All-solid-state bipolar cell structure and preparation system, method and battery thereof

Through the all-solid-state bipolar unit structure and preparation system, the problems of poor complexity and compatibility of the two-electrode structure of all-solid-state batteries are solved, and efficient and safe battery mass production and excellent electrochemical performance are achieved.

CN118335893BActive Publication Date: 2024-12-03SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410569153.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-09
Publication Date
2024-12-03
Estimated Expiration
2044-05-09

AI Technical Summary

Technical Problem

The dual-electrode structure process of all-solid-state batteries is complex, and the compatibility of the positive and negative electrodes of solid electrolytes is poor, which limits its development and application.

Method used

Adopting an all-solid state bipolar unit structure, including a current collector, a positive electrode layer, an anode layer, a first electrolyte layer and a second electrolyte layer, through a specific material composition and layer structure design, combined with the electrode retracting and rolling device and a pressing roller assembly, the The integrated molding and manufacturing of bipolar all-solid-state batteries simplifies the production process.

Benefits of technology

It reduces the short circuit problem of all-solid-state batteries, improves the mass production capacity and safety performance of high-voltage bipolar all-solid-state batteries, improves the energy density, rate performance and cycle life of the battery cell, and simplifies the production process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118335893B_ABST
    Figure CN118335893B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and more specifically, to an all-solid-state bipolar unit structure and its preparation system, method and battery. The all-solid-state bipolar unit structure of the present invention comprises a current collector, a positive electrode layer, a negative electrode layer, a first electrolyte layer and a second electrolyte layer; the positive electrode layer and the negative electrode layer are respectively arranged on both side surfaces of the current collector, and the positive electrode layer and the negative electrode layer form a densest packing structure through particle grading to reduce the internal interface resistance of the electrode; the first electrolyte layer covers the positive electrode layer; and the second electrolyte layer covers the negative electrode layer. The all-solid-state bipolar unit structure of the present invention can reduce the short circuit problem of all-solid-state batteries, is conducive to the mass production of high-voltage bipolar all-solid-state batteries, and has good safety performance and high energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to an all-solid-state bipolar unit structure and a preparation system, method and battery thereof. Background Art

[0002] All-solid-state batteries refer to energy storage devices that do not contain liquid in their structure and all materials exist in solid form. Specifically, they are composed of negative electrode materials, positive electrode materials, and electrolytes. Because the electrolyte of solid-state batteries is solid, the density and structure can allow more charged ions to gather at one end, conduct greater current, and increase the capacity of the battery. Its volume is relatively smaller and easier to seal.

[0003] In the prior art, the process of the dual-electrode structure of all-solid-state batteries is complex, and the poor compatibility of the positive and negative electrodes of solid electrolytes still limits the development and application of all-solid-state batteries.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One object of the present invention is to provide an all-solid-state bipolar unit structure, which can reduce the short-circuit problem of all-solid-state batteries, facilitate the mass production of high-voltage bipolar all-solid-state batteries, and have good safety performance.

[0006] Another object of the present invention is to provide a system for preparing the all-solid-state bipolar unit structure, which is safe and efficient.

[0007] Another object of the present invention is to provide a method for preparing an all-solid-state bipolar unit structure, which can realize the integrated molding and manufacturing of bipolar all-solid-state batteries and simplify the production process of all-solid-state batteries.

[0008] Another object of the present invention is to provide a battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A fully solid-state bipolar unit structure comprises a current collector, a positive electrode layer, a negative electrode layer, a first electrolyte layer and a second electrolyte layer; the positive electrode layer and the negative electrode layer are respectively arranged on both side surfaces of the current collector; the first electrolyte layer covers the positive electrode layer; and the second electrolyte layer covers the negative electrode layer.

[0011] In one embodiment, the positive electrode layer includes a positive electrode active material, wherein the positive electrode active material is composed of a first single crystal positive electrode material and a second single crystal positive electrode material, wherein the D 50 The particle size d1 is 2 to 4 μm, and the D 50The particle size d2=0.414d1, and the distribution widths of the first single crystal positive electrode material and the second single crystal positive electrode material are each independently less than 0.8.

[0012] In one embodiment, the negative electrode layer includes a negative electrode active material, wherein the negative electrode active material is composed of a first single-particle negative electrode material and a second single-particle negative electrode material. 50 The particle size d3 is 8 to 10 μm, and the D 50 The particle size d4=0.414d3, and the particle size distribution widths of the first single-particle negative electrode material and the second single-particle negative electrode material are each independently less than 1.

[0013] In one embodiment, the cathode electrolyte has a D 50 The particle size d5=0.225d1, and the particle size distribution width of the positive electrode electrolyte is less than 1.3.

[0014] In one embodiment, the negative electrode electrolyte has a D 50 The particle size d6=0.225d3, and the particle size distribution width of the negative electrode electrolyte is less than 1.5.

[0015] In one embodiment, the positive electrode layer comprises 80% to 92% of positive electrode active material, 0.5% to 2% of positive electrode conductor, 0.5% to 3% of positive electrode binder and 0.01% to 19% of positive electrode electrolyte in terms of mass percentage; the negative electrode layer comprises 70% to 90% of negative electrode active material, 0.5% to 2% of negative electrode conductor, 0.5% to 3% of negative electrode binder and 0.01% to 28% of negative electrode electrolyte in terms of mass percentage; the first electrolyte layer comprises a first electrolyte and a first binder, and the mass proportion of the positive electrode electrolyte is 95% to 99.5%; the second electrolyte layer comprises a second electrolyte and a second binder, and the mass proportion of the negative electrode electrolyte is 95% to 99.5%.

[0016] In one embodiment, the positive electrode active material includes at least one of a nickel-cobalt-manganese ternary positive electrode material, a nickel-cobalt-manganese-aluminum quaternary positive electrode material, a lithium-rich manganese-based positive electrode material, lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium manganese oxide, and lithium nickel manganese oxide.

[0017] In one embodiment, the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon oxygen, silicon carbon, elemental silicon, elemental tin and metallic lithium.

[0018] In one embodiment, the positive electrode conductive agent and the negative electrode conductive agent each independently include at least one of conductive carbon black, carbon nanotubes, carbon fibers, Ketjen black, and graphene.

[0019] In one embodiment, the cathode electrolyte and the first electrolyte each independently include a halide electrolyte and / or a sulfide electrolyte.

[0020] In one embodiment, the negative electrolyte and the second electrolyte each independently include Li (6-n) PS (5-n) Q (1+n) and at least one of zLi2S·(1-z)P2S5; wherein Q is Cl, Br or I; 0≤n≤0.6; 0.2≤z≤0.8.

[0021] In one embodiment, the thickness of the first electrolyte layer and the second electrolyte layer are independently 7 to 20 μm.

[0022] In one embodiment, the thickness of the positive electrode layer is 80 to 150 μm, and the thickness of the negative electrode layer is 90 to 160 μm.

[0023] In one embodiment, the current collector is selected from steel foil and / or nickel foil, and the thickness of the current collector is 2 to 12 μm.

[0024] The preparation system of the all-solid-state bipolar unit structure as described above comprises an electrode unwinding and winding device, a first calendering transfer roller assembly, a positive electrode feeding device, a first electrolyte feeding device, a second calendering transfer roller assembly, a negative electrode feeding device, and a second electrolyte feeding device; the electrode unwinding and winding device comprises a current collector material supply device and a winding device; the first calendering transfer roller assembly and the second calendering transfer roller assembly are separated on both sides of the current collector surface between the supply device and the winding device, and are arranged oppositely; the first calendering transfer roller assembly and the second calendering transfer roller assembly each independently comprise a plurality of pressing rollers; the positive electrode feeding device is used to provide positive electrode material, and the first electrolyte feeding device is used to provide a first electrolyte; the first calendering transfer roller assembly is used to roll the positive electrode material to obtain a positive electrode The invention relates to a material belt, which is used to roll-combine the first electrolyte with the positive electrode material belt to obtain a composite positive electrode belt having a first electrolyte material belt and a positive electrode material belt; the negative electrode feeding device is used to provide negative electrode materials, and the second electrolyte feeding device is used to provide a second electrolyte; the second calendering transfer roller assembly is used to roll-combine the negative electrode material to obtain a negative electrode material belt, and to roll-combine the second electrolyte with the negative electrode material belt to obtain a composite negative electrode belt having a second electrolyte material belt and a negative electrode material belt; the pressing roller of the first calendering transfer roller assembly close to the current collector material belt cooperates with the pressing roller of the second calendering transfer roller assembly close to the current collector material belt to roll-combine the composite positive electrode belt, the composite negative electrode belt and the current collector material belt to obtain a fully solid-state bipolar unit structure.

[0025] In one embodiment, the first calendering transfer roller assembly includes a first positive electrode roller, a second positive electrode roller, a third positive electrode roller and a fourth positive electrode roller which are arranged in sequence, and the fourth positive electrode roller is close to the current collector strip; the first positive electrode roller and the second positive electrode roller are used to roll the positive electrode material to obtain the positive electrode strip, and the third positive electrode roller and the fourth positive electrode roller are used to roll and composite the first electrolyte and the positive electrode strip to obtain the composite positive electrode strip; the second calendering transfer roller assembly includes a first negative electrode roller, a second negative electrode roller, a third negative electrode roller and a fourth negative electrode roller which are arranged in sequence, and the fourth negative electrode roller is close to the current collector strip; the first negative electrode roller and the second negative electrode roller are used to roll the negative electrode material to obtain the negative electrode strip, and the third negative electrode roller and the fourth negative electrode roller are used to roll and composite the first electrolyte and the negative electrode strip to obtain the composite negative electrode strip.

[0026] In one embodiment, in the direction from the first positive electrode pressing roller to the third positive electrode pressing roller, the temperature of each pressing roller gradually increases, and the rotation speed of each pressing roller gradually increases; the third positive electrode pressing roller and the fourth positive electrode pressing roller have the same temperature and rotation speed.

[0027] In one embodiment, among the first to third positive electrode rollers, the temperature of the rollers is 80-200°C, and the temperature difference between adjacent rollers is 2-20°C, the linear speed of the rollers is 20-50 m / min, and the linear speed ratio of adjacent rollers is 1.05-1.2.

[0028] In one embodiment, in the direction from the first negative electrode pressing roller to the third negative electrode pressing roller, the temperature of each pressing roller gradually increases, and the rotation speed of each pressing roller gradually increases; the third negative electrode pressing roller and the fourth negative electrode pressing roller have the same temperature and rotation speed.

[0029] In one embodiment, among the first to third negative electrode rollers, the temperature of the rollers is 80-200°C, and the temperature difference between adjacent rollers is 2-20°C, the linear speed of the rollers is 20-50 m / min, and the linear speed ratio of adjacent rollers is 1.05-1.2.

[0030] In one embodiment, the preparation system also includes a first trimming structure, a second trimming mechanism, a third trimming structure, and a fourth trimming mechanism; the first trimming structure is used to perform edge trimming on the positive electrode material strip, the second trimming mechanism is used to perform edge trimming on the first electrolyte material strip, the third trimming structure is used to perform edge trimming on the negative electrode material strip, and the fourth trimming mechanism is used to perform edge trimming on the second electrolyte material strip.

[0031] A method for preparing an all-solid-state bipolar unit structure, using the preparation system, comprises the following steps:

[0032] A current collector tape supply device of an electrode winding and unwinding device is used to provide a current collector tape; a first calendering transfer roller assembly is used to roll-press the positive electrode material to obtain a positive electrode tape, a first solid electrolyte and the positive electrode tape are roll-compounded to form a first electrolyte tape on the surface of the positive electrode tape to obtain a composite positive electrode tape; a second calendering transfer roller assembly is used to roll-press the negative electrode material to obtain a negative electrode tape, a second solid electrolyte and the negative electrode tape are roll-compounded to form a second electrolyte tape on the surface of the negative electrode tape to obtain a composite negative electrode tape; a pressure roller in the first calendering transfer roller assembly close to the current collector cooperates with a pressure roller in the second calendering transfer roller assembly close to the current collector to roll-compound the composite positive electrode tape, the current collector tape and the composite negative electrode tape to obtain a fully solid-state bipolar unit structure; a winding device is used to wind up the fully solid-state bipolar unit structure.

[0033] In one embodiment, a first trimming structure is used to trim the edges of the positive electrode material strip, and a second trimming structure is used to trim the edges of the first electrolyte material strip, so that the width of the positive electrode material strip is smaller than the width of the first electrolyte material strip; a third trimming structure is used to trim the edges of the negative electrode material strip, and a fourth trimming structure is used to trim the edges of the second electrolyte material strip, so that the width of the negative electrode material strip is smaller than the width of the second electrolyte material strip.

[0034] In one embodiment, the method further includes: cutting the all-solid-state bipolar unit structure.

[0035] A battery comprises a plurality of stacked all-solid-state bipolar unit structures, wherein the all-solid-state bipolar unit structures are all-solid-state bipolar unit structures prepared by the preparation system or the method.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] (1) The all-solid-state bipolar unit structure of the present invention can reduce the short-circuit problem of all-solid-state batteries, is conducive to the mass production of high-voltage bipolar all-solid-state batteries, and has good safety performance.

[0038] (2) The present invention forms a dense electrode structure by densely stacking particles inside the electrode, thereby reducing the electrode interface impedance and improving the energy density, rate performance and cycle life of the battery cell.

[0039] (3) The preparation system of the all-solid-state bipolar unit structure of the present invention can realize the preparation of the all-solid-state bipolar unit structure through the cooperation of various devices, and has the characteristics of high efficiency and safety, which is conducive to ensuring the quality of the all-solid-state bipolar unit structure and ensuring that it has excellent electrochemical performance.

[0040] (4) The method of the present invention can realize the integrated molding and manufacturing of bipolar all-solid-state batteries, which can greatly simplify the production process of all-solid-state batteries and has the characteristics of high efficiency and safety.

[0041] (5) The battery of the present invention has excellent cycle performance and safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0043] Figure 1 It is a structural schematic diagram of the all-solid-state bipolar unit structure of the present invention;

[0044] Figure 2 Schematic diagram of a system for preparing an all-solid-state bipolar unit structure of the present invention.

[0045] Reference numerals:

[0046] 1-current collector, 2-positive electrode layer, 3-negative electrode layer, 4-first electrolyte layer, 5-second electrolyte layer, 6-current collector tape supply device, 7-winding device, 8-first calendering transfer roller assembly, 801-first positive electrode pressure roller, 802-second positive electrode pressure roller, 803-third positive electrode pressure roller, 804-fourth positive electrode pressure roller, 9-second calendering transfer roller assembly, 901-first negative electrode pressure roller, 902-second negative electrode pressure roller, 903-third negative electrode pressure roller, 904-fourth negative electrode pressure roller, 10-positive electrode feeding device, 11-first electrolyte feeding device, 12-negative electrode feeding device, 13-second electrolyte feeding device. DETAILED DESCRIPTION

[0047] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0048] According to one aspect of the present invention, the present invention relates to an all-solid-state bipolar unit structure, comprising a current collector, a positive electrode layer, a negative electrode layer, a first electrolyte layer and a second electrolyte layer; the positive electrode layer and the negative electrode layer are respectively arranged on both side surfaces of the current collector; the first electrolyte layer covers the positive electrode layer; and the second electrolyte layer covers the negative electrode layer.

[0049] The all-solid-state bipolar unit structure of the present invention can reduce the short-circuit problem of the all-solid-state battery, is conducive to the mass production of high-voltage bipolar all-solid-state batteries, and has good safety performance.

[0050] In one embodiment, the positive electrode layer includes a positive electrode active material, wherein the positive electrode active material is composed of a first single crystal positive electrode material and a second single crystal positive electrode material, wherein the D 50 The particle size d1 is 2 to 4 μm, for example, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, 3.3 μm, 3.5 μm or 4 μm; the particle size D1 of the second single crystal positive electrode material is 2 to 4 μm, for example, 2 μm, 2.2 μm, 2.5 μm, 2.8 μm, 3 μm, 3.3 μm, 3.5 μm or 4 μm; 50 The particle size d2=0.414d1; the distribution widths of the first single crystal positive electrode material and the second single crystal positive electrode material are each independently less than 0.8, such as 0.2, 0.3, 0.4, 0.5, 0.7, 0.75, etc. The positive electrode active material of the present invention is more conducive to ensuring the electrochemical performance of the positive electrode through the combination of the first single crystal positive electrode material and the second single crystal positive electrode material.

[0051] In one embodiment, the negative electrode layer includes a negative electrode active material, wherein the negative electrode active material is composed of a first single-particle negative electrode material and a second single-particle negative electrode material. 50 The particle size d3 is 8 to 10 μm, for example, 8 μm, 8.2 μm, 8.5 μm, 8.8 μm, 9 μm, 9.2 μm, 9.5 μm, 10 μm, etc. The D 50 The particle size d4=0.414d3, the particle size distribution widths of the first single-particle negative electrode material and the second single-particle negative electrode material are each independently less than 1, such as 0.2, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, etc. The negative electrode active material of the present invention is more conducive to ensuring the electrochemical performance of the negative electrode through the combination of the first single-particle negative electrode material and the second single-particle negative electrode material.

[0052] In one embodiment, the cathode electrolyte has a D 50 The particle size d5=0.225d1, the particle size distribution width of the positive electrolyte is less than 1.3, for example, 0.2, 0.5, 0.7, 0.8, 0.9, 1.1, 1.2, etc. The particle size distribution width of the positive electrolyte of the present invention is less than 1.3, for example, 0.2, 0.5, 0.7, 0.8, 0.9, 1.1, 1.2, etc. 50 Particle size and D of a single crystal cathode material 50 The particle size d1 satisfies the above relationship, which is more conducive to the coordinated cooperation of the components of the positive electrode to improve the comprehensive performance of the positive electrode layer.

[0053] In one embodiment, the negative electrode electrolyte has a D 50The particle size d6=0.225d3, the particle size distribution width of the negative electrode electrolyte is less than 1.5, for example, 0.2, 0.4, 0.5, 0.7, 0.9, 1, 1.1, 1.2, 1.4, etc. The particle size distribution width of the negative electrode electrolyte is less than 1.5, for example, 0.2, 0.4, 0.5, 0.7, 0.9, 1, 1.1, 1.2, 1.4, etc. 50 The particle size d6 and the D 50 The particle size d3 satisfies the above relationship, which is more conducive to the coordination of the negative electrode components to improve the comprehensive performance of the negative electrode layer.

[0054] In one embodiment, the positive electrode layer comprises 80% to 92% of positive electrode active material, 0.5% to 2% of positive electrode conductor, 0.5% to 3% of positive electrode binder and 0.01% to 19% of positive electrode electrolyte in terms of mass percentage; the negative electrode layer comprises 70% to 90% of negative electrode active material, 0.5% to 2% of negative electrode conductor, 0.5% to 3% of negative electrode binder and 0.01% to 28% of negative electrode electrolyte in terms of mass percentage; the first electrolyte layer comprises a first electrolyte and a first binder, and the mass proportion of the positive electrode electrolyte is 95% to 99.5%; the second electrolyte layer comprises a second electrolyte and a second binder, and the mass proportion of the negative electrode electrolyte is 95% to 99.5%.

[0055] In one embodiment, in terms of mass percentage, the positive electrode active material is 80%, 85%, 90% or 92%, etc.; the positive electrode conductive agent is 0.5%, 0.8%, 1%, 1.5%, or 2%, etc.; the positive electrode binder is 0.5%, 0.8%, 1%, 1.5%, 2% or 3%, etc.; the positive electrode electrolyte is 0.01%, 1%, 5%, 8%, 10%, 12%, 15% or 19%, etc. The positive electrode active material includes at least one of a nickel-cobalt-manganese ternary positive electrode material, a nickel-cobalt-manganese-aluminum quaternary positive electrode material, a lithium-rich manganese-based positive electrode material, lithium iron phosphate, lithium manganese phosphate, lithium manganese oxide, and lithium nickel manganese oxide. The present invention is suitable for the combination of positive electrode layer materials in a certain amount ratio to ensure the electrochemical performance of the battery. In one embodiment, the thickness of the positive electrode layer is 80 to 150 μm.

[0056] In one embodiment, in terms of mass percentage, the negative electrode active material is 70%, 75%, 80%, 85% or 90%, etc.; the negative electrode conductive agent is 0.5%, 0.8%, 1%, 1.2%, 1.5% or 2%, etc.; the negative electrode binder is 0.5%, 0.8%, 1%, 1.2%, 1.5%, 2%, 2.5% or 3%, etc.; the negative electrode electrolyte is 0.01%, 0.5%, 1%, 5%, 8%, 10%, 12%, 15%, 20%, 28%, etc.; the negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon oxygen, silicon carbon, elemental silicon, elemental tin and metallic lithium. The combination of the negative electrode layer materials in the appropriate dosage ratio of the present invention is conducive to ensuring the electrochemical performance of the battery. In one embodiment, the thickness of the negative electrode layer is 90 to 160 μm.

[0057] In one embodiment, the mass percentage of the positive electrode electrolyte is 95%, 96%, 97%, 99.5%, etc.

[0058] In one embodiment, the mass percentage of the negative electrode electrolyte is 95%, 96%, 97%, 98% or 99.5%, etc.

[0059] In one embodiment, the positive electrode binder, the negative electrode binder, the first binder and the second binder each independently include at least one of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), polyacrylic acid (PAA) and polyethylene (PE).

[0060] In one embodiment, the positive electrode conductive agent and the negative electrode conductive agent each independently include at least one of conductive carbon black (SP), carbon nanotubes (CNT), carbon fibers (VGCF), Ketjen black (ECP), and graphene.

[0061] In one embodiment, the cathode electrolyte and the first electrolyte are each independently selected from Li x MB6, Li (6-m) PS (5-m) X (1+m) and yLi2S·(1-y)P2S5, Li 10 GeP2S 12 and one or more combinations of element-doped materials with the same structure; wherein M is at least one of Y, Zr, In, Sc, Ta and La, and B is selected from at least one of Cl, Br and I; X is Cl, Br or I, 0≤m≤0.6; 0.2≤y≤0.8.

[0062] In one embodiment, the negative electrolyte and the second electrolyte each independently include Li(6-n) PS (5-n) Q (1+n) and at least one of zLi2S·(1-z)P2S5; wherein Q is Cl, Br or I; 0≤n≤0.6; 0.2≤z≤0.8.

[0063] In one embodiment, the thickness of the first electrolyte layer and the second electrolyte layer are independently 7 to 20 μm, for example, 7 μm, 10 μm, 15 μm, 20 μm, etc.

[0064] In one embodiment, the first electrolyte and the positive electrode electrolyte are made of the same material; the second electrolyte and the negative electrode electrolyte are made of the same material.

[0065] In one embodiment, when the first binder and the second binder are of multiple types, the first binder and the second binder independently include: at least one of PVDF, PAN, PMMA, PAA and PE, and PTFE.

[0066] In one embodiment, the current collector is selected from steel foil and / or nickel foil, and the thickness of the current collector is 2 to 12 μm, such as 2 μm, 5 μm, 10 μm, 12 μm, etc.

[0067] According to another aspect of the present invention, the present invention also relates to a preparation system for the all-solid-state bipolar unit structure, comprising an electrode unwinding and winding device, a first calendering transfer roller assembly, a positive electrode feeding device, a first electrolyte feeding device, a second calendering transfer roller assembly, a negative electrode feeding device, and a second electrolyte feeding device. The electrode unwinding and winding device comprises a current collector supply device and a winding device, wherein the current collector supply device is used to provide the current collector, and the winding device is used to wind up the all-solid-state bipolar unit structure. The first calendering transfer roller assembly and the second calendering transfer roller assembly are separated on both sides of the current collector surface between the supply device and the winding device, and are arranged oppositely; the first calendering transfer roller assembly and the second calendering transfer roller assembly each independently include a plurality of pressing rollers; the positive electrode feeding device is used to provide positive electrode material, and the first electrolyte feeding device is used to provide a first electrolyte; the first calendering transfer roller assembly is used to roll the positive electrode material to obtain a positive electrode material strip, and to roll and composite the first electrolyte with the positive electrode material strip to obtain a composite positive electrode strip having a first electrolyte material strip and a positive electrode material strip; the negative electrode feeding device is used to roll and composite the first electrolyte with the positive electrode material strip to obtain a composite positive electrode strip having a first electrolyte material strip and a positive electrode material strip; The first feeding device is used to provide negative electrode material, and the second electrolyte feeding device is used to provide a second electrolyte; the second calendering transfer roller assembly is used to roll the negative electrode material to obtain a negative electrode material strip, and is used to roll-compound the second electrolyte and the negative electrode material strip to obtain a composite negative electrode strip having a second electrolyte material strip and a negative electrode material strip; the pressing roller close to the current collector material strip in the first calendering transfer roller assembly cooperates with the pressing roller close to the current collector material strip in the second calendering transfer roller assembly to roll-compound the composite positive electrode strip, the composite negative electrode strip and the current collector material strip to obtain a fully solid-state bipolar unit structure.

[0068] The preparation system of the all-solid-state bipolar unit structure of the present invention can realize the preparation of the all-solid-state bipolar unit structure through the cooperation of various devices, has the characteristics of high efficiency and safety, is conducive to ensuring the quality of the all-solid-state bipolar unit structure, and ensures that it has excellent electrochemical performance.

[0069] In one embodiment, the first calendering transfer roller assembly includes a first positive electrode roller, a second positive electrode roller, a third positive electrode roller and a fourth positive electrode roller which are arranged in sequence, and the fourth positive electrode roller is close to the current collector strip; the first positive electrode roller and the second positive electrode roller are used to roll the positive electrode material to obtain the positive electrode strip, and the third positive electrode roller and the fourth positive electrode roller are used to roll and composite the first electrolyte and the positive electrode strip to obtain the composite positive electrode strip; the second calendering transfer roller assembly includes a first negative electrode roller, a second negative electrode roller, a third negative electrode roller and a fourth negative electrode roller which are arranged in sequence, and the fourth negative electrode roller is close to the current collector strip; the first negative electrode roller and the second negative electrode roller are used to roll the negative electrode material to obtain the negative electrode strip, and the third negative electrode roller and the fourth negative electrode roller are used to roll and composite the first electrolyte and the negative electrode strip to obtain the composite negative electrode strip.

[0070] In one embodiment, in the first calendering transfer roller assembly, in the direction from the first positive electrode roller to the third positive electrode roller, the temperature of each roller gradually increases, and the rotation speed of each roller gradually increases; the third positive electrode roller and the fourth positive electrode roller have the same temperature and rotation speed. In one embodiment, the temperature of the rollers from the first positive electrode roller to the third positive electrode roller is 80 to 200°C, such as 80°C, 100°C, 120°C, 150°C, 180°C or 200°C, etc.; and the temperature difference between adjacent rollers is 2 to 20°C, such as 2°C, 5°C, 10°C, 20°C, etc.; the linear speed of the roller is 20 to 50m / min, such as 20m / min, 30m / min, 40m / min or 50m / min, etc., and the linear speed ratio of adjacent rollers is 1.05 to 1.2, such as 1.05, 1.1, 1.12, 1.15, 1.18 or 1.2, etc. Each roller in the first calender transfer roller assembly adopts appropriate temperature and rotation speed to meet appropriate temperature relationship and rotation speed relationship, thereby ensuring the density and stability of the first electrolyte layer.

[0071] In one embodiment, in the direction from the first negative electrode roller to the third negative electrode roller, the temperature of each roller gradually increases, and the rotation speed of each roller gradually increases; the third negative electrode roller and the fourth negative electrode roller have the same temperature and rotation speed. In one embodiment, the temperature of the rollers from the first negative electrode roller to the third negative electrode roller is 80 to 200°C, such as 80°C, 100°C, 120°C, 150°C, 180°C or 200°C, etc.; and the temperature difference between adjacent rollers is 2 to 20°C, such as 2°C, 5°C, 10°C, 15°C or 20°C, etc. The linear speed of the roller is 20 to 50 m / min, such as 20 m / min, 30 m / min, 40 m / min, 50 m / min, etc.; and the linear speed ratio of adjacent rollers is 1.05 to 1.2, such as 1.05, 1.06, 1.1, 1.12, 1.15, 1.18, 1.2, etc. Each roller in the second calender transfer roller assembly adopts appropriate temperature and rotation speed to meet appropriate temperature relationship and rotation speed relationship, thereby ensuring the density and stability of the second electrolyte layer.

[0072] In one embodiment, the number, radius, temperature, and linear speed of the calendering transfer rollers in the first calendering transfer roller assembly and the second calendering transfer roller assembly may be the same or different, but the linear speed of the transfer rollers close to both sides of the collector strip must remain the same.

[0073] In one embodiment, the preparation system further includes a first trimming structure, a second trimming mechanism, a third trimming structure, and a fourth trimming mechanism; the first trimming structure is located at the third positive electrode pressing roller, and the second trimming mechanism is located at the fourth positive electrode pressing roller; the third trimming structure is located at the third negative electrode pressing roller, and the fourth trimming mechanism is located at the fourth negative electrode pressing roller. The first trimming structure is used to trim the edges of the positive electrode material strip, the second trimming mechanism is used to trim the edges of the first electrolyte material strip, the third trimming structure is used to trim the edges of the negative electrode material strip, and the fourth trimming mechanism is used to trim the edges of the second electrolyte material strip.

[0074] According to another aspect of the present invention, the present invention also relates to a method for preparing an all-solid-state bipolar unit structure, using the preparation system, comprising the following steps:

[0075] A current collector tape supply device of an electrode winding and unwinding device is used to provide a current collector tape; a first calendering transfer roller assembly is used to roll-press the positive electrode material to obtain a positive electrode tape, a first solid electrolyte and the positive electrode tape are roll-compounded to form a first electrolyte tape on the surface of the positive electrode tape to obtain a composite positive electrode tape; a second calendering transfer roller assembly is used to roll-press the negative electrode material to obtain a negative electrode tape, a second solid electrolyte and the negative electrode tape are roll-compounded to form a second electrolyte tape on the surface of the negative electrode tape to obtain a composite negative electrode tape; a pressure roller in the first calendering transfer roller assembly close to the current collector cooperates with a pressure roller in the second calendering transfer roller assembly close to the current collector to roll-compound the composite positive electrode tape, the current collector tape and the composite negative electrode tape to obtain a fully solid-state bipolar unit structure; a winding device is used to wind up the fully solid-state bipolar unit structure.

[0076] The method of the present invention can realize the integrated molding and manufacturing of bipolar all-solid-state batteries, can greatly simplify the production process of all-solid-state batteries, and has the characteristics of high efficiency and safety.

[0077] In one embodiment, the first trimming structure is used to trim the edge of the positive electrode material strip, and the second trimming mechanism is used to trim the edge of the first electrolyte material strip, so that the width of the positive electrode material strip is smaller than the width of the first electrolyte material strip. The third trimming structure is used to trim the edge of the negative electrode material strip, and the fourth trimming mechanism is used to trim the edge of the second electrolyte material strip, so that the width of the negative electrode material strip is smaller than the width of the second electrolyte material strip.

[0078] Furthermore, the bipolar all-solid-state battery is die-cut to the designed size, stacked and soft-packed, and then isostatically pressed to complete the preparation of the all-solid-state battery.

[0079] According to another aspect of the present invention, the present invention also relates to a battery comprising a plurality of all-solid-state bipolar unit structures.

[0080] The battery of the present invention has excellent cycle performance and safety performance.

[0081] The following is further explained in conjunction with specific embodiments.

[0082] Example 1

[0083] The preparation device of the all-solid-state bipolar unit structure, such as Figure 2 As shown, it includes an electrode winding and unwinding device, a first calendering transfer roller assembly 8, a positive electrode feeding device 10, a first electrolyte feeding device 11, a second calendering transfer roller assembly 9, a negative electrode feeding device 12, and a second electrolyte feeding device 13.

[0084] The electrode winding and unwinding device includes a current collector tape supply device 6 and a winding device 7 .

[0085] The positive electrode feeding device 10 is used to provide positive electrode materials, the first electrolyte feeding device 11 is used to provide a first electrolyte, the negative electrode feeding device 12 is used to provide negative electrode materials, and the second electrolyte feeding device 13 is used to provide a second electrolyte.

[0086] The first calendering transfer roller assembly 8 and the second calendering transfer roller assembly 9 are located on both sides of the current collector surface between the supply device and the winding device 7 and are arranged opposite to each other.

[0087] The first calendering transfer roller assembly 8 includes a first positive electrode roller 801, a second positive electrode roller 802, a third positive electrode roller 803 and a fourth positive electrode roller 804 which are arranged in sequence, and the fourth positive electrode roller 804 is close to the current collector strip; the first positive electrode roller 801 and the second positive electrode roller 802 are used to roll the positive electrode material to obtain the positive electrode strip, and the third positive electrode roller 803 and the fourth positive electrode roller 804 are used to roll and composite the first electrolyte and the positive electrode strip to obtain a composite positive electrode strip having the first electrolyte strip and the positive electrode strip.

[0088] The second calendering transfer roller assembly 9 includes a first negative electrode pressing roller 901, a second negative electrode pressing roller 902, a third negative electrode pressing roller 903 and a fourth negative electrode pressing roller 904 which are arranged in sequence, and the fourth negative electrode pressing roller 904 is close to the current collector strip; the first negative electrode pressing roller 901 and the second negative electrode pressing roller 902 are used to roll the negative electrode material to obtain the negative electrode strip, and the third negative electrode pressing roller 903 and the fourth negative electrode pressing roller 904 are used to roll and composite the first electrolyte and the negative electrode strip to obtain a composite negative electrode strip having a second electrolyte strip and a negative electrode strip.

[0089] The fourth positive electrode pressing roller 804 cooperates with the fourth negative electrode pressing roller 904 to roll-combine the composite positive electrode strip, the composite negative electrode strip and the current collector strip to obtain a fully solid bipolar unit structure.

[0090] The preparation system also includes a first trimming structure, a second trimming mechanism, a third trimming structure, and a fourth trimming mechanism; the first trimming structure is used to trim the edges of the positive electrode material strip, the second trimming mechanism is used to trim the edges of the first electrolyte material strip, the third trimming structure is used to trim the edges of the negative electrode material strip, and the fourth trimming mechanism is used to trim the edges of the second electrolyte material strip.

[0091] Example 2

[0092] An all-solid-state bipolar cell structure, such as Figure 1As shown, it includes a current collector 1, a positive electrode layer 2, a negative electrode layer 3, a first electrolyte layer 4 and a second electrolyte layer 5; the positive electrode layer 2 and the negative electrode layer 3 are respectively arranged on both side surfaces of the current collector 1; the first electrolyte layer 4 covers the positive electrode layer 2; and the second electrolyte layer 5 covers the negative electrode layer 3.

[0093] The positive electrode layer 2 includes positive electrode active material NCM811, positive electrode conductive agent SP and CNT, positive electrode electrolyte Li3YCl6 and positive electrode binder PTFE; in terms of mass percentage, the positive electrode active material is 88.5%, SP is 1%, CNT is 0.5%, the positive electrode binder is 2%, and the positive electrode electrolyte is 8%; the thickness of the positive electrode layer 2 is 100 μm. The negative electrode layer 3 includes negative electrode active material Gr, negative electrode conductive agent SP, negative electrode electrolyte Li3PS4 and negative electrode binder PTFE; in terms of mass percentage, the negative electrode active material is 83%, the negative electrode conductive agent is 1%, the negative electrode binder is 1%, the negative electrode electrolyte is 15%, and the thickness of the negative electrode layer 3 is 110 μm.

[0094] The positive electrode active material is composed of a first single crystal positive electrode material and a second single crystal positive electrode material. 50 The particle size d1 is 3 μm, the distribution width is 0.6, and the D 50 The particle size d2 is 1.242 μm, and the distribution width is 0.75; the negative electrode active material is composed of a first single particle negative electrode material and a second single particle negative electrode material, and the D 50 The particle size d3 is 9 μm, the distribution width is 0.8, and the D 50 The particle size d4 is 3.726 μm, and the distribution width is 0.92; the D 50 The particle size d5 is 0.675 μm and the distribution width is 1.2; the D 50 The particle size d6 is 2.025 μm and the distribution width is 1.3.

[0095] The first electrolyte layer 4 includes Li3YCl6 and PTFE, the mass ratio of Li3YCl6 and PTFE is 99:1, and the thickness is 10 μm. The second electrolyte layer 5 includes Li3PS4 and PTFE, the mass ratio is 99:1, and the thickness is 10 μm. The current collector 1 is selected from steel foil, and the thickness of the current collector 1 is 6 μm.

[0096] The method for preparing the all-solid-state bipolar unit structure in this embodiment adopts the system of embodiment 1, and comprises the following steps:

[0097] The current collector tape supply device 6 of the electrode winding and unwinding device provides the current collector tape.

[0098] A composite positive electrode tape is prepared by using a first calendering transfer roller assembly 8: a positive electrode feeding device 10 provides positive electrode material, which is a mixture of positive electrode active material NCM811, positive electrode conductive agent SP and CNT, positive electrode electrolyte Li3YCl6 and positive electrode binder PTFE and then fiberized; a positive electrode tape is obtained by rolling the first positive electrode pressing roller 801 and the second positive electrode pressing roller 802; the positive electrode tape is passed between a third positive electrode pressing roller 803 and a fourth positive electrode pressing roller 804, and at the same time, the first electrolyte feeding device 11 provides a first electrolyte, which is distributed on the surface and roller surface of the positive electrode tape, and the third positive electrode pressing roller 803 and the fourth positive electrode pressing roller 804 perform rolling composite treatment on the first electrolyte and the positive electrode tape to obtain a composite positive electrode tape having a positive electrode tape and a first electrolyte tape.

[0099] In the above process, the first trimming structure is used to trim the edge of the positive electrode material strip, and the second trimming structure is used to trim the edge of the first electrolyte material strip, so that the width of the positive electrode material strip is smaller than the width of the first electrolyte material strip.

[0100] The temperatures of the first positive electrode pressing roller 801, the second positive electrode pressing roller 802, the third positive electrode pressing roller 803 and the fourth positive electrode pressing roller 804 are 140°C, 150°C, 160°C, 160°C respectively, the line speeds are 10m / min, 11m / min, 12m / min, 12m / min respectively, and the pressure is 2t.

[0101] At the same time, a second calendering transfer roller assembly 9 is used to prepare a composite negative electrode belt: the negative electrode feeding device 12 provides negative electrode materials, and the negative electrode materials are fiberized after mixing negative electrode active material Gr, negative electrode conductive agent SP, negative electrode electrolyte Li3PS4 and negative electrode binder PTFE; the first negative electrode pressing roller 901 and the second negative electrode pressing roller 902 perform rolling processing on the negative electrode materials to obtain a negative electrode belt; the negative electrode belt enters between the third negative electrode pressing roller 903 and the fourth negative electrode pressing roller 904, and at the same time, the second electrolyte feeding device 13 provides the second electrolyte, so that the second electrolyte is distributed on the surface of the negative electrode belt and the roller surface, and the third negative electrode pressing roller 903 and the fourth negative electrode pressing roller 904 cooperate to perform rolling composite processing on the second electrolyte and the negative electrode belt to obtain a composite negative electrode belt having a negative electrode belt and a second electrolyte belt.

[0102] The third trimming structure is used to trim the edge of the negative electrode material strip, and the fourth trimming structure is used to trim the edge of the second electrolyte material strip, so that the width of the negative electrode material strip is smaller than the width of the second electrolyte material strip.

[0103] The temperatures of the first negative electrode pressing roller 901, the second negative electrode pressing roller 902, the third negative electrode pressing roller 903 and the fourth negative electrode pressing roller 904 are 120°C, 125°C, 130°C, 130°C respectively, the line speeds are 10m / min, 11m / min, 12m / min, 12m / min respectively, and the pressure is 2t.

[0104] Through the cooperation of the fourth positive electrode pressing roller 804 and the fourth negative electrode pressing roller 904, the composite positive electrode strip, the current collector strip and the composite negative electrode strip are rolled and composited to obtain a full solid bipolar unit structure.

[0105] The winding device 7 performs a winding process on the prepared all-solid-state bipolar unit structure.

[0106] A method for preparing a battery comprises: cutting the above-mentioned all-solid-state bipolar unit structure, laminating, packaging, isobaric pressing and molding to obtain an all-solid-state battery.

[0107] Example 3

[0108] A method for preparing an all-solid-state bipolar unit structure, wherein the temperatures of the first positive electrode roller 801, the second positive electrode roller 802, the third positive electrode roller 803 and the fourth positive electrode roller 804 are 80°C, 100°C, 120°C, 120°C, respectively, and the line speeds are 20m / min, 22m / min, 26m / min, 26m / min, respectively; the temperatures of the first negative electrode roller 901, the second negative electrode roller 902, the third negative electrode roller 903 and the fourth negative electrode roller 904 are 90°C, 100°C, 120°C, 120°C, respectively, and the line speeds are 20m / min, 22m / min, 26m / min, 26m / min, respectively. Other conditions are the same as in Example 2.

[0109] Example 4

[0110] A method for preparing an all-solid-state bipolar unit structure, wherein the temperatures of the first positive electrode roller 801, the second positive electrode roller 802, the third positive electrode roller 803 and the fourth positive electrode roller 804 are 150°C, 160°C, 170°C, 170°C, respectively, and the line speeds are 40m / min, 44m / min, 48.5m / min, 48.5m / min, respectively; the temperatures of the first negative electrode roller 901, the second negative electrode roller 902, the third negative electrode roller 903 and the fourth negative electrode roller 904 are 160°C, 180°C, 200°C, 200°C, respectively, and the line speeds are 40m / min, 44m / min, 48.5m / min, 48.5m / min, respectively, and the other conditions are the same as in Example 2.

[0111] Example 5

[0112] A fully solid-state bipolar unit structure, in which, by mass percentage, the positive electrode active material is 92%, SP is 0.5%, CNT is 0.5%, the positive electrode binder is 1%, and the positive electrode electrolyte is 6%; by mass percentage, the thickness is 100 μm, the negative electrode artificial graphite accounts for 70%, the elemental silicon accounts for 20%, the negative electrode conductive agent is 2%, the negative electrode binder is 0.5%, the negative electrode electrolyte is 7.5%, the thickness is 92 μm, the first single-particle negative electrode material is artificial graphite, the second single-particle negative electrode material is elemental silicon, and other conditions are the same as in Example 2.

[0113] Example 6

[0114] A fully solid-state bipolar unit structure, except that the thickness of the positive electrode layer 2 is 90 μm; the thickness of the negative electrode layer 3 is 100 μm; the thickness of the first electrolyte layer 4 is 8 μm; the thickness of the second electrolyte layer 5 is 8 μm; the thickness of the current collector 1 is 10 μm, and other conditions are the same as those in Example 2.

[0115] Example 7

[0116] A fully solid-state bipolar unit structure, except that the thickness of the positive electrode layer 2 is 90 μm; the thickness of the negative electrode layer 3 is 100 μm; the thickness of the first electrolyte layer 4 is 20 μm; the thickness of the second electrolyte layer 5 is 20 μm; the thickness of the current collector 1 is 8 μm, and other conditions are the same as those in Example 2.

[0117] Example 8

[0118] An all-solid-state bipolar unit structure, which is different from Example 2 in that:

[0119] The first single crystal cathode material D 50 The particle size d1 is 4 μm, the distribution width is 0.56, and the D 50 The particle size d2 is 1.656 μm and the distribution width is 0.74; the D 50 The particle size d3 is 10 μm, the distribution width is 0.66, and the D 50 The particle size d4 is 4.14 μm, and the distribution width is 0.84; the D 50 The particle size d5 is 0.9 μm and the distribution width is 1.1; the D 50 The particle size d6 is 2.25 μm and the distribution width is 1.3.

[0120] Comparative Example 1

[0121] The electrolyte layer only has the first electrolyte layer, which has a thickness of 20 μm, and the rest is consistent with Example 2.

[0122] Comparative Example 2

[0123] The electrolyte layer only has the second electrolyte layer, which has a thickness of 20 μm, and the rest is consistent with Example 2.

[0124] Comparative Example 3

[0125] The positive electrode active material only includes the first single crystal positive electrode material, the negative electrode active material only includes the first single particle negative electrode material, and other conditions are the same as those in Example 2.

[0126] Test plan

[0127] The electrochemical performance of the batteries prepared with the all-solid-state bipolar unit structures of the embodiments of the present invention and the comparative examples was tested.

[0128] 1C capacity retention rate: After fully charged at 0.1C, discharge at 1C and 0.1C respectively. The 1C discharge capacity is divided by the 0.1C discharge capacity.

[0129] Cycle life: 0.5C charge and discharge cycle test, until the capacity retention rate reaches 80% of the cycle number.

[0130] The electrochemical performance test results of each battery are shown in Table 1.

[0131] Table 1 Electrochemical performance test results of each battery

[0132] Group 1C capacity retention rate (%) Cycle life (times) Example 2 85.6 1387 Example 3 83.1 1263 Example 4 85.7 1192 Example 5 87.3 1078 Example 6 86.9 1249 Example 7 86.7 1421 Example 8 83.4 1292 Comparative Example 1 79.2 935 Comparative Example 2 81.3 1023 Comparative Example 3 80.4 1163

[0133] As can be seen from Table 1, the batteries obtained by the methods of the embodiments of the present invention have excellent capacity retention and cycle life, with a 1C capacity retention of 83.1% or more and a cycle life of 1078 times or more. The capacity retention and cycle life of the batteries obtained in Comparative Examples 1, 2 and 3 are all poor.

[0134] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A system for preparing an all-solid-state bipolar unit structure, It is characterized in that It includes an electrode winding and unwinding device, a first calendering transfer roller assembly, a positive electrode feeding device, a first electrolyte feeding device, a second calendering transfer roller assembly, a negative electrode feeding device, and a second electrolyte feeding device; The electrode winding and unwinding device comprises a current collector strip supply device and a winding device; The first calender transfer roller assembly and the second calender transfer roller assembly are located on both sides of the current collector surface between the supply device and the winding device, and are arranged opposite to each other; the first calender transfer roller assembly and the second calender transfer roller assembly each independently include a plurality of pressing rollers; The positive electrode feeding device is used to provide positive electrode material, and the first electrolyte feeding device is used to provide a first electrolyte; the first calendering transfer roller assembly is used to roll the positive electrode material to obtain a positive electrode material strip, and to roll and composite the first electrolyte with the positive electrode material strip to obtain a composite positive electrode strip having a first electrolyte material strip and a positive electrode material strip; The negative electrode feeding device is used to provide negative electrode material, and the second electrolyte feeding device is used to provide a second electrolyte; the second calendering transfer roller assembly is used to roll the negative electrode material to obtain a negative electrode material belt, and to roll and composite the second electrolyte and the negative electrode material belt to obtain a composite negative electrode belt having a second electrolyte material belt and a negative electrode material belt; The pressing roller of the first calendering transfer roller assembly close to the current collector material belt cooperates with the pressing roller of the second calendering transfer roller assembly close to the current collector material belt to roll-press and composite the composite positive electrode belt, the composite negative electrode belt and the current collector material belt to obtain an all-solid-state bipolar unit structure; the all-solid-state bipolar unit structure includes a current collector, a positive electrode layer, a negative electrode layer, a first electrolyte layer and a second electrolyte layer; the positive electrode layer and the negative electrode layer are respectively arranged on both side surfaces of the current collector; the first electrolyte layer completely covers the positive electrode layer; the second electrolyte layer completely covers the negative electrode layer; The preparation system further includes a first trimming structure, a second trimming mechanism, a third trimming structure, and a fourth trimming mechanism; the first trimming structure is used to trim the edge of the positive electrode material strip, the second trimming mechanism is used to trim the edge of the first electrolyte material strip, the third trimming structure is used to trim the edge of the negative electrode material strip, and the fourth trimming mechanism is used to trim the edge of the second electrolyte material strip; The first trimming structure is used to trim the edge of the positive electrode material strip, and the second trimming mechanism is used to trim the edge of the first electrolyte material strip, so that the width of the positive electrode material strip is smaller than the width of the first electrolyte material strip; the third trimming structure is used to trim the edge of the negative electrode material strip, and the fourth trimming mechanism is used to trim the edge of the second electrolyte material strip, so that the width of the negative electrode material strip is smaller than the width of the second electrolyte material strip.

2. The system for preparing the all-solid-state bipolar unit structure according to claim 1, It is characterized in that Contains at least one of the following features (1) to (2): (1) The positive electrode layer includes a positive electrode active material, wherein the positive electrode active material is composed of a first single crystal positive electrode material and a second single crystal positive electrode material, wherein the D 50 Particle size 1 The D of the second single crystal positive electrode material is 2-4 μm. 50 Particle size 2 =0.414 d 1 ; (2) The negative electrode layer includes a negative electrode active material, wherein the negative electrode active material is composed of a first single-particle negative electrode material and a second single-particle negative electrode material, wherein the D 50 Particle size 3 The D of the second single-particle negative electrode material is 8-10 μm. 50 Particle size 4 =0.414d 3 .

3. The system for preparing the all-solid-state bipolar unit structure according to claim 2, It is characterized in that In terms of mass percentage, the positive electrode layer comprises 80% to 92% of positive electrode active material, 0.5% to 2% of positive electrode conductive agent, 0.5% to 3% of positive electrode binder and 0.01% to 19% of positive electrode electrolyte; the D 50 Particle size 5 =0.225d 1 ; In terms of mass percentage, the negative electrode layer comprises 70% to 90% of negative electrode active material, 0.5% to 2% of negative electrode conductive agent, 0.5% to 3% of negative electrode binder and 0.01% to 28% of negative electrode electrolyte; the negative electrode electrolyte has a D 50 Particle size 6 =0.225d 3 ; The first electrolyte layer comprises a first electrolyte and a first binder, and the mass proportion of the positive electrode electrolyte is 95% to 99.5%; the second electrolyte layer comprises a second electrolyte and a second binder, and the mass proportion of the negative electrode electrolyte is 95% to 99.5%.

4. The system for preparing the all-solid-state bipolar unit structure according to claim 3, It is characterized in that Contains at least one of the following features (1) to (5): (1) The positive electrode active material includes at least one of a nickel-cobalt-manganese ternary positive electrode material, a nickel-cobalt-manganese-aluminum quaternary positive electrode material, a lithium-rich manganese-based positive electrode material, lithium iron phosphate, lithium manganese phosphate, lithium iron manganese phosphate, lithium manganese oxide, and lithium nickel manganese oxide; (2) The negative electrode active material includes at least one of artificial graphite, natural graphite, soft carbon, hard carbon, silicon oxygen, silicon carbon, elemental silicon, elemental tin and metallic lithium; (3) The positive electrode conductive agent and the negative electrode conductive agent each independently include at least one of conductive carbon black, carbon nanotubes, carbon fibers, Ketjen black and graphene; (4) The positive electrode electrolyte and the first electrolyte each independently include a halide electrolyte and / or a sulfide electrolyte; (5) The negative electrode electrolyte and the second electrolyte each independently include Li (6-n) PS (5-n) Q (1+n) and zLi 2 S·(1-z)P 2 S 5 At least one of; wherein, Q is Cl, Br or I; 0≤n≤0.6; 0.2≤z≤0.

8.

5. The system for preparing the all-solid-state bipolar unit structure according to claim 1, It is characterized in that Contains at least one of the following features (1) to (3): (1) The thickness of the first electrolyte layer and the second electrolyte layer are independently 7 to 20 μm; (2) The current collector is selected from steel foil and / or nickel foil, and the thickness of the current collector is 2-12 μm; (3) The thickness of the positive electrode layer is 80-150 μm, and the thickness of the negative electrode layer is 90-160 μm.

6. The system for preparing the all-solid-state bipolar unit structure according to claim 1, It is characterized in that The first calendering transfer roller assembly comprises a first positive electrode pressing roller, a second positive electrode pressing roller, a third positive electrode pressing roller and a fourth positive electrode pressing roller which are arranged in sequence, and the fourth positive electrode pressing roller is close to the current collector material strip; the first positive electrode pressing roller and the second positive electrode pressing roller are used to roll the positive electrode material to obtain the positive electrode material strip, and the third positive electrode pressing roller and the fourth positive electrode pressing roller are used to roll and composite the first electrolyte and the positive electrode material strip to obtain a composite positive electrode strip; The second calendering transfer roller assembly includes a first negative electrode pressing roller, a second negative electrode pressing roller, a third negative electrode pressing roller and a fourth negative electrode pressing roller which are arranged in sequence, and the fourth negative electrode pressing roller is close to the current collector strip; the first negative electrode pressing roller and the second negative electrode pressing roller are used to roll the negative electrode material to obtain the negative electrode strip, and the third negative electrode pressing roller and the fourth negative electrode pressing roller are used to roll and composite the first electrolyte and the negative electrode strip to obtain a composite negative electrode strip.

7. The system for preparing the all-solid-state bipolar unit structure according to claim 6, It is characterized in that In the direction from the first positive electrode pressing roller to the third positive electrode pressing roller, the temperature of each pressing roller gradually increases, and the rotation speed of each pressing roller gradually increases; the third positive electrode pressing roller and the fourth positive electrode pressing roller have the same temperature and rotation speed; In the direction from the first negative electrode pressing roller to the third negative electrode pressing roller, the temperature of each pressing roller gradually increases, and the rotation speed of each pressing roller gradually increases; the third negative electrode pressing roller and the fourth negative electrode pressing roller have the same temperature and rotation speed.

8. The system for preparing the all-solid-state bipolar unit structure according to claim 7, It is characterized in that Contains at least one of the following features (1) to (2): (1) Among the first to third positive electrode rollers, the temperature of the rollers is 80-200°C, and the temperature difference between adjacent rollers is 2-20°C; the linear speed of the rollers is 20-50 m / min, and the linear speed ratio of adjacent rollers is 1.05-1.2; (2) Among the first negative electrode roller to the third negative electrode roller, the temperature of the roller is 80-200°C, and the temperature difference between adjacent rollers is 2-20°C. The linear speed of the roller is 20-50 m / min, and the linear speed ratio of adjacent rollers is 1.05-1.

2.

9. A method for preparing an all-solid-state bipolar unit structure, It is characterized in that The preparation system according to any one of claims 1 to 8 comprises the following steps: The current collector tape supply device of the electrode winding and unwinding device is used to provide the current collector tape; The positive electrode material is subjected to a rolling process using a first calendering transfer roller assembly to obtain a positive electrode material strip, and the first solid electrolyte and the positive electrode material strip are subjected to a rolling composite process to obtain a composite positive electrode strip having a positive electrode material strip and a first electrolyte material strip; The negative electrode material is subjected to a rolling process using a second calendering transfer roller assembly to obtain a negative electrode material strip, and the second solid electrolyte and the negative electrode material strip are subjected to a rolling composite process to obtain a composite negative electrode strip having a negative electrode material strip and a second electrolyte material strip; The pressing roller close to the current collector in the first calendering transfer roller assembly cooperates with the pressing roller close to the current collector in the second calendering transfer roller assembly to roll-combine the composite positive electrode strip, the current collector strip and the composite negative electrode strip to obtain an all-solid-state bipolar unit structure; A winding device is used to roll up the all-solid-state bipolar unit structure.

10. The method for preparing the all-solid-state bipolar unit structure according to claim 9, It is characterized in that Also includes: The all-solid-state bipolar unit structure is trimmed.

Citation Information

Patent Citations

  • Positive pole piece and secondary battery

    CN115295804A

  • Solid-state battery manufacturing equipment

    CN117525534A

  • All-solid-state battery and preparation method thereof

    CN117913351A

  • Bipolar type lithium ion battery and manufacturing method thereof

    JP2019212632A

  • Method for preparing bi-polar all solid battery

    KR1020160081369A