the device to be prepared, and optimize the device structure. to reduce dark current.
Theoretical optimization of the doping concentration and transition layer thickness of each layer of the conventional p on n mesa long-wave mercury cadmium telluride infrared detector has been achieved, reducing the dark current of the device and improving the sensitivity and responsivity of the device.
Smart Images

Figure CN118335849B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of diodes, and in particular to a low dark current ponn-type mercury cadmium telluride device, a preparation method and an infrared detector. Background Art
[0002] HgCdTe materials have the advantages of extremely high photoelectric conversion efficiency, good carrier transport characteristics, and adjustable response range with components. Mercury cadmium telluride (HgCdTe) infrared detectors are widely used in infrared detection systems and can work in the atmospheric windows of 1~3, 3~5 and 8~12μm. With the development of HgCdTe infrared detection technology in the past 50 years, the position of HgCdTe materials in the field of infrared detection has become as important as that of silicon materials in the field of microelectronics. Photodetectors, especially ponn mercury cadmium telluride photodetectors, have recently been widely used in fiber optic communications, 3D lidar, astronomical observations, and atmospheric detection due to their good detection performance.
[0003] Compared with the traditional n on p structure, the p on n type HgCdTe infrared detector can obtain lower dark current. The In-doped HgCdTe n-type absorption layer material is grown in situ on the CdZnTe substrate by the horizontal slide boat tellurium-rich liquid phase epitaxial growth method, and then the p-type As-externally doped p on n type planar type and double-layer heterojunction mesa type chip preparation are realized by As ion implantation technology and mercury-rich vertical liquid phase epitaxial growth technology respectively. In addition, the n-type series resistance is low. By optimizing the device process and controlling the non-intrinsic In and Au doping levels, the p on n type HgCdTe infrared detector can reduce the dark current by 1~2 orders of magnitude compared with the traditional n on p structure.
[0004] However, the performance level of ponn-type HgCdTe infrared detectors is still difficult to meet the needs of technological development in various fields. Moreover, due to the current measurement methods, preparation conditions, dark current and other factors, the systematic relationship between the doping concentration of each material structure layer, device structure and device dark current cannot be accurately obtained during the device preparation process to optimize the device. In addition, the relevant literature and process experience have inconsistent or even opposite descriptions of the relationship between material doping concentration, device structure thickness and dark current. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to prepare a low dark current pon n-type mercury cadmium telluride device. The present invention provides a low dark current pon n-type mercury cadmium telluride device, a preparation method and an infrared detector.
[0006] A method for preparing a low dark current pon n-type mercury cadmium telluride device according to an embodiment of the present invention comprises:
[0007] S10, establishing a simulation model of a p on n-type HgCdTe device, and obtaining the relationship trends among the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness and the dark current through performance test experiments;
[0008] S20, determining a p-type layer doping concentration range, an n-type layer doping concentration range, and a transition layer thickness range of a p on n-type cadmium telluride device to be prepared based on the obtained relationship trends among the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness, and the dark current;
[0009] S30, growing a substrate layer, and sequentially growing an n-type layer, a transition layer, and a p-type layer on the substrate layer;
[0010] Wherein, when the p on n-type cadmium telluride device is a table-type long-wave device, the doping In concentration range of the n-type layer is 1×10 15 / cm 3 ~1×10 18 / cm 3 The thickness of the transition layer is in the range of 0.1 μm to 0.3 μm, and the concentration of Hg vacancies or As doped in the p-type layer is in the range of 5×10 15 / cm 3 ~5×10 17 / cm 3 .
[0011] According to some embodiments of the present invention, in step S10, simulation software is used to establish a p on n-type mercury cadmium telluride simulation model, and p-type layer doping concentration and dark current performance test experiments, n-type layer doping concentration and dark current performance test experiments, and transition layer thickness and dark current performance test experiments are performed respectively.
[0012] In some embodiments of the present invention, step S20 includes:
[0013] S21, generating a first relationship trend graph between p-type layer doping concentration and dark current from the experimental data obtained from the performance test experiment, and obtaining the p-type layer doping concentration range from the first relationship trend graph;
[0014] S22, generating a second relationship trend graph between n-type layer doping concentration and dark current from the experimental data obtained from the performance test experiment, and obtaining the n-type layer doping concentration range from the second relationship trend graph;
[0015] S23, generating a third relationship trend graph between transition layer thickness and dark current from the experimental data obtained from the performance test experiment, and obtaining the thickness range of the transition layer from the third relationship trend graph.
[0016] According to some embodiments of the present invention, when the ponn-type cadmium telluride device is a mesa-type long-wave device, the thickness of the n-type layer ranges from 9 μm to 10 μm, and the Cd component value ranges from 0.2 to 0.25.
[0017] In some embodiments of the present invention, when the ponn-type cadmium telluride device is a mesa-type long-wave device, the transition layer is doped with In at a concentration of 1×10 15 / cm 3 , and the Cd component of the transition layer adopts a Gaussian state slow change, the Cd component value is between 0.25 and 0.35, and the Cd component value of the transition layer is 0.02 to 0.05 higher than the Cd component value of the p-type layer.
[0018] According to some embodiments of the present invention, when the p on n-type cadmium telluride device is a mesa-type long-wave device, the thickness range of the p-type layer is 1.8 μm~2.0 μm, the Cd component value is between 0.22~0.27, and the Cd component value of the p-type layer is 0.02~0.05 higher than the Cd component value of the n-type layer.
[0019] According to the low dark current pon n-type mercury cadmium telluride device of the embodiment of the present invention, the mercury cadmium telluride device is obtained by using the preparation method of the low dark current pon n-type mercury cadmium telluride device as described above, and the mercury cadmium telluride device is a mesa-type long-wave device, comprising:
[0020] substrate layer;
[0021] An n-type layer is grown on the substrate layer, and the doping concentration of the n-type layer is in the range of 1×10 15 / cm 3 ~1×10 18 / cm 3 ;
[0022] A transition layer, grown on the n-type layer, wherein the thickness of the transition layer is in the range of 0.1 μm to 0.3 μm;
[0023] A p-type layer is grown on the transition layer, and the p-type layer is doped with Hg vacancies or As at a concentration of 5×10 15 / cm 3 ~5×10 17 / cm 3 .
[0024] According to some embodiments of the present invention, the thickness range of the n-type layer is 9 μm~10 μm, and the Cd component value is between 0.2~0.25; the thickness range of the p-type layer is 1.8 μm~2.0 μm, and the Cd component value is 0.22~0.27, and the Cd component value of the p-type layer is 0.02~0.05 higher than the Cd component value of the n-type layer.
[0025] In some embodiments of the present invention, the transition layer is doped with In at a concentration of 1×10 15 cm 3 , and the Cd component of the transition layer adopts a Gaussian state slow change, the Cd component value is between 0.25 and 0.35, and the Cd component value of the transition layer is 0.02 to 0.05 higher than the Cd component value of the p-type layer.
[0026] The low dark current ponn-type mercury cadmium telluride infrared detector according to an embodiment of the present invention comprises:
[0027] A p on n type mercury cadmium telluride device is prepared by using the method for preparing the low dark current p on n type mercury cadmium telluride device as described above.
[0028] The present invention has the following beneficial effects:
[0029] The present invention obtains theoretical optimal values and related trends of doping concentration of each layer and thickness of transition layer of conventional p on n table-top long-wave HgCdTe infrared detector through performance experiments and calculations from multiple angles. Corresponding only to dark current, the higher the doping concentration of n-type layer (n-type layer doped with In), the smaller the dark current. As the doping concentration of p-type layer (p-type layer doped with Hg vacancies or As) increases, the dark current of the device decreases first and then increases. At 1×10 16 / cm 3 The dark current near the detector reaches the minimum value. Combined with other device performances, such as sensitivity, responsiveness, etc., referring to the relationship trend, the n-type layer doping concentration range of the p on n table-top long-wave HgCdTe infrared detector device can be selected in the range of 1×10 15 / cm 3 ~1×10 18 / cm 3 The p-type layer doping concentration range can be selected between 5×10 15 / cm 3 ~5×10 17 / cm 3 The thickness of the transition layer can be selected between 0.1μm and 0.3μm, and according to the trend graph, the doping concentration of each layer of the device and the thickness of the device structure can be selected for each specific application scenario to optimize the device. The present invention has a very important reference significance for improving the high performance of conventional ponn table-type long-wave HgCdTe infrared detector devices while maintaining relatively low dark current of the device.
[0030] At the same time, under the conditions of preparation and other device performance conditions, in order to further smooth the energy band, reduce the dark current of the device, and reduce the device capacitance, the table-type and planar ponn mercury cadmium telluride infrared detector devices can be improved as follows:
[0031] (1) In the transition region from the mesa p-type layer to the transition layer (e.g. within 1 μm), the Cd component can be increased slowly from the p-type layer component to the transition layer peak, and the doping concentration in the transition region is the same as the p-type layer or slightly lower than the p-type layer but higher than the transition layer; (2) The mesa transition layer component value can be in the form of Gaussian distribution, and the doping concentration is slightly lower than the p-type layer and the n-type layer; (3) In the transition region from the mesa n-type layer to the transition layer, a transition drift layer can be appropriately added with a thickness of 0.5 μm to 2 μm, and the component slowly increases from the n-type layer component to the transition layer peak, and the doping concentration slowly decreases from the n-type layer doping concentration to the transition layer. The addition of this layer can smooth the device energy band, reduce the device dark current, reduce the device capacitance, and improve the device performance; (4) The side of the mesa p-type pixel can be kept moderately tilted to reduce electric field crowding and dark current; (5) The planar p-type injection region can be kept moderately tilted to further reduce electric field crowding and reduce device dark current. The present invention realizes the preparation of low dark current devices and has high application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a flow chart of a method for preparing a low dark current pon n-type mercury cadmium telluride device according to an embodiment of the present invention;
[0033] Figure 2 is a flow chart of a method for preparing a low dark current pon n-type mercury cadmium telluride device according to an embodiment of the present invention;
[0034] Figure 3 Schematic diagram of the structure of a low dark current mesa-type ponn mercury cadmium telluride device according to an embodiment of the present invention;
[0035] Figure 4 is a trend diagram of the relationship between the doping concentration of the n-type layer and the dark current of the low dark current mesa ponn HgCdTe device according to an embodiment of the present invention (the small figure in the right figure is an enlarged view of the data in the circle);
[0036] Figure 5 is a trend diagram of the relationship between the transition layer thickness and the dark current of a low dark current mesa-type ponn HgCdTe device according to an embodiment of the present invention;
[0037] Figure 6 Schematic diagram showing the main influencing factors of dark current of a mesa-type ponn HgCdTe device according to an embodiment of the present invention: the influence of minority carrier lifetime and doping concentration in the n-type layer on dark current;
[0038] Figure 7 is a schematic structural diagram of a mesa-type ponn device according to an embodiment of the present invention;
[0039] Figure 8 Schematic diagram of the structure of a planar pon device according to an embodiment of the present invention.
[0040] Reference numerals:
[0041] Mercury cadmium telluride device 100,
[0042] The substrate layer 10 , the n-type layer 20 , the transition layer 30 , the p-type layer 40 , and the drift enhancement layer 50 . DETAILED DESCRIPTION
[0043] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose, the present invention is described in detail below in conjunction with the accompanying drawings and preferred embodiments.
[0044] The description of the method flow in the specification of the present invention and the steps of the flowchart in the drawings of the specification of the present invention do not have to be strictly executed according to the step numbers, and the method steps can be executed in a different order. Moreover, some steps can be omitted, multiple steps can be combined into one step, and / or one step can be decomposed into multiple steps.
[0045] In order to meet people's requirements for high sensitivity, high responsiveness, high power and low dark current of mercury cadmium telluride avalanche photodetectors and for the rationality of device preparation, the present invention provides the correlation trend of the doping concentration, thickness and dark current of each layer of the ponn mercury cadmium telluride photodetector according to the physical mechanism of dark current generation of the mercury cadmium telluride photodetector by establishing a simulation model and conducting performance test experiments, and optimizes the material preparation and device structure parameters, thereby providing a high-performance photodetector with good sensitivity, high response speed, small dark current and other noises.
[0046] Combination Figure 1 and Figure 3 As shown, a method for preparing a low dark current pon n-type mercury cadmium telluride device according to an embodiment of the present invention includes:
[0047] S10, establishing a simulation model of a p on n-type HgCdTe device, and obtaining the relationship trends among the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness and the dark current through performance test experiments;
[0048] According to some embodiments of the present invention, in step S10, simulation software can be used to establish a p on n-type mercury cadmium telluride simulation model, and p-type layer doping concentration and dark current performance test experiments, n-type layer doping concentration and dark current performance test experiments, and transition layer thickness and dark current performance test experiments are performed respectively.
[0049] S20, determining the p-type layer doping concentration range and extreme value, the n-type layer doping concentration range and the transition layer thickness range of the p-on-n-type cadmium telluride device to be prepared based on the obtained relationship trends among the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness and the dark current;
[0050] In some embodiments of the present invention, step S20 includes:
[0051] S21, generating a first relationship trend diagram between the p-type layer doping concentration and the dark current from the experimental data obtained from the performance test experiment, such as Figure 4 As shown in the right figure in , the doping concentration range, extreme value and optimal value of the p-type layer are obtained from the first relationship trend diagram;
[0052] S22, generating a second relationship trend diagram between the n-type layer doping concentration and the dark current from the experimental data obtained from the performance test experiment, such as Figure 4 As shown in the left figure in , the doping concentration range and the optimal value of the n-type layer are obtained from the second relationship trend diagram;
[0053] S23, generating a third relationship trend diagram between transition layer thickness and dark current from the experimental data obtained from the performance test experiment, such as Figure 5 As shown, the thickness range and the optimal value of the transition layer are obtained from the third relationship trend diagram.
[0054] S30, growing a substrate layer, and sequentially growing an n-type layer, a transition layer, and a p-type layer on the substrate layer.
[0055] It should be noted that if Figure 7 and Figure 8 As shown, the ponn type HgCdTe device includes a mesa type device and a planar type device. The above method of the present invention can be applied to mesa type devices and planar type devices. In practical applications, a corresponding simulation model can be established according to the specific structure of the ponn type HgCdTe device to be prepared.
[0056] Among them, Figure 2 As shown in the figure, when the p on n-type HgCdTe device is a table-type long-wave device, the optimal range of the doping In concentration of the n-type layer is 1×10 15 / cm 3 ~1×10 18 / cm 3 According to some embodiments of the present invention, in step S30, the thickness of the n-type layer ranges from 9 μm to 10 μm, for example, the thickness of the n-type layer can be selected to be 9.7 μm, and the Cd component value is between 0.2 and 0.25, for example, the Cd component value can be selected to be 0.22.
[0057] When the p on n type HgCdTe device is a table-type long-wave device, the thickness of the transition layer ranges from 0.1 μm to 0.3 μm. For example, the thickness of the transition layer can be selected to be 0.3 μm. In some embodiments of the present invention, when the p on n type HgCdTe device is a table-type long-wave device, the transition layer is doped with In at a concentration of 1×10 15 / cm 3, and the Cd component of the transition layer adopts a Gaussian state to slowly change, and the Cd component value is between 0.25 and 0.35.
[0058] When the p on n-type HgCdTe device is a table-type long-wave device, the optimal concentration of Hg vacancies or As doping in the p-type layer is 5×10 15 / cm 3 ~5×10 17 / cm 3 .Depend on Figure 4 As can be seen from the right figure, the concentration of Hg vacancies or As in the p-type layer is 1×10 16 / cm 3 According to some embodiments of the present invention, when the ponn-type HgCdTe device is a mesa-type long-wave device, the thickness of the p-type layer ranges from 1.8 μm to 2.0 μm, and the Cd component value ranges from 0.22 to 0.25.
[0059] It is worth emphasizing that there are many factors that affect the dark current of p on n type HgCdTe devices. Due to the limitations of the current measurement methods and preparation conditions in this field, the current method to reduce the dark current of p on n type HgCdTe devices is mainly to optimize and improve the layer structure of the device. In the current preparation process of p on n type HgCdTe devices, it is impossible to determine the clear relationship between the doping concentration and thickness of each material structure layer and the dark current of the device. Therefore, there is a lack of technology to adjust the material doping concentration and device structure thickness to achieve the optimization of reducing the dark current of the device.
[0060] The method for preparing a low dark current p on n-type mercury cadmium telluride device of the present invention obtains a clear relationship trend between the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness and the dark current, and accordingly prepares the low dark current p on n-type mercury cadmium telluride device by adjusting the p-type layer doping concentration, the n-type layer doping concentration and the transition layer thickness.
[0061] Among them, the difficulty in obtaining the above relationship lies in the determination of the experimental scheme. At present, there is no relatively accurate exploration of the relationship between the doping concentration of each material structure layer and the thickness of the material structure layer and the dark current of the pon n-type mercury cadmium telluride device in the field. Moreover, the current technology cannot achieve accurate control of the doping concentration of each material structure layer. Therefore, it is impossible to simply obtain the relationship between the doping concentration of each material structure layer and the thickness of the material structure layer and the dark current of the pon n-type mercury cadmium telluride device through experiments. The present invention creatively explores the relationship between the doping concentration of each material structure layer of the device and the thickness of the material structure layer and the dark current, and uses simulation models and performance test experiments and multiple angles ( Figure 6 ) obtained a clear relationship between the doping concentration of each material structure layer, the thickness of the material structure layer and the dark current.
[0062] Another difficulty in obtaining the above relationship is that the relationship between the doping concentration of each material structure layer and the thickness of the material structure layer and the dark current was previously unknown. The dark current does not produce a conventional linear change with the linear change of the doping concentration or thickness. In particular, the effect of the doped Hg vacancies or As concentration of the p-type layer on the dark current of the device. The dark current does not continue to decrease with the decrease of the doped Hg vacancies or As concentration of the p-type layer, but there is an extreme point where the dark current reaches the minimum value. In the absence of theoretical guidance, it is very difficult for technical personnel in this field to derive the above relationship.
[0063] According to the guidance of the above relationship, the present invention can design a low dark current pon n-type mercury cadmium telluride device whose dark current is significantly lower than that of existing devices. It has important guiding significance for the preparation of low dark current pon n-type mercury cadmium telluride devices, produces unexpected technical effects, and corresponding low dark current devices have been prepared through actual operation.
[0064] like Figure 3 As shown, according to the low dark current pon n-type mercury cadmium telluride device 100 of an embodiment of the present invention, the mercury cadmium telluride device 100 is obtained by adopting the preparation method of the low dark current pon n-type mercury cadmium telluride device 100 as described above. When the mercury cadmium telluride device 100 is a mesa-type device, the mercury cadmium telluride device 100 includes: a substrate layer 10, an n-type layer 20, a transition layer 30 and a p-type layer 40.
[0065] The n-type layer 20 is grown on the substrate layer 10, and the doping concentration of the n-type layer 20 is in the range of 1×10 15 / cm 3 ~1×10 18 / cm 3 The transition layer 30 is grown on the n-type layer 20, and the thickness of the transition layer 30 is in the range of 0.1 μm to 0.3 μm. The p-type layer 40 is grown on the transition layer 30, and the concentration of Hg vacancies or As doped in the p-type layer 40 is in the range of 5×10 15 / cm 3 ~5×10 17 / cm 3 .
[0066] According to some embodiments of the present invention, the thickness of the n-type layer 20 ranges from 9 μm to 10 μm. For example, the thickness of the n-type layer 20 can be selected to be 9.7 μm, and the Cd component value is 0.22; the thickness of the p-type layer 40 ranges from 1.8 μm to 2.0 μm, for example, the thickness of the p-type layer 40 can be selected to be 2.0 μm, and the Cd component value is between 0.22 and 0.27, for example, the Cd component value of the p-type layer can be selected to be 0.25.
[0067] In some embodiments of the present invention, the transition layer 30 is doped with In at a concentration of 1×10 15 / cm3 , and the Cd component of the transition layer 30 adopts a Gaussian state slow change, and the Cd component value is between 0.25 and 0.35.
[0068] The low dark current ponn-type mercury cadmium telluride infrared detector according to an embodiment of the present invention comprises:
[0069] The ponn-type HgCdTe device 100 is manufactured by using the method for manufacturing the ponn-type HgCdTe device 100 with low dark current as described above.
[0070] The present invention has the following beneficial effects:
[0071] The present invention obtains the theoretical optimal values and related trends of the doping concentration of each layer and the thickness of the transition layer of the conventional table-top ponn HgCdTe infrared detector through performance experiments and calculations. Corresponding only to the dark current, the higher the doping concentration of the n-type layer of the device (n-type layer doped with In), the smaller the dark current. As the doping concentration of the p-type layer increases, the dark current (p-type layer doped with Hg vacancies or As) decreases first and then increases, and at 1×10 16 / cm 3 Combined with other device properties, such as sensitivity and responsiveness, and referring to the relationship trend, the doping concentration range of the n-type layer of the mesa-type ponn HgCdTe infrared detector device can be selected to be 1×10 15 / cm 3 ~1×10 18 / cm 3 The p-type layer doping concentration range can be selected between 5×10 15 / cm 3 ~5×10 17 / cm 3 The thickness of the transition layer can be selected between 0.1μm and 0.3μm, and according to the trend chart, the doping concentration of each layer of the device and the thickness of the device structure can be selected according to each specific application scenario to optimize the device.
[0072] The following is a detailed description of the method for preparing a low dark current ponn-type HgCdTe device according to a specific embodiment of the present invention with reference to the accompanying drawings. It should be understood that the following description is only an exemplary description and should not be construed as a specific limitation on the present invention.
[0073] The present invention designs and optimizes the doping concentration of material preparation and device structural parameters according to actual needs, such as the dark current, sensitivity, and responsiveness of the device, so as to keep the dark current of the device as low as possible while ensuring the high performance of the device.
[0074] The present invention includes a specific parameter selection process and parameter value selection and determination for optimizing the doping concentration and device structure thickness of a ponn type mercury cadmium telluride infrared detector device material preparation. The specific implementation scheme includes a performance test experiment on the relationship between doping concentration and dark current of the n-type layer and the p-type layer of the ponn type mercury cadmium telluride infrared detector, a performance test experiment on the relationship between thickness and dark current of the device transition layer, and determining the selectable range and selection value, so as to optimize the device.
[0075] like Figure 4 As shown in the figure, according to the calculation results, the n-type layer of the conventional table-top ponn HgCdTe detector (calculated with a thickness of 2μm as an example, where the conventional n-type layer is doped with In concentration of 1×10 14 / cm 3 ~1×10 18 / cm 3 The dark current decreases with the increase of doping concentration. The p-type layer of conventional mesa-type ponn HgCdTe detector (calculated with a thickness of 9.7μm as an example, where the conventional p-type layer is doped with Hg vacancies or As at a concentration of 1×10 15 / cm 3 ~1×10 18 / cm 3 The dark current first decreases and then increases with the doping concentration.
[0076] Depend on Figure 4 It can be seen that only for the dark current, the higher the doping concentration of the n-type layer of the device, the smaller the dark current. As the doping concentration of the p-type layer increases, the dark current first decreases and then increases. 16 / cm 3 Considering the influence of dark current, sensitivity, responsiveness and other aspects on the device, the doping concentration, structure thickness and other aspects of the device can be optimized according to actual needs while maintaining an acceptable low dark current of the device.
[0077] The doping concentration range of the n-type layer can be selected within 1×10 15 / cm 3 ~1×10 18 / cm 3 The p-type layer doping concentration range can be selected between 5×10 15 / cm 3 ~5×10 17 / cm 3 The thickness of the transition layer can be selected between 0.1μm and 0.3μm, and according to the trend chart, the doping concentration of each layer of the device and the thickness of the transition layer can be selected according to each specific application scenario.
[0078] It is worth emphasizing that the minority carrier lifetime and doping concentration of the n-type layer of the p on n photodetector have a major influence on the dark current of the device. Figure 6 As shown, the present invention calculates the influence of the In doping concentration of the n-type layer and the minority carrier lifetime on the dark current of the device, and reveals from another perspective that the higher the In doping concentration of the n-type layer, the smaller the dark current of the device.
[0079] The low dark current ponn HgCdTe infrared photodetector material of the present invention is a multi-layered thin film. The present invention is described in detail below using a specific example. Figure 1-Figure 3 As shown, the preparation method is as follows:
[0080] A10, Figure 3 Taking the schematic diagram of the structure of the mercury cadmium telluride infrared photoelectric detector as an example, a corresponding simulation model is established in the simulation software according to the design structure using simulation software;
[0081] A20, for the purpose of regulating and controlling the dark current of the device, adjusts the doping concentration of the p-type layer and n-type layer of the device, the thickness of the transition layer, etc., and obtains a trend diagram of the relationship between the doping concentration, thickness, etc. and the dark current;
[0082] A30, the growth substrate or the composite substrate is the first layer material;
[0083] A40, grow an n-type layer on a substrate or composite substrate, with a thickness of about 9.7 μm and an In doping concentration of 1×10 15 / cm 3 ~1×10 18 / cm 3 , the Cd component value is 0.22;
[0084] A50, a transition layer is grown on the n-type layer, with a thickness of about 0.3 μm and an In doping concentration of 1×10 15 / cm 3 , and the Cd component of the transition layer adopts a Gaussian state slow change, and the Cd component value is between 0.25 and 0.35, forming a barrier layer to effectively reduce the dark current;
[0085] A60, a p-type HgCdTe layer is grown on the transition layer, with a thickness of 1.8 μm to 2.0 μm and a Hg vacancy concentration of 1×10 17 / cm 3 , the Cd component value is 0.25.
[0086] The present invention can optimize the thickness of the structure, doping concentration, etc. of the device while maintaining an acceptable low dark current of the device according to the actual requirements of high performance and low dark current of the device, taking into account the influence of sensitivity, responsiveness, etc. on the device. It has a very important reference significance for improving the high performance of conventional table-top ponn mercury cadmium telluride infrared detector devices while maintaining relatively low dark current of the device.
[0087] It should be noted that, under the conditions of preparation and other device performance conditions, in order to further smooth the energy band, reduce the device dark current, and lower the device capacitance, the table-type and planar ponn mercury cadmium telluride infrared detector devices can be improved as follows:
[0088] (1) Combination Figure 7 As shown, in the transition region from the mesa p-type layer 40 to the transition layer 30 (e.g., within 1 μm), the Cd component can be slowly increased from the p-type layer 40 component to the transition layer 30 peak, and the doping concentration in the transition region is the same as the p-type layer 40 or slightly lower than the p-type layer 40 but higher than the transition layer 30;
[0089] (2) The composition value of the mesa-type transition layer 30 may be in the form of a Gaussian distribution, and the doping concentration is slightly lower than that of the p-type layer 40 and the n-type layer 20;
[0090] (3) A transition drift layer 50 can be appropriately added in the transition zone from the mesa n-type layer 20 to the transition layer 30, with a thickness of 0.5 μm to 2 μm. The composition slowly increases from the composition of the n-type layer 20 to the peak of the transition layer 30, and the doping concentration slowly decreases from the doping concentration of the n-type layer 20 to the transition layer 30. The addition of this layer can smooth the device energy band, reduce the device dark current, reduce the device capacitance, and improve the device performance;
[0091] (4) The side of the mesa-type p-type pixel can maintain a moderate inclination to reduce electric field crowding and dark current;
[0092] (5) If Figure 8 As shown, the planar p-type injection region can maintain a moderate inclination to further reduce electric field crowding and dark current. The present invention realizes the preparation of low dark current devices and has high application value.
[0093] Through the description of the specific implementation methods, a deeper and more specific understanding of the technical means and effects adopted by the present invention to achieve the predetermined purpose should be obtained. However, the accompanying drawings are only for reference and illustration purposes and are not intended to limit the present invention.
Claims
1. A method for preparing a low dark current p on n-type mercury cadmium telluride device, characterized in that: The preparation method is used to prepare a table-type long-wave device, and the preparation method comprises: S10, establish a simulation model of a p on n-type HgCdTe device, calculate and obtain the relationship trends between the p-type layer doping concentration, n-type layer doping concentration, transition layer thickness and dark current from multiple angles through performance test experiments; it is concluded that the higher the n-type layer doping In concentration, the smaller the dark current of the mesa-type long-wave device; as the p-type layer doping concentration increases, the dark current first decreases and then increases, and there is a minimum value; S20, determining a p-type layer doping concentration range, an n-type layer doping concentration range, and a transition layer thickness range of a p on n-type cadmium telluride device to be prepared based on the obtained relationship trends among the p-type layer doping concentration, the n-type layer doping concentration, the transition layer thickness, and the dark current; S30, growing a substrate layer, and sequentially growing an n-type layer, a transition layer, and a p-type layer on the substrate layer; The doping concentration of the n-type layer is in the range of 1×10 15 / cm 3 ~1×10 18 / cm 3 The thickness of the n-type layer is in the range of 9 μm to 10 μm, and the Cd component value is between 0.2 and 0.25; the thickness of the transition layer is in the range of 0.1 μm to 0.3 μm; the concentration of Hg vacancies or As doped in the p-type layer is in the range of 5×10 15 / cm 3 ~5×10 17 / cm 3 The thickness of the p-type layer is in the range of 1.8 μm to 2.0 μm, the Cd component value is between 0.22 and 0.27, and the Cd component value of the p-type layer is 0.02 to 0.05 higher than the Cd component value of the n-type layer.
2. The method for preparing a low dark current pon n-type HgCdTe device according to claim 1, characterized in that: In step S10, simulation software is used to establish a p on n type HgCdTe simulation model, and p-type layer doping concentration and dark current performance test experiments, n-type layer doping concentration and dark current performance test experiments, transition layer thickness and dark current performance test experiments are respectively performed.
3. The method for preparing a low dark current pon n-type HgCdTe device according to claim 2, characterized in that: Step S20 includes: S21, generating a first relationship trend graph between p-type layer doping concentration and dark current from the experimental data obtained from the performance test experiment, and obtaining the p-type layer doping concentration range from the first relationship trend graph; S22, generating a second relationship trend graph between n-type layer doping concentration and dark current from the experimental data obtained from the performance test experiment, and obtaining the n-type layer doping concentration range from the second relationship trend graph; S23, generating a third relationship trend graph between transition layer thickness and dark current from the experimental data obtained from the performance test experiment, and obtaining the thickness range of the transition layer from the third relationship trend graph.
4. The method for preparing a low dark current pon n-type HgCdTe device according to claim 1, characterized in that: The transition layer is doped with In at a concentration of 1×10 15 / cm 3 , and the Cd component of the transition layer adopts a Gaussian state slow change, the Cd component value is between 0.25 and 0.35, and the Cd component value of the transition layer is 0.02 to 0.05 higher than the Cd component value of the p-type layer.
5. A low dark current p on n-type mercury cadmium telluride device, characterized in that: The mercury cadmium telluride device is obtained by using the preparation method of the low dark current ponn-type mercury cadmium telluride device according to any one of claims 1 to 4, and the mercury cadmium telluride device is a mesa-type long-wave device, comprising: substrate layer; An n-type layer is grown on the substrate layer, and the doping concentration of the n-type layer is in the range of 1×10 15 / cm 3 ~1×10 18 / cm 3 , the thickness of the n-type layer ranges from 9 μm to 10 μm, and the Cd component value ranges from 0.2 to 0.25; A transition layer, grown on the n-type layer, wherein the thickness of the transition layer is in the range of 0.1 μm to 0.3 μm; A p-type layer is grown on the transition layer, and the p-type layer is doped with Hg vacancies or As at a concentration of 5×10 15 / cm 3 ~5×10 17 / cm 3 The thickness of the p-type layer is in the range of 1.8 μm to 2.0 μm, the Cd component value is in the range of 0.22 to 0.27, and the Cd component value of the p-type layer is 0.02 to 0.05 higher than the Cd component value of the n-type layer.
6. The low dark current pon n-type HgCdTe device according to claim 5, characterized in that: The transition layer is doped with In at a concentration of 1×10 15 cm 3 , and the Cd component of the transition layer adopts a Gaussian state slow change, the Cd component value is between 0.25 and 0.35, and the Cd component value of the transition layer is 0.02 to 0.05 higher than the Cd component value of the p-type layer.
7. A low dark current p on n-type mercury cadmium telluride infrared detector, characterized in that: include: A pon n type mercury cadmium telluride device, wherein the pon n type mercury cadmium telluride device is prepared by the preparation method of the low dark current pon n type mercury cadmium telluride device according to any one of claims 1 to 4.