Catalyst products with high local rhodium concentration

By introducing a mixed structure of locally high-concentration rhodium-supported material particles and non-supported material particles into the catalyst, the problem of rhodium being easily encapsulated or dissolved is solved, the ignition performance and durability of the catalyst are improved, and efficient emission treatment under low rhodium loading is achieved.

CN118338960BActive Publication Date: 2026-11-10JOHNSON MATTHEY PLC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380014803.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-22
Publication Date
2026-11-10
Estimated Expiration
2043-02-22

AI Technical Summary

Technical Problem

In existing technologies, the precious metal rhodium is easily encapsulated or dissolved by the support material in the catalyst, leading to a deterioration in catalytic performance, especially under low loading conditions, making it difficult to simultaneously meet the requirements of emission control and cost reduction.

Method used

By introducing locally high concentrations of rhodium-supported material particles into the catalyst product, combined with unsupported material particles, a hybrid structure of rhodium-supported and unsupported material particles is formed. The rhodium concentration is from 0.001 wt% to 3.5 wt%, and the rhodium loading is up to 20 g/ft3. The distribution of rhodium is optimized to improve catalytic activity and durability.

Benefits of technology

This approach achieves improved ignition performance and sintering resistance of the catalyst with low total rhodium loading, maintains high conversion rate, reduces the amount of precious metals used, and meets the requirements of emission control and cost reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118338960B_ABST
    Figure CN118338960B_ABST
Patent Text Reader

Abstract

The present invention provides a catalyst article for treating waste gas, the catalyst article comprising: a substrate having an inlet end and an outlet end and having an axial length L; a first catalytic region comprising carrier material particles; at least some of the carrier material particles being rhodium-loaded carrier material particles on which rhodium is loaded, the concentration of rhodium being from 0.001 wt% to 3.5 wt% based on the weight of the rhodium-loaded carrier material particles; and the rhodium being present relative to the first catalytic region at a loading of up to 20 g / ft³.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a catalyst article, a method for manufacturing the catalyst article, a catalyst article obtained by or obtainable by the method, an emission treatment system, and a method for treating waste gas. Background Technology

[0002] Three-way catalytic converter (TWC) catalyzes CO, HC and NO from gasoline engine exhaust. x At a stoichiometric air-fuel ratio, approximately 98% of the CO and HC are simultaneously converted into non-toxic compounds. Specifically, the oxidation of CO and HC to CO2 and vapor (H2O) is primarily catalyzed by Pd, while NO... x The reduction to N2 is primarily catalyzed by Rh. Modern TWC utilizes supported platinum group metal (PGM) catalysts (Pd, Rh, Pt, etc.) deposited on monolayer, bilayer, or multilayer supports. The support material consists of metal oxides with high specific surface areas, primarily stable alumina and cerium dioxide-containing oxygen storage materials. The supported catalyst support coating is then applied to a single ceramic substrate.

[0003] With the significant increase in PGM prices and increasingly stringent emission regulations in recent years, there is a need to reduce the amount of precious metals used in exhaust gas purification catalysts. Among precious metals, Rh is the rarest and most expensive substance on Earth. Therefore, there is a particular desire to highly activate Rh to reduce the cost of PGM use while still meeting stringent emission control regulations.

[0004] In emission control catalysts, one method to reduce the amount of precious metals used is to load the precious metals onto a support and use them as fine particles. For example, WO2016123534A1 reports PGM particle sizes in the range of 10 nm to 92 nm. These PGM nanoparticles are achieved by loading nanoscale supports in the range of 1 nm to 100 nm.

[0005] In areas with low Rh loading (e.g., <20 g / ft) 3 In some emission control catalysts, extremely fine Rh particles form. These particles tend to be encapsulated by the support material due to strong metal-support interaction (SMSI), leading to deterioration of catalytic performance during subsequent catalyst lifetime. Besides moisture in the feed gas composition, high-temperature exposure is a major cause of encapsulation or dissolution of fine Rh particles in the support matrix. Therefore, catalyst durability is insufficient.

[0006] However, when the initial Rh particles are large enough, the Rh encapsulation / dissolution problem is less severe. This is typically seen with higher Rh loadings (e.g., 20 g / ft). 3 Observed in catalysts (or higher). Summary of the Invention

[0007] One aspect of this disclosure relates to providing a catalyst article for treating waste gas, the catalyst article comprising: a substrate including an inlet end and an outlet end, having an axial length L; a first catalytic region including support material particles; at least some of the support material particles being rhodium-loaded support material particles on which rhodium is loaded, the rhodium concentration being from 0.001 wt% to 3.5 wt% based on the weight of the rhodium-loaded support material particles; and the rhodium concentration relative to the first catalytic region being up to 20 g / ft. 3 The capacity exists.

[0008] Another aspect of this disclosure relates to a method of manufacturing a catalyst article, the method comprising: providing rhodium-supported material particles thereon, wherein the concentration of rhodium is from 0.001 wt% to 3.5 wt% based on the weight of the rhodium-supported material particles; providing unsupported material particles thereon that are substantially unsupported by rhodium, preferably unsupported by rhodium; forming a carrier coating comprising the rhodium-supported material particles and the unsupported material particles; and coating a substrate with the carrier coating to provide the catalyst article, wherein the concentration of rhodium is up to 20 g / ft. 3 The capacity exists.

[0009] Another aspect of this disclosure relates to a catalyst article obtained by or obtainable by the methods described above.

[0010] The present invention also covers an emission treatment system comprising the catalyst article described herein and a method for treating waste gas, the method comprising: providing the catalyst article described herein; and contacting the catalyst article with the waste gas. Attached Figure Description

[0011] Figure 1 An embodiment of the invention is shown, comprising a first catalytic region (monolayer) having a length equal to 100% of the axial length L of the substrate.

[0012] Figure 2a An embodiment of the present invention is shown, wherein a first catalytic region extends 100% of the axial length L as a bottom layer; and a second catalytic region extends 100% of the axial length L as a top layer. Figure 2b Depicting Figure 2a A variant of .

[0013] Figure 3a An embodiment of the invention is shown, wherein the first catalytic region extends from the inlet end with an axial length L of less than 100%; and the second catalytic region extends from the outlet end with an axial length L of less than 100%. The total length of the second catalytic region and the first catalytic region is equal to or less than the axial length L. Figure 3b Depicting Figure 3a A variant of .

[0014] Figure 3c An embodiment of the present invention is shown, wherein the first catalytic region extends from the inlet end with an axial length L of less than 100%; and the second catalytic region extends from the outlet end with an axial length L of less than 100%. The total length of the second catalytic region and the first catalytic region is greater than the axial length L. Figure 3d Depicting Figure 3c A variant of .

[0015] Figure 4a An embodiment of the invention is shown, wherein a first catalytic region extends from the inlet end for less than 100% of its axial length L; a second catalytic region extends from the outlet end for less than 100% of its axial length L. The total length of the second and first catalytic regions is less than or equal to the axial length L. A third catalytic region extends for 100% of its axial length L and serves as a top layer covering the first and second catalytic regions. Figure 4b Depicting Figure 4a A variant of .

[0016] Figure 4c An embodiment of the invention is shown, wherein a third catalytic region extends as a bottom layer for 100% of the axial length L. A first catalytic region extends from the inlet end for less than 100% of the axial length L; a second catalytic region extends from the outlet end for less than 100% of the axial length L. The total length of the second catalytic region and the first catalytic region is less than or equal to the axial length L. Figure 4d Depicting Figure 4c A variant of .

[0017] Figure 5a An embodiment of the invention is shown, wherein a first catalytic region extends 100% of the axial length L as a bottom layer; a second catalytic region extends 100% of the axial length L as an intermediate layer; and a third catalytic region extends 100% of the axial length L as a top layer. Figure 5b and Figure 5c Depicting Figure 5a A variant of .

[0018] Figure 6a An embodiment of the invention is shown, wherein a first catalytic region extends from the inlet end for less than 100% of its axial length L; a second catalytic region extends from the outlet end for less than 100% of its axial length L. The total length of the second and first catalytic regions is greater than the axial length L. A third catalytic region extends for 100% of its axial length L and serves as a top layer covering the first and second catalytic regions. Figures 6b to 6f Depicting Figure 6a A variant of .

[0019] Figure 6gAn embodiment of the invention is shown, wherein a first catalytic region extends from the inlet end with an axial length L of less than 100%; a second catalytic region extends from the outlet end with an axial length L of less than 100%. The total length of the second catalytic region and the first catalytic region may be less than, equal to, or greater than the axial length L. A third catalytic region extends from the inlet end with an axial length L of less than 100% and at least partially covers the first catalytic region and / or the second catalytic region. Figure 6h and Figure 6i Depicting Figure 6g A variant of .

[0020] Figure 6j An embodiment of the invention is shown, wherein a first catalytic region extends from the inlet end with an axial length L of less than 100%; a second catalytic region extends from the outlet end with an axial length L of less than 100%. The total length of the second and first catalytic regions may be less than, equal to, or greater than the axial length L. A third catalytic region extends from the outlet end with an axial length L of less than 100% and at least partially covers the second and / or first catalytic regions. Figure 6k and Figure 6l Depicting Figure 6j A variant of .

[0021] Figure 7 The NO levels of reference catalyst 1 and inventive catalysts 1-3 were shown in the λ scan test during engine testing. x The results of CO conversion rate.

[0022] Figure 8 The results of THC conversion tests during engine testing are shown for reference catalyst 1 and inventive catalysts 1-3 using λ scan.

[0023] Figure 9 The NO levels of reference catalyst 2 and inventive catalysts 4-6 were shown in the λ scan test during engine testing. x The results of CO conversion rate.

[0024] Figure 10 The results of THC conversion tests using λ-scan during engine testing are shown for reference catalyst 2 and inventive catalysts 4-6.

[0025] Figure 11 The NO levels of reference catalyst 3, inventive catalyst 7, and inventive catalyst 8 were shown in the λ scan test during engine testing. x The results of CO conversion rate.

[0026] Figure 12 The results of THC conversion tests during engine testing are shown for reference catalyst 3, inventive catalyst 7, and inventive catalyst 8 using λ-scan.

[0027] Figure 13The NO content at the post-catalyst position during thermal RDE testing of reference catalyst 1 and inventive catalysts 1-3 in engine testing is shown. x The cumulative mass.

[0028] Figure 14 The cumulative mass of CO at the post-catalyst position during the thermal RDE test of reference catalyst 1 and inventive catalysts 1-3 during engine testing is shown.

[0029] Figure 15 The cumulative THC at the post-catalyst position during the thermal RDE test of reference catalyst 1 and inventive catalysts 1-3 during engine testing is shown.

[0030] Figure 16 The NO content at the post-catalyst location is shown for reference catalyst 2 and inventive catalysts 4-6 during thermal RDE testing in engine testing. x The cumulative mass.

[0031] Figure 17 The cumulative mass of CO at the post-catalyst position during the thermal RDE test of reference catalyst 2 and inventive catalysts 4-6 during engine testing is shown.

[0032] Figure 18 The cumulative THC at the post-catalyst position is shown for reference catalyst 2 and inventive catalysts 4-6 during the thermal RDE test during engine testing.

[0033] Figure 19 The NO content at the post-catalyst location is shown for reference catalyst 3, inventive catalyst 7, and inventive catalyst 8 during thermal RDE testing in engine testing. x The cumulative mass.

[0034] Figure 20 The cumulative mass of CO at the post-catalyst position during the thermal RDE test of reference catalyst 3, inventive catalyst 7, and inventive catalyst 8 during engine testing is shown.

[0035] Figure 21 The cumulative mass of THC at the post-catalyst position during the thermal RDE test of reference catalyst 3, inventive catalyst 7, and inventive catalyst 8 during engine testing is shown.

[0036] Figure 22 The NO content at the post-catalyst position during thermal RDE testing of reference catalyst 4 and inventive catalysts 9-11 in engine testing is shown. x The cumulative mass.

[0037] Figure 23The cumulative mass of CO at the post-catalyst position during the thermal RDE test of reference catalyst 4 and inventive catalysts 9-11 during engine testing is shown.

[0038] Figure 24 The cumulative THC at the post-catalyst position during the thermal RDE test of reference catalyst 4 and inventive catalysts 9-11 during engine testing is shown.

[0039] Figure 25 The NO content at the post-catalyst position is shown for reference catalyst 4 and inventive catalysts 9-11 during WLTC testing in engine testing. x The cumulative mass.

[0040] Figure 26 The cumulative mass of CO at the post-catalyst position during WLTC testing of reference catalyst 4 and inventive catalysts 9-11 during engine testing is shown.

[0041] Figure 27 The cumulative THC at the post-catalyst position is shown for reference catalyst 4 and inventive catalysts 9-11 during WLTC testing during engine testing.

[0042] Figure 28 This illustrates the concept of locally concentrating Rh on a portion of the carrier material to increase the Rh particle size. Detailed Implementation

[0043] This invention seeks to solve at least some of the problems associated with the prior art or to provide at least commercially acceptable alternative solutions.

[0044] In a first aspect, the present invention provides a catalyst article for treating waste gas, the catalyst article comprising:

[0045] A substrate, comprising an inlet end and an outlet end, having an axial length L;

[0046] A first catalytic region, the first catalytic region comprising support material particles;

[0047] At least some of the carrier material particles are rhodium-loaded carrier material particles on which rhodium is loaded, and the concentration of rhodium is from 0.001% to 3.5% by weight based on the weight of the rhodium-loaded carrier material particles; and

[0048] Rhodium relative to the first catalytic region at up to 20 g / ft 3 The capacity exists.

[0049] Unless expressly indicated otherwise, each aspect or embodiment as defined herein may be combined with any other aspect or embodiment. Specifically, any feature indicated as preferred or advantageous may be combined with any other feature indicated as preferred or advantageous.

[0050] First catalytic region

[0051] Preferably, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.3 wt% to 3.5 wt%. More preferably, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.4 wt% to 3.0 wt%, even more preferably 0.4 wt% to 2.0 wt%, and still more preferably 0.4 wt% to 1.5 wt%. Alternatively, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.3 wt% to 1.8 wt%, even more preferably 0.4 wt% to 1.2 wt%, and still more preferably 0.4 wt% to 1.0 wt%.

[0052] In known catalyst preparations, when rhodium is at a rate of up to 20 g / ft relative to the first catalytic region... 3 When a relatively low loading of rhodium is present, the rhodium-loaded support material particles may not have the high rhodium concentration loaded on them as required in this invention. This may be because rhodium is typically uniformly loaded, i.e., loaded at a uniform concentration on each support material particle present in a particular catalyst region. In other words, the rhodium-loaded support material particles do not have locally high concentrations of rhodium.

[0053] Surprisingly, when used in emission treatment systems, the catalyst of the present invention, having a locally higher concentration of rhodium as defined herein but still with a low total rhodium loading to reduce PGM usage, exhibits significantly improved ignition performance (i.e., lower ignition temperature, higher ignition temperature for specific target substances [NO]) compared to catalysts without a locally higher concentration of rhodium. x The temperature at which the conversion of [CO or total hydrocarbons (THC)] reaches 50%. Furthermore, having a locally high concentration of rhodium while maintaining a low total rhodium loading can result in larger rhodium particles on the rhodium-supported material, which can surprisingly lead to catalysts in which the rhodium particles are more resistant to sintering, oxidation, and migration compared to other low-rhodium-loading catalysts. However, it has also been found that over-concentrating rhodium on the rhodium-supported material particles can then lead to a decrease in catalytic activity. Therefore, for a given low total rhodium loading, there may be an optimal local rhodium concentration.

[0054] The aforementioned effects may be particularly beneficial for catalyst articles with low total rhodium loadings, but may not be observed for catalyst articles with high total rhodium loadings. Not wishing to be bound by theory, it is thought that this may be because when the total rhodium loading relative to the support is already high, the local concentration of rhodium on each of the support material particles is already high, and therefore it may not be necessary to locally concentrate rhodium on a portion of the support material. In other words, due to the presence of locally concentrated rhodium, the present invention can mitigate the problems caused by reducing the total Rh loading on the catalyst article by allowing some of the benefits associated with higher loadings to exist at lower total loadings.

[0055] As used herein, the term "catalyst article" may cover articles on or in which a catalyst is supported. Such articles may take the form of, for example, monolithic honeycomb materials or filters, such as wall-flow filters or flow-through filters.

[0056] As used herein, the term "substrate" can encompass, for example, ceramic or metal honeycomb structures or filter blocks (e.g., wall-flow or flow-through filters). The substrate may include a single ceramic substrate. The substrate can vary in its material composition, size and construction, pore shape and density, and wall thickness. Suitable substrates are known in the art.

[0057] As used herein, the term "catalyst region" can encompass a region on a substrate, typically obtained by drying and / or calcining a support coating. For example, a "region" may be set or supported on the substrate in the form of a "layer" or "zone." The regions or arrangement on the substrate are generally controlled during the application of the support coating to the substrate. "Regions" typically have distinct boundaries or edges (i.e., one region can be distinguished from another using conventional analytical techniques).

[0058] Preferably, the "catalyst region" has a substantially uniform composition (i.e., on average, the composition of the carrier coating does not differ significantly when a portion of the region is compared to another portion of the region). In this context, a substantially uniform composition means that the difference in composition between a portion of the region and another portion of the region is 5% or less, typically 2.5% or less, and most typically 1% or less of the material (e.g., the region).

[0059] The first catalyst region is preferably disposed on the substrate. In the context of this aspect, the term "disposed on" may cover both directly disposed on the substrate (i.e., without intermediary material) and / or indirectly disposed on the substrate (i.e., with intermediary material). If the substrate is porous, the term "disposed on" may also cover disposing the catalyst region therein, for example, disposed within pores of the substrate, i.e., wherein the catalyst region is disposed on and / or therein.

[0060] As used herein, the term "carrier coating" is well known in the art and refers to an adhesive coating typically applied to a substrate during catalyst production. Preferably, the first catalyst region is the carrier coating.

[0061] As used herein, the term "carrier material" may encompass any known carrier material that can be used to load PGMs in the field of this invention, typically in powder form. Carrier materials are not particularly limited, and suitable carrier materials are known in the art. It is not intended to be theoretically restrictive, but rather to suggest that the benefits of the invention may be independent of the carrier material. However, preferred carrier materials are outlined herein.

[0062] In the context of this invention, "rhodium-loaded carrier material particles" are carrier material particles on which rhodium is loaded. In this context, the term "loaded thereon" means that rhodium, typically in the form of nanoparticles, is in direct contact with and physically and / or chemically bonded to the surface of the carrier material. The term "surface of the carrier material" may encompass the surface of pores within a porous carrier material.

[0063] Preferably, rhodium is not alloyed with another metal.

[0064] Preferably, the rhodium-supported material particles are substantially uniformly dispersed throughout the first catalyst region. In this context, the term "substantially uniformly dispersed" may cover a concentration of rhodium-supported material particles in any sub-region of the first catalyst region that is substantially the same as the concentration of rhodium-supported material particles in different arbitrary sub-regions of the first catalyst region, such as within 5%, 3%, 2%, and preferably within 1% of the concentration.

[0065] At least some of the carrier material particles are rhodium-loaded carrier material particles on which rhodium is loaded, and the concentration of rhodium is from 0.001% to 3.5% by weight based on the weight of the rhodium-loaded carrier material particles. "Based on the weight of the rhodium-loaded carrier material particles" means that the weight of rhodium is from 0.001% to 3.5% of the weight of the carrier material particles (e.g., alumina powder particles). In other words, the term "% by weight" refers to the weight of the carrier material particles, not the total weight of the carrier material particles and rhodium. Preferably, based on the weight of the rhodium-loaded carrier material particles, the rhodium-loaded carrier material particles have rhodium loaded thereon at a concentration of 0.3% to 3.5% by weight, more preferably 0.4% to 3.0% by weight, even more preferably 0.4% to 2.0% by weight, even more preferably 0.4% to 1.8% by weight, even more preferably 0.4% to 1.6% by weight, and even more preferably 0.4% to 1.5% by weight. For example, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles preferably have rhodium loaded thereon at a concentration of 0.4 wt% to 1.3 wt%. In another preferred embodiment, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.4 wt% to 1.8 wt%. It should be understood that the present invention may cover preferred sub-ranges formed by any combination of the above endpoints.

[0066] Without being bound by theory, it is believed that maintaining a similar amount of total support material allows for the maintenance of the thermal durability of the support material (such as alumina) compared to conventional catalyst regions that do not have locally concentrated rhodium-supported material but have a uniformly distributed low concentration of rhodium. Therefore, it is preferred that at least some of the support material particles are unsupported support material particles that are substantially free of rhodium, and preferably free of rhodium. In the context of this invention, "unsupported support material particles" are support material particles that are substantially free of rhodium, and preferably free of rhodium.

[0067] As used herein, the term "substantially rhodium-free" can cover, based on a weight of unsupported carrier material particles having rhodium loaded thereon at a concentration of less than 0.001% by weight, preferably less than 0.0005% by weight, and more preferably less than 0.0001% by weight. In other words, the amount of rhodium preferably loaded on the unsupported carrier material particles is negligible. However, it should be understood that in practice, under the high-temperature conditions of the intended use of such catalyst articles, small amounts of rhodium can migrate from the rhodium-supported carrier material particles to the unsupported carrier material particles. To a certain extent, this is unavoidable within the limitations of the technology. Therefore, the present invention aims to cover the unavoidable amount of rhodium loaded on the unsupported carrier material particles.

[0068] Furthermore, to avoid being bound by theory, it is also believed that the presence of unsupported material particles can provide a physical barrier and / or create further distance between rhodium-supported material particles, thereby reducing the likelihood of rhodium nanoparticles sintering and agglomerating on different rhodium-supported material particles, for example, when the catalyst product is subjected to aging conditions. Such advantages may not be achievable by simply reducing the total amount of support material in known catalysts while maintaining the same amount of rhodium to achieve a higher rhodium concentration on each support material particle (i.e., 100% rhodium-supported material particles in the first catalyst region based on the total amount of support material in the first catalyst region).

[0069] Preferably, 5% to 80% of the support material particles in the first catalyst region are rhodium-supported support material particles. In other words, 5% to 80% of the rhodium-supported and unsupported support material particles in the first catalyst region are rhodium-supported support material particles. In this context, % is simply a numerical percentage that can be measured by TEM or any other suitable method. More preferably, 7% to 60%, even more preferably 10% to 50%, still more preferably 11% to 45%, still more preferably 13% to 40%, and still more preferably 15% to 35% of the support material particles in the first catalyst region are rhodium-supported support material particles. For example, preferably, 10% to 25% of the support material particles in the first catalyst region are rhodium-supported support material particles. In another preferred embodiment, 20% to 35% of the support material particles in the first catalyst region are rhodium-supported support material particles.

[0070] Without being bound by theory, it is believed that loading rhodium only on a small percentage of the support material particles can produce improved catalysts with improved ignition performance and sintering resistance, compared to catalysts with similar rhodium loading but with rhodium loaded on all support material particles, due to the assumptions in this paper.

[0071] Preferably, the support material particles, i.e., the support material particles in the first catalyst region, are substantially composed of rhodium-supported support material particles and unsupported support material particles. In other words, the rhodium-supported support material particles and unsupported support material particles preferably account for 90% or more by weight of the support material particles, more preferably 95% or more by weight, even more preferably 97% or more by weight, and still more preferably 99% or more by weight. Most preferably, the support material particles, i.e., the support material particles in the first catalyst region, are composed of rhodium-supported support material particles and unsupported support material particles.

[0072] Preferably, the first catalyst region comprises rhodium-supported carrier material particles, unsupported carrier material particles, and optionally a binder.

[0073] The carrier material particles can be alumina, cerium dioxide, zirconium oxide, magnesium oxide, silicon dioxide, lanthanum, neodymium, praseodymium, yttrium oxides, and mixed or composite oxides thereof. In some embodiments, the carrier material particles can be oxygen storage capacity (OSC) materials, such as cerium oxide, cerium dioxide-zirconia mixed oxides, alumina-cerium dioxide-zirconia mixed oxides, or combinations thereof. In other embodiments, the carrier material particles can be alumina, lanthanum / alumina composite oxides, or magnesium oxide / alumina composite oxides. Preferably, the carrier material particles comprise alumina and / or cerium dioxide-zirconia mixed oxides. In some preferred embodiments, the carrier material is alumina. In other preferred embodiments, the carrier material is a cerium dioxide-zirconia mixed oxide. Preferably, the alumina and / or cerium dioxide-zirconia mixed oxide is doped with one or more of the following substances: lanthanum, neodymium, yttrium, niobium, praseodymium, hafnium, molybdenum, titanium, vanadium, zinc, cadmium, manganese, iron, copper, calcium, barium, strontium, cesium, magnesium, potassium, and sodium, preferably one or more of lanthanum, neodymium, and yttrium, and preferably wherein the alumina and / or cerium dioxide-zirconia mixed oxide is doped with oxides of these substances. Preferably, the dopant is present in the alumina and / or cerium dioxide-zirconia mixed oxide in an amount of 0.001% to 20% by weight, more preferably 0.5% to 10% by weight. The weight percentage can be based on the total weight of the alumina and / or cerium dioxide-zirconia mixed oxide.

[0074] Preferably, the carrier material particles have a density of 0.1µm to 25µm, more preferably 0.5µm to 5µm. 90 As used in this article, the term "D" 90 "It can cover values ​​in the size distribution, up to and including those values, with 90% of the total volume of material in the sample being 'included'." D 90 Any suitable technique can be used for measurement, such as TEM.

[0075] Preferably, the carrier material particles comprise a cerium dioxide-zirconia mixed oxide; and wherein, when the cross-sectional area of ​​the first catalyst region of the catalyst article is analyzed by FE-EPMA under conditions of a pixel (section) size of 0.34µm × 0.34µm and a measurement pixel (section) number of 256 × 256, the characteristic X-ray intensity (α: cps) of zirconium (Zr) and the characteristic X-ray intensity (β: cps) of rhodium (Rh) are measured for each pixel, and the Pearson correlation coefficient calculated using the obtained α and β in each pixel is designated as R. Zr / Rh At that time R Zr / Rh The value is between 0.15 and 0.48. More preferably, R Zr / Rh The value ranges from 0.3 to 0.45.

[0076] The Pearson correlation coefficient (product-moment correlation coefficient) is known to those skilled in the art and is calculated based on the results of area analysis performed by FE-EPMA (field emission-electron probe microscopy). The correlation coefficient R... Zr / Rh R is determined by the following formula: Zr / Rh = (covariance) / (standard deviation of α × standard deviation of β), where in the area analysis performed by FE-EPMA, the first variable (α) is the characteristic X-ray intensity of zirconium (Zr), and the second variable (β) is the characteristic X-ray intensity of rhodium (Rh). This calculation is known to those skilled in the art. In other words, preferably, zirconium and rhodium are not highly correlated in such catalyst articles. That is, rhodium is preferably not highly dispersed relative to zirconium in the support material. This may be due to the locally higher concentration of rhodium on some support material particles, followed by the presence of unsupported support material particles. Therefore, this can be a convenient method for characterizing the preferred distribution of rhodium on the support material in this invention, which can achieve the above-mentioned technical advantages.

[0077] Preferably, the rhodium content relative to the first catalytic region (e.g., particularly when the first catalytic region extends less than the total length L of the substrate, such as 20% to 80%, 30% to 70%, or 40% to 60% of the total length L) is 1 g / ft. 3 Up to 20g / ft 3 More preferably 2g / ft 3 Up to 18g / ft 3 , or even better, 3g / ft 3 Up to 16g / ft 3 Even better, 4g / ft 3 Up to 16g / ft 3 The loading is present. Alternatively, rhodium is added at a rate of 1 g / ft relative to the first catalytic region (e.g., particularly when the first catalytic region extends the entire length of the substrate). 3 Up to 20g / ft 3 More preferably 2g / ft 3 Up to 15g / ft 3 , or even better, 3g / ft 3 Up to 10g / ft 3 Even better, 4g / ft 3 Up to 10g / ft 3 The available load capacity is significant. The benefits described herein may be particularly pronounced at such low loads. Furthermore, such low load capacity aligns with the general expectation in the art of reducing PGM usage.

[0078] Preferably, the carrier material particles are positioned relative to the first catalytic region at a ratio of 0.5 g / in. 3 Up to 3g / in 3The loading is present. Methods for calculating such loading are well known to those skilled in the art. More preferably, the carrier material particles relative to the first catalytic region have a loading rate of 0.5 g / in. 3 Up to 2g / in 3 , or even more preferably 0.6g / in 3 Up to 2g / in 3 Even more preferably 0.75g / in 3 Up to 2g / in 3 , or even more preferably 0.8g / in 3 Up to 2g / in 3 The loading is present. In some preferred embodiments, the support material particles are positioned relative to the first catalytic region at a loading of approximately 1 g / in. 3 The loading is present. This loading is particularly suitable for obtaining the advantages described herein at the specific rhodium loading claimed in the claims.

[0079] Preferably, the first catalyst region further comprises a binder, preferably wherein the binder comprises additional alumina material, such as alumina, preferably γ-alumina, more preferably lanthanum-doped γ-alumina, such as 4% La-Al2O3. The binder is preferably present at a concentration of 0.5 g / in relative to the substrate. 3 Up to 2g / in 3 More preferably about 1.0 g / in 3 The amount is present. For example, the presence of this additional binder may be particularly suitable when the first catalyst region is a carrier coating.

[0080] The catalyst article preferably further comprises one or more additional catalyst regions. These additional catalyst regions may differ from those described herein and required by the invention. For example, the one or more additional catalyst regions may be any suitable additional catalyst regions known to those skilled in the art. In particular, it is preferred that the one or more additional catalyst regions comprise one or more catalyst regions for three-way catalysis. Preferably, one or more of the additional catalyst regions comprise platinum and / or palladium. Platinum and / or palladium may be supported on a support material. Suitable support materials are known in the art.

[0081] Second catalytic region

[0082] The catalyst may further include a second catalytic region.

[0083] The second catalytic region may further include a second PGM component, a second oxygen storage capacity (OSC) material, a second alkali metal or alkaline earth metal component, and / or a second inorganic oxide.

[0084] The second PGM component may be selected from the group consisting of platinum, palladium, rhodium, and mixtures thereof. In some embodiments, the second PGM component may be Pd, Rh, or mixtures thereof.

[0085] The second OSC material can be cerium oxide, zirconium oxide, a cerium dioxide-zirconia mixed oxide, an aluminum oxide-cerium dioxide-zirconia mixed oxide, or a combination thereof. More preferably, the second OSC material comprises a cerium dioxide-zirconia mixed oxide, an aluminum oxide-cerium dioxide-zirconia mixed oxide, or a combination thereof. Additionally, the second OSC material may also contain one or more dopants, such as lanthanum, neodymium, praseodymium, yttrium, etc. Furthermore, the second OSC material can function as a carrier material for the second PGM component. In some embodiments, the second OSC material comprises a cerium dioxide-zirconia mixed oxide and an aluminum oxide-cerium dioxide-zirconia mixed oxide.

[0086] The cerium dioxide-zirconia mixed oxide may have a cerium dioxide to zirconium dioxide weight ratio of at least 50:50, preferably higher than 60:40, and more preferably higher than 70:30. Alternatively, the cerium dioxide-zirconia mixed oxide may also have a cerium dioxide to zirconium dioxide weight ratio of less than 50:50, preferably less than 40:60, and more preferably less than 30:70.

[0087] Based on the total load of the support coating in the second catalytic region, the second OSC material (e.g., cerium dioxide-zirconia mixed oxide) may be 10% to 90% by weight; preferably 25% to 75% by weight; more preferably 30% to 60% by weight.

[0088] The loading of the second OSC material in the second catalytic region can be less than 2 g / in. 3 In some implementations, the loading of the second OSC material in the second catalytic region is no greater than 1.5 g / in. 3 1.2g / in 3 1g / in 3 0.8g / in 3 or 0.7g / in 3 .

[0089] The second alkali metal or alkaline earth metal is preferably barium or strontium, or a mixed oxide or composite oxide thereof. Preferably, based on the total weight of the second catalytic region, barium or strontium (if present) is 0.1% to 15% by weight, and more preferably 3% to 10% by weight.

[0090] Even more preferably, the second alkali metal or alkaline earth metal is strontium. Based on the total weight of the second catalytic region, strontium (when present) is preferably present in an amount of 0.1% to 15% by weight, and more preferably 3% to 10% by weight.

[0091] Also preferably, the second alkali metal or alkaline earth metal is a mixed oxide or composite oxide of barium and strontium. Preferably, the mixed oxide or composite oxide of barium or strontium is present in an amount of 0.1% to 15% by weight, and more preferably 3% to 10% by weight, based on the total weight of the second catalytic region. More preferably, the second alkali metal or alkaline earth metal is a composite oxide of barium and strontium.

[0092] Preferably, barium or strontium is present in the form of BaCO3 or SrCO3. Such materials can be pre-formed by any method known in the art, such as initial wetting impregnation or spray drying.

[0093] The second inorganic oxide is preferably an oxide of an element from Groups 2, 3, 4, 5, 13, and 14. Preferably, the second inorganic oxide is selected from the group consisting of aluminum oxide, magnesium oxide, silicon dioxide, zirconium oxide, barium oxide, and mixed or composite oxides thereof. Particularly preferably, the second inorganic oxide is aluminum oxide, lanthanum-alumina, zirconium oxide, or a magnesium oxide / alumina composite oxide. A particularly preferred second inorganic oxide is aluminum oxide or lanthanum-alumina.

[0094] The second OSC material and the second inorganic oxide can have the following weight ratio: not greater than 10:1; preferably not greater than 8:1 or 5:1; more preferably not greater than 4:1 or 3:1; and most preferably not greater than 2:1.

[0095] Alternatively, the weight ratio of the second OSC material to the second inorganic oxide may be 10:1 to 1:10, preferably 8:1 to 1:8 or 5:1 to 1:5; more preferably 4:1 to 1:4 or 3:1 to 1:3; and most preferably 2:1 to 1:2.

[0096] In some embodiments, the weight ratio of the second OSC material to the second inorganic oxide may be not less than 2:1. In another embodiment, the weight ratio of the second OSC material to the second inorganic oxide may be not less than 10:1. In yet another embodiment, the weight ratio of the second OSC material to the second inorganic oxide may be not less than 20:1 or not less than 30:1. In still another embodiment, the weight ratio of the second OSC material to the second inorganic oxide may be not less than 40:1 or not less than 50:1.

[0097] The total carrier coating loading in the second catalytic region can be less than 3.5 g / in. 3 Preferably less than 3.0 g / in3 Or 2.5g / in 3 Alternatively, the total carrier coating loading in the first catalytic region can be 0.5 g / in. 3 Up to 3.5g / in 3 Preferably, it can be 0.6 g / in 3 Up to 3g / in 3 or 0.7g / in 3 Up to 2.5g / in 3 .

[0098] The second catalytic region can extend to 100% of the axial length L (e.g., see...). Figure 2a , Figure 2b and Figures 6a to 6c ).

[0099] The second catalytic region can extend from 30% to 70% of the axial length L. Preferably, it extends from 40% to 60% of the axial length L, more preferably from 45% to 55% of the axial length L, and most preferably, the total length of the second and first regions is equal to or greater than the axial length L (see, for example, [reference needed]). Figure 3a To Figure 5d and Figure 7 a to Figure 7 l).

[0100] The second catalytic region may overlap with the first catalytic region by 0.1% to 99% of its axial length L (e.g., see [reference]). Figure 3c and Figure 3d The first catalytic region may cover the second catalytic region, or the second catalytic region may cover the first catalytic region. Alternatively, the total length of the second catalytic region and the first catalytic region may be equal to the axial length L (e.g., see [reference]). Figure 3a and Figure 3b In another alternative, the total length of the second catalytic region and the first catalytic region may be less than the axial length L, for example, no more than 95%, 90%, 80% or 70% of the axial length L.

[0101] In some embodiments, the first catalytic region can be directly supported / deposited on the substrate. In some embodiments, the second catalytic region can be directly supported / deposited on the substrate.

[0102] Third catalytic region

[0103] The catalyst may further include a third catalytic region.

[0104] The third catalytic region may further include a third PGM component, a third oxygen storage capacity (OSC) material, a third alkali metal or alkaline earth metal component, and / or a third inorganic oxide.

[0105] The third PGM component may be selected from the group consisting of platinum, palladium, rhodium, and mixtures thereof. In some embodiments, the third PGM component may be Pd, Rh, or mixtures thereof.

[0106] The third OSC material may be cerium oxide, zirconium oxide, a cerium dioxide-zirconia mixed oxide, an aluminum oxide-cerium dioxide-zirconia mixed oxide, or a combination thereof. More preferably, the third OSC material comprises a cerium dioxide-zirconia mixed oxide, an aluminum oxide-cerium dioxide-zirconia mixed oxide, or a combination thereof. Additionally, the third OSC material may further comprise one or more dopants, such as lanthanum, neodymium, praseodymium, yttrium, etc. Furthermore, the third OSC material may function as a carrier material for the third PGM component. In some embodiments, the third OSC material comprises a cerium dioxide-zirconia mixed oxide and an aluminum oxide-cerium dioxide-zirconia mixed oxide.

[0107] The cerium dioxide-zirconia mixed oxide can have a cerium dioxide to zirconium dioxide weight ratio of at least 50:50, preferably higher than 60:40, and more preferably higher than 75:25. Alternatively, the cerium dioxide-zirconia mixed oxide can also have a cerium dioxide to zirconium dioxide weight ratio of less than 50:50; preferably less than 40:60; and more preferably less than 25:75.

[0108] Based on the total load of the support coating in the third catalytic region, the third OSC material (e.g., cerium dioxide-zirconia mixed oxide) may be 10% to 90% by weight; preferably 25% to 75% by weight; more preferably 30% to 60% by weight.

[0109] The loading of the third OSC material in the third catalytic region can be less than 1.5 g / in. 3 In some implementations, the loading of the third OSC material in the second catalytic region is no greater than 1.2 g / in. 3 1.0g / in 3 0.9g / in 3 0.8g / in 3 or 0.7g / in 3 .

[0110] The total carrier coating loading in the third catalytic region can be less than 3.5 g / in. 3 Preferably, the concentration is no more than 3.0 g / in. 3 2.5g / in 3 or 2g / in 3 .

[0111] The third alkali metal or alkaline earth metal is preferably barium or strontium, or their mixed oxides or composite oxides. Preferably, based on the total weight of the third catalytic region, barium or strontium (when present) is 0.1% to 15% by weight, and more preferably 3% to 10% by weight.

[0112] Even more preferably, the third alkali metal or alkaline earth metal is strontium. Based on the total weight of the third catalytic region, strontium (when present) is preferably present in an amount of 0.1% to 15% by weight, and more preferably 3% to 10% by weight.

[0113] Also preferably, the third alkali metal or alkaline earth metal is a mixed oxide or composite oxide of barium and strontium. Preferably, the mixed oxide or composite oxide of barium or strontium is present in an amount of 0.1% to 15% by weight, and more preferably 3% to 10% by weight, based on the total weight of the third catalytic region. More preferably, the third alkali metal or alkaline earth metal is a composite oxide of barium and strontium.

[0114] Preferably, barium or strontium is present in the form of BaCO3 or SrCO3. Such materials can be pre-formed by any method known in the art, such as initial wetting impregnation or spray drying.

[0115] The third inorganic oxide is preferably an oxide of elements from Groups 2, 3, 4, 5, 13, and 14. Preferably, the third inorganic oxide is selected from the group consisting of aluminum oxide, magnesium oxide, silicon dioxide, zirconium oxide, barium oxide, and mixed or composite oxides thereof. Particularly preferably, the third inorganic oxide is aluminum oxide, lanthanum-alumina, zirconium oxide, or a magnesium oxide / alumina composite oxide. A particularly preferred third inorganic oxide is aluminum oxide or lanthanum-alumina.

[0116] The weight ratio of the third OSC material to the third inorganic oxide can be no greater than 10:1; preferably no greater than 8:1 or 5:1; more preferably no greater than 4:1 or 3:1; and most preferably no greater than 2:1.

[0117] Alternatively, the weight ratio of the third OSC material to the third inorganic oxide may be 10:1 to 1:10, preferably 8:1 to 1:8 or 5:1 to 1:5; more preferably 4:1 to 1:4 or 3:1 to 1:3; and most preferably 2:1 to 1:2.

[0118] In some embodiments, the weight ratio of the third OSC material to the third inorganic oxide may be not less than 2:1. In another embodiment, the weight ratio of the third OSC material to the third inorganic oxide may be not less than 10:1. In yet another embodiment, the weight ratio of the third OSC material to the third inorganic oxide may be not less than 20:1 or not less than 30:1. In still another embodiment, the weight ratio of the third OSC material to the third inorganic oxide may be not less than 40:1 or not less than 50:1.

[0119] The third catalytic region can extend to 100% of the axial length L (e.g., see...). Figures 4a to 4d and Figures 6a to 6c ).

[0120] The third catalytic region may be smaller than the axial length L, for example, no more than 95%, 90%, 80%, or 70% of the axial length L (see, for example, see...). Figure 5a To Figure 5d and Figure 7 g to Figure 7 l).

[0121] The second catalytic region may overlap with the first catalytic region by 0.1% to 99% of its axial length L (e.g., see [reference]). Figure 7 a to Figure 7 (l), the first catalytic region may cover the second catalytic region, or the second catalytic region may cover the first catalytic region. Alternatively, either the second region or the first region may extend from 30% to 70% of the axial length L. Preferably, it is 40% to 60% of the axial length L, more preferably 45% to 55% of the axial length L, and most preferably, the total length of the second region and the first region is equal to or less than the axial length L (e.g., see...). Figures 4a to 4d ).

[0122] Preferably, the catalyst article comprises a substrate, a first catalyst region as described herein, and a second catalyst region. In other words, the catalyst article preferably further comprises a second catalyst region. The second catalyst region preferably has a different composition from the first catalyst region. Preferably, the second catalyst region comprises a PGM supported on a support material, and optionally one or more of a binder and a promoter. The PGM preferably comprises palladium. The support material preferably comprises alumina and / or a cerium dioxide-zirconia mixed oxide as described herein. The binder preferably comprises alumina. The promoter preferably comprises barium.

[0123] The first catalyst region is preferably disposed on the second catalyst region, and more preferably directly disposed on the second catalyst region. For example, preferably, the second catalyst region is disposed directly on the substrate, and the first catalyst region is disposed directly on the second catalyst region. In these embodiments, the first catalyst region and the second catalyst region are preferably carrier coatings, and each carrier coating is preferably applied over the entire length of the substrate.

[0124] In an alternative preferred embodiment, the catalyst article includes a substrate, a first catalyst region, a second catalyst region, and a third catalyst region as described herein. In other words, the catalyst article preferably further includes the second catalyst region and the third catalyst region. The second catalyst region and the third catalyst region preferably have a different composition than the first catalyst region. Furthermore, the second catalyst region preferably has a different composition than the third catalyst region.

[0125] Preferably, the second catalyst region in this embodiment is as described in the alternative preferred embodiments above. However, in this embodiment, the first catalyst region and the third catalyst region are preferably disposed in the form of zones on the second catalyst region, and preferably directly disposed on the second catalyst region. In particular, the second catalyst region is preferably disposed directly on the substrate, and the first catalyst region and the third catalyst region are preferably each disposed directly on the second catalyst region. The second catalyst region is preferably disposed along the entire length of the substrate, and the first catalyst region and the third catalyst region are preferably disposed in the form of zones on the second catalyst region. In these preferred embodiments, the first catalyst region, the second catalyst region, and the third catalyst region are preferably in the form of a carrier coating.

[0126] In these preferred embodiments, the first catalyst region is preferably a rear region, i.e., located at the intended outlet end of the catalyst article, and the third catalyst region is preferably a front region, i.e., located at the intended inlet end of the catalyst article.

[0127] The third catalyst region preferably contains rhodium supported on a carrier material. Rhodium is preferably disposed on all carrier material particles, as in the standard catalyst region. The carrier material is preferably alumina and / or a cerium dioxide-zirconia mixed oxide as described herein. When the carrier material of the rhodium-supported carrier material particles in the first catalyst region contains alumina, the carrier material of the third catalyst region preferably contains a cerium dioxide-zirconia mixed oxide. When the carrier material of the rhodium-supported carrier material particles in the first catalyst region contains a cerium dioxide-zirconia composite oxide, the carrier material of the third catalyst region preferably contains alumina.

[0128] When the first catalyst region and the third catalyst region are partitioned, these two regions are preferably applied together over the entire length of the substrate, which is preferably the entire length of the second catalyst region.

[0129] Such a preferred arrangement of the first catalyst region, the second catalyst region, and optionally the third catalyst region can surprisingly lead to improved NO. x Elimination, especially during cold start conditions and at lower ignition temperatures, is observed. Improved CO and / or THC elimination is also observed. Improved aging OSC characteristics are also observed.

[0130] As used herein, the term “zone” refers to a region whose length is less than the total length of the base, such as ≤75% of the total length of the base. A “zone” typically has a length of at least 5% (e.g., ≥5%) of the total length of the base (i.e., a substantially uniform length).

[0131] The total length of the substrate is the distance between its inlet end and its outlet end (e.g., the opposite end of the substrate).

[0132] As used herein, any reference to "a region disposed at the inlet end of the substrate" refers to a region disposed on or supported on the substrate, wherein the region is closer to the inlet end of the substrate than a region near the outlet end of the substrate. Therefore, the midpoint of this region is closer to the inlet end of the substrate than the midpoint near the outlet end of the substrate (i.e., at half its length). Similarly, as used herein, any reference to "a region disposed at the outlet end of the substrate" refers to a region disposed on or supported on the substrate, wherein the region is closer to the outlet end of the substrate than a region near the inlet end of the substrate. Therefore, the midpoint of this region is closer to the outlet end of the substrate than the midpoint near the inlet end of the substrate (i.e., at half its length).

[0133] When the substrate is a wall-flow filter, generally speaking, any reference to "the area located at the inlet end of the substrate" refers to the area that is mounted or supported on the substrate, which is:

[0134] (a) The area closer to the inlet end (e.g., the open end) of the inlet channel than the area near the closed end (e.g., the sealed end or the blocked end) of the inlet channel, and / or

[0135] (b) The closed end (e.g., the blocked end or the shut end) of the outlet channel closer to the substrate than the area near the outlet end (e.g., the open end) of the outlet channel.

[0136] Therefore, the midpoint of this zone (i.e., at half its length) (a) is closer to the entrance end of the base's entrance channel than the midpoint near the closed end of the entrance channel, and / or (b) is closer to the closed end of the base's exit channel than the midpoint near the exit end of the exit channel.

[0137] Similarly, when the substrate is a wall-flow filter, any reference to "the area located at the outlet end of the substrate" refers to the area disposed on or supported on the substrate, which is:

[0138] (a) The area closer to the outlet end (e.g., open end) of the outlet channel than the area near the closed end (e.g., closed or blocked end) of the outlet channel, and / or

[0139] (b) The area closer to the closed end (e.g., the sealed end or the blocked end) of the inlet channel than the inlet end (e.g., the open end) of the inlet channel.

[0140] Therefore, the midpoint of this zone (i.e., at half its length) (a) is closer to the exit end of the base's exit channel than the midpoint near the closed end of the exit channel, and / or (b) is closer to the closed end of the base's inlet channel than the midpoint near the inlet end of the inlet channel.

[0141] When the carrier coating is present in the wall of the wall-flow filter (i.e., the zone is in the wall), the zone can satisfy both (a) and (b) at the same time.

[0142] Preferably, the first catalyst region is a single carrier coating disposed on a substrate. The single carrier coating may be applied along the entire length of the substrate or only on a portion thereof. For example, preferably, the single carrier coating is applied from one end of the substrate (e.g., the inlet or outlet end in terms of the intended use in the exhaust system), preferably covering less than 90%, less than 80%, less than 70%, less than 60%, less than 50%, less than 40%, less than 30%, less than 20%, or less than 10% of the substrate length. Preferably, the single carrier coating is applied directly to the substrate. In another preferred embodiment, one or more intervening carrier coatings exist between the single carrier coating of the invention and the substrate. The one or more intervening carrier coatings in this embodiment can be any suitable carrier coating known to those skilled in the art. Preferably, the one or more intervening carrier coatings are suitable for a three-way catalytic converter. In other words, the catalyst article preferably also includes one or more additional carrier coatings.

[0143] Preferably, the first catalyst region further comprises platinum and / or palladium. Platinum and / or palladium may be supported on a support material. Suitable support materials are known in the art.

[0144] Preferably, the catalyst product is used for three-way catalysis. In other words, the catalyst product is preferably TWC.

[0145] base

[0146] Preferably, the substrate is a flow-through solid material. Alternatively, the substrate may be a wall-flow filter.

[0147] The flow-through substrate has a first surface and a second surface defining a longitudinal direction therebetween. The flow-through substrate has a plurality of channels extending between the first and second surfaces. The plurality of channels extend in the longitudinal direction and provide a plurality of inner surfaces (e.g., surfaces defining the walls of each channel). Each of the plurality of channels has an opening at the first surface and an opening at the second surface. For the avoidance of confusion, the flow-through substrate is not a wall-flow filter.

[0148] The first surface is typically located at the inlet end of the substrate, and the second surface is located at the outlet end of the substrate.

[0149] The channels may have a constant width, and each of the multiple channels may have a uniform channel width.

[0150] Preferably, in a plane orthogonal to the longitudinal direction, the monolithic substrate has 300 to 900 channels / square inch, more preferably 400 to 800 channels / square inch. For example, on the first surface, the density of open first channels and closed second channels is 600 to 700 channels / square inch. The channels may have cross-sections of rectangles, squares, circles, ellipses, triangles, hexagons, or other polygonal shapes.

[0151] The monolithic substrate acts as a support for holding the catalytic material. Suitable materials for forming the monolithic substrate include ceramic-like materials such as cordierite, silicon carbide, silicon nitride, zirconium oxide, mullite, spodumene, alumina-silica magnesium oxide or zirconium silicate, or porous refractory metals. Such materials and their uses in the manufacture of porous monolithic substrates are well known in the art.

[0152] It should be noted that the flow-through monolithic substrate described herein is a single component (i.e., a single brick-shaped object). Nevertheless, when forming an emissions treatment system, the substrate used can be formed by adhering multiple channels together or by adhering multiple smaller substrates together, as described herein. Such techniques, as well as suitable housings and configurations for emissions treatment systems, are well known in the art.

[0153] In embodiments where the catalyst article of the present invention comprises a ceramic substrate, the ceramic substrate may be made of any suitable refractory material, such as alumina, silicon dioxide, cerium dioxide, zirconium oxide, magnesium oxide, zeolite, silicon nitride, silicon carbide, zirconium silicate, magnesium silicate, aluminosilicates and metallic aluminosilicates (such as cordierite and spodumene), or any mixture or mixed oxide of two or more thereof. Cordierite, magnesium aluminosilicate, and silicon carbide are particularly preferred.

[0154] In embodiments of the catalyst article of the present invention comprising a metal substrate, the metal substrate may be made of any suitable metal, and specifically of heat-resistant metals and metal alloys, such as titanium and stainless steel, and ferritic alloys containing iron, nickel, chromium and / or aluminum in addition to other trace metals.

[0155] Preferably, the substrate comprises a wall-flow filter substrate. In an alternative preferred embodiment, the substrate comprises a flow-through substrate. The substrate may be "blank," i.e., a substrate without a carrier coating. Alternatively, the substrate may have one or more carrier coatings already loaded thereon. In this case, the final catalyst article may comprise multiple layers of different carrier coatings. The substrate preferably comprises cordierite. However, the composition of the substrate is not particularly limited.

[0156] In another aspect, the present invention provides a method for manufacturing a catalyst article, the method comprising:

[0157] Provided are rhodium-loaded carrier material particles on which rhodium is loaded, wherein the rhodium concentration is from 0.001% to 3.5% by weight based on the weight of the rhodium-loaded carrier material particles.

[0158] Provides non-loaded carrier material particles that are substantially free of rhodium, and preferably free of rhodium;

[0159] Forming a carrier coating comprising rhodium-loaded carrier material particles and non-loaded carrier material particles; and

[0160] A substrate is coated with a carrier coating to provide a catalyst article, wherein rhodium is applied relative to the substrate at a concentration of up to 20 g / ft. 3 The capacity exists.

[0161] Unless otherwise stated, the preferred features and embodiments relating to the first aspect, and in particular any preferred features of the rhodium-supported support material particles, unsupported support material particles, the first catalyst region and / or additional catalyst regions, the general support material particles, the substrate as a whole and the catalyst article, also apply to this aspect.

[0162] Providing rhodium-loaded carrier material particles thereon may include providing carrier material particles and loading rhodium thereon. This method is known in the art, and any suitable technique may be used.

[0163] Forming a carrier coating comprising rhodium-loaded carrier material particles and non-loaded carrier material particles preferably involves mixing the rhodium-loaded carrier material particles and non-loaded carrier material particles with water in any order to form a slurry. As used herein, the term "slurry" can encompass a liquid containing insoluble materials (e.g., insoluble particles). The slurry is typically stirred, more typically for at least 10 minutes, more typically for at least 30 minutes, and even more typically for at least one hour. This method of preparing the carrier coating is known in the art, and the technique is not particularly limited.

[0164] The substrate can be coated with a carrier coating using techniques known in the art. Typically, the carrier coating is applied to the substrate by pouring a predetermined amount of the carrier coating into the inlet of the substrate using a specific molding tool. Alternatively, the substrate can be coated with the carrier coating by immersing the substrate in the carrier coating. Subsequent vacuum and / or air knife and / or drying steps may be employed during the coating step. When the substrate is a filter block, the carrier coating may be applied to the filter wall, inside the filter wall (if porous), or both.

[0165] Importantly, coating the substrate with a support coating provides a catalyst article in which rhodium relative to the substrate is at a concentration of up to 20 g / ft. 3 The loading is present. Those skilled in the art can readily plan the relative amounts of each component (e.g., carrier coating and substrate) used in the method accordingly to achieve this desired rhodium loading.

[0166] Preferably, based on the weight of the rhodium-loaded carrier material particles, the rhodium-loaded carrier material particles have rhodium loaded thereon at a concentration of 0.3% to 3.5% by weight.

[0167] The method preferably further includes adding an adhesive to the carrier coating before coating the substrate with the carrier coating. Preferred adhesives are described elsewhere herein. Preferably, the method further includes adding one or more of an acid, alkali, thickener, and reducing agent to the carrier coating before coating the substrate with the carrier coating.

[0168] Preferably, providing rhodium-loaded carrier material particles includes loading rhodium onto the carrier material particles using initial wet impregnation. Initial wet impregnation is a technique well known to those skilled in the art. Those skilled in the art will be able to perform appropriate initial wet impregnation without further instruction.

[0169] Preferably, providing the rhodium-supported carrier material particles further includes drying and calcining the rhodium-supported carrier material particles. This drying and calcination step is preferably performed before the formation of the carrier coating.

[0170] After coating the substrate with a carrier coating, the resulting catalyst product (or the coated substrate) is preferably dried and / or calcined.

[0171] Preferably, the catalyst article in this aspect is based on the first aspect.

[0172] In another aspect, the present invention provides a catalyst article obtained by or that can be obtained by the methods described above.

[0173] Surprisingly, when used in emission treatment systems, catalysts exhibiting locally higher rhodium concentrations as defined herein, but still with lower total rhodium loadings to reduce PGM usage, show significantly improved ignition performance (i.e., lower ignition temperature, higher ignition efficiency for specific target substances [NO]) compared to catalysts without such concentrations, compared to those without. x The temperature at which the conversion of [CO or total hydrocarbons (THC)] reaches 50%. Furthermore, having a locally high concentration of rhodium while maintaining a low total rhodium loading can result in larger rhodium particles on the rhodium-supported material, which can surprisingly lead to catalysts in which the rhodium particles are more resistant to sintering, oxidation, and migration compared to other low-rhodium-loading catalysts. However, it has also been found that over-concentrating rhodium on the rhodium-supported material particles can then lead to a decrease in catalytic activity. Therefore, for a given low total rhodium loading, there may be an optimal local rhodium concentration.

[0174] The aforementioned effects may be particularly beneficial for catalysts with low total rhodium loadings, but may not be observed in catalysts with high total rhodium loadings. Without being bound by theory, it is thought that this may be because when the total rhodium loading relative to the support is already high, the local concentration of rhodium on each of the support material particles is already high, and therefore it may not be necessary to locally concentrate rhodium on a portion of the support material.

[0175] In another aspect, the present invention provides an emission treatment system comprising the catalyst article described herein. Preferably, the emission treatment system is used in a gasoline engine. Preferably, the gasoline engine operates under stoichiometric conditions.

[0176] In another aspect, the present invention provides a method for treating exhaust gas, the method comprising: providing a catalyst article as described herein; and contacting the catalyst article with the exhaust gas. Preferably, the exhaust gas originates from a gasoline engine. Preferably, the gasoline engine operates under stoichiometric conditions.

[0177] The invention will now be described in conjunction with the following non-limiting embodiments.

[0178] Manufacturing of catalyst products

[0179] Several catalyst products were prepared according to the following examples:

[0180] Reference catalyst 1

[0181] 1. Rh cerium dioxide and zirconium oxide mixed oxide (CZO) pre-fixed powder was prepared by impregnating CZO with a nitric acid Rh solution to achieve an Rh concentration of 0.23% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0182] 2. The calculated amount of pre-fixed Rh CZO powder was slurried, with a target yield of 1.0 g / in. 3 CZO and 4g / ft 3 Rh.

[0183] 3. Blend the slurry with 4% La-Al2O3 slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0184] 4. Adjust the solids and thicken the carrier coating.

[0185] 5. First, coat the substrate with the carrier coating (4) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0186] Invention Catalyst 1

[0187] 1. Rh cerium dioxide and zirconium oxide mixed oxide (CZO) pre-fixed powder was prepared by impregnating CZO with a nitric acid Rh solution to achieve an Rh concentration of 0.75% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0188] 2. The calculated amount of pre-fixed Rh CZO powder was slurried, with a target yield of 0.3 g / in. 3 CZO and 4g / ft 3 Rh.

[0189] 3. Add 0.7g / in 3 An additional amount of CZO slurry was added to make the total CZO equivalent to 1 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated on approximately 31% of the CZO carrier, while the remaining CZO carrier does not contain Rh. This mixture is then continuously blended.

[0190] 4. Blend the slurry with 4% La-Al2O3 slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0191] 5. Adjust the solids and thicken the carrier coating.

[0192] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0193] Invention Catalyst 2

[0194] 1. Rh cerium dioxide and zirconium oxide mixed oxide (CZO) pre-fixed powder was prepared by impregnating CZO with a nitric acid Rh solution to achieve an Rh concentration of 1.5% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0195] 2. The calculated amount of pre-fixed Rh CZO powder was slurried, with a target yield of 0.15 g / in. 3 CZO and 4g / ft 3 Rh.

[0196] 3. Add 0.85g / in 3 An additional amount of CZO slurry was added to make the total CZO equivalent to 1 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated on approximately 15% of the CZO carrier, while the remaining CZO carrier does not contain Rh. This mixture is then continuously blended.

[0197] 4. Blend the slurry with 4% La-Al2O3 slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0198] 5. Adjust the solids and thicken the carrier coating.

[0199] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0200] Invention Catalyst 3

[0201] 1. Rh cerium dioxide and zirconium oxide mixed oxide (CZO) pre-fixed powder was prepared by impregnating CZO with a nitric acid Rh solution to achieve a 3% by weight Rh concentration. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0202] 2. The calculated amount of pre-fixed Rh CZO powder was slurried, with a target yield of 0.08 g / in. 3 CZO and 4g / ft 3 Rh.

[0203] 3. Add 0.92g / in 3 An additional amount of CZO slurry was added to make the total CZO equivalent to 1 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated on approximately 8% of the CZO carrier, while the remaining CZO carrier does not contain Rh. This mixture is then continuously blended.

[0204] 4. Blend the slurry with 4% La-Al2O3 slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0205] 5. Adjust the solids and thicken the carrier coating.

[0206] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0207] Reference catalyst 2

[0208] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 0.2% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0209] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 1.0 g / in. 3 La-Al2O3 and 4g / ft 3 Rh.

[0210] 3. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0211] 4. Adjust the solids and thicken the carrier coating.

[0212] 5. First, coat the substrate with the carrier coating (4) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0213] Invention Catalyst 4

[0214] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 0.75 wt%. The powder was dried overnight at 80 °C, calcined at 500 °C for 2 hours, and then ground.

[0215] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 0.3 g / in. 3 La-Al2O3 and 4g / ft 3 Rh.

[0216] 3. Add 0.7g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to 2 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated on approximately 31% of the La-Al2O3 carrier, while the remaining La-Al2O3 carrier does not contain Rh. This mixture is then continuously blended.

[0217] 4. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target yield of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0218] 5. Adjust the solids and thicken the carrier coating.

[0219] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0220] Invented Catalyst 5

[0221] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 1.5% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground with a mortar and pestle.

[0222] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 0.15 g / in. 3 La-Al2O3 and 4g / ft 3 Rh.

[0223] 3. Add 0.85g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to 2 (1.0 g / in) of the reference catalyst.3 In this carrier coating, Rh is locally concentrated on approximately 15% of the La-Al2O3 carrier, while the remainder of the La-Al2O3 carrier does not contain Rh. This mixture is then continuously blended.

[0224] 4. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target yield of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0225] 5. Adjust the solids and thicken the carrier coating.

[0226] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0227] Invention Catalyst 6

[0228] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve a 3% wt% Rh concentration. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0229] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 0.08 g / in. 3 La-Al2O3 and 4g / ft 3 Rh.

[0230] 3. Add 0.92g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to 2 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated on approximately 8% of the La-Al2O3 carrier, while the remainder of the La-Al2O3 carrier does not contain Rh. The carrier is then continuously mixed.

[0231] 4. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target yield of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0232] 5. Adjust the solids and thicken the carrier coating.

[0233] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0234] Reference catalyst 3

[0235] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 0.5% by weight. The powder was dried overnight at 80°C, calcined at 500°C for 2 hours, and then ground.

[0236] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 1.3 g / in. 3 La-Al2O3 and 10 g / ft 3 Rh.

[0237] 3. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0238] 4. Adjust the solids and thicken the carrier coating.

[0239] 5. First, coat the substrate with the carrier coating (4) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0240] Invention Catalyst 7

[0241] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 0.9 wt%. The powder was dried overnight at 80 °C, calcined at 500 °C for 2 hours, and then ground.

[0242] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 0.6 g / in. 3 La-Al2O3 and 10 g / ft 3 Rh.

[0243] 3. Add 0.6g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to the reference catalyst 3 (1.3 g / in). 3 In this carrier coating, Rh is locally concentrated on approximately 50% of the La-Al2O3 carrier, while the remaining La-Al2O3 carrier does not contain Rh. This mixture is then continuously blended.

[0244] 4. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target yield of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0245] 5. Adjust the solids and thicken the carrier coating.

[0246] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0247] Invention Catalyst 8

[0248] 1. Rh La-stabilized alumina pre-fixed powder was prepared by impregnating La-stabilized alumina (La-Al2O3) with a nitric acid Rh solution to achieve an Rh concentration of 1.9 wt%. The powder was dried overnight at 80 °C, calcined at 500 °C for 2 hours, and then ground with a mortar and pestle.

[0249] 2. The calculated amount of pre-fixed Rh La-Al2O3 powder was slurried, with a target yield of 0.3 g / in. 3 La-Al2O3 and 10 g / ft 3 Rh.

[0250] 3. Add 1.0g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to the reference catalyst 3 (1.3 g / in). 3 In this carrier coating, Rh is locally concentrated on approximately 25% of the La-Al2O3 carrier, while the remaining La-Al2O3 carrier does not contain Rh. This mixture is then continuously blended.

[0251] 4. Blend the slurry with a cerium dioxide-zirconia mixed oxide (CZO) slurry, with a target yield of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0252] 5. Adjust the solids and thicken the carrier coating.

[0253] 6. First, coat the substrate with the carrier coating (5) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0254] Reference catalyst 4

[0255] The underlying carrier coating is prepared by the following method:

[0256] 1. Grind and prepare a slurry containing 4% La2O3-doped alumina.

[0257] 2. Grind and prepare a slurry containing a mixture of cerium dioxide and zirconium oxide (CZO).

[0258] 3. Mix the two slurries together.

[0259] 4. Add barium hydroxide and palladium nitrate to the slurry (3).

[0260] 5. Adjust the solidity of the carrier coating (4) and thicken it with a rheology modifier.

[0261] 6. The final composition of the underlying carrier coating contains 1.0 g / in 3 La-Al2O3, 1.0 g / in 3 Cerium dioxide-zirconia composite, 400 g / ft 3 Ba element and 149g / ft 3 The Pd element.

[0262] 7. First, coat the substrate with the carrier coating (6) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0263] The top carrier coating is prepared by the following method:

[0264] 1. Grind and prepare a slurry containing La-stabilized alumina (La-Al2O3).

[0265] 2. Add the calculated amount of rhodium nitrate solution to the slurry (1), with a target of 1.0 g / in. 3 La-Al2O3 and 6 g / ft 3 Rh.

[0266] 3. The pH of the slurry (2) was increased to 6 to 7 with ammonia to obtain a local Rh concentration of 0.35%.

[0267] 4. Blend slurry (3) with pre-ground cerium dioxide-zirconia mixed oxide (CZO) slurry to a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0268] 5. Adjust the solidity of the carrier coating (4) and thicken it with a rheology modifier.

[0269] 6. The final composition of the top carrier coating contains 1.0 g / in 3 4% La2O3-doped alumina, 1.0 g / in3 Cerium dioxide-zirconia complex and 6 g / ft 3 The Rh element.

[0270] 7. First, apply the carrier coating (5) to the undercoated brick from one side, targeting a dose length of 50%-55%. Dry with hot air to 80% or more moisture content. Then coat the other side, targeting a dose length of 50%-55%, and then dry and calcine again to obtain the final catalyst.

[0271] Inventive catalyst 9 (for example, see Figure 2b )

[0272] The underlying support coating was prepared and coated in the same manner as the reference catalyst 4. Figure 2b (The second catalytic region in the middle).

[0273] Top carrier coating ( Figure 2b The first catalytic region in the sample is prepared by the following method:

[0274] 1. Grind and prepare a slurry containing La-stabilized alumina (La-Al2O3).

[0275] 2. Add the calculated amount of rhodium nitrate solution to the slurry (1), with a target concentration of 0.35 g / in. 3 La-Al2O3 and 6 g / ft 3 Rh.

[0276] 3. Increase the pH of the slurry (2) to 6 or 7 with ammonia.

[0277] 4. Add 0.65g / in 3 An additional amount of La-Al2O3 slurry was added to make the total La-Al2O3 equivalent to 4 (1.0 g / in) of the reference catalyst. 3 In this carrier coating, Rh is locally concentrated at a concentration of 1% on approximately 35% of the La-Al2O3 carrier, while the remaining La-Al2O3 carrier does not contain Rh. The mixture is then continuously stirred.

[0278] 5. Blend the slurry (4) with a pre-ground cerium dioxide-zirconia mixed oxide (CZO) slurry to a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0279] 6. Adjust the solidity of the carrier coating (5) and thicken it with a rheology modifier.

[0280] 7. The final composition of the top support coating is the same as that of reference catalyst 4, containing 1.0 g / in 3 4% La2O3-doped alumina, 1.0 g / in 3Cerium dioxide-zirconia complex and 6 g / ft 3 The Rh element.

[0281] 8. First, apply the carrier coating (7) to the undercoated brick from one side, targeting a dose length of 50%-55%. Dry with hot air to 80% or more moisture content. Then coat the other side, targeting a dose length of 50%-55%, and then dry and calcine again to obtain the final catalyst.

[0282] The inventive catalyst 10 has a partitioned formulation (see, for example, see...) Figure 4d )

[0283] The underlying support coating was prepared and coated in the same manner as the reference catalyst 4. Figure 4d (The third catalytic region in the middle).

[0284] The top layer of the inventive catalyst 10 has a partitioned formulation.

[0285] The inlet region support coating was prepared in the same manner as the top support coating of reference catalyst 4. Figure 4d (The second catalytic region in the process). Then, the carrier coating is applied to the undercoated brick from the inlet side, targeting a dose length of 50%-55%. It is then dried with hot air to 80% or more moisture content.

[0286] The outlet region support coating was prepared in the same manner as the top support coating of the invented catalyst 9. Figure 4d The first catalytic region is then formed. The support coating is then applied to the underlying coated brick from the outlet side, targeting a dose length of 50%-55%. The brick is dried with hot air to 80% or more moisture content. Finally, the brick is calcined to obtain the final catalytic product.

[0287] The inventive catalyst 11 has a partitioned formulation (see, for example, see...) Figure 4d )

[0288] The underlying support coating was prepared and coated in the same manner as the reference catalyst 4. Figure 4d (The third catalytic region in the middle).

[0289] The top layer of the inventive catalyst 11 has a partitioned formulation.

[0290] The inlet region support coating was prepared in the same manner as the top support coating of reference catalyst 4. Figure 4d (The second catalytic region in the process). Then, the carrier coating is applied to the undercoated brick from the inlet side, targeting a dose length of 50%-55%. It is then dried with hot air to 80% or more moisture content.

[0291] Export area carrier coating ( Figure 4d The first catalytic region in the sample is prepared by the following method:

[0292] 1. Grind and prepare a slurry containing a cerium dioxide-zirconia mixed oxide (CZO).

[0293] 2. Add the calculated amount of rhodium nitrate solution to the slurry (1), with a target concentration of 0.35 g / in. 3 CZO and 6g / ft 3 Rh.

[0294] 3. Increase the pH of the slurry (2) to 6 or 7 with ammonia.

[0295] 4. Add 0.65g / in 3 An additional amount of cerium dioxide-zirconia mixed oxide (CZO) slurry was added to make the total cerium dioxide-zirconia mixed oxide (CZO) equivalent to reference catalyst 4 (1.0 g / in). 3 In this carrier coating, Rh is locally concentrated at a concentration of 1% on approximately 35% of the cerium dioxide-zirconia mixed oxide (CZO) carrier, while the remaining cerium dioxide-zirconia mixed oxide (CZO) carrier does not contain Rh. This mixture is continuously blended.

[0296] 5. Blend slurry (4) with pre-ground La-Al2O3 slurry to a target concentration of 1.0 g / in. 3 Load capacity. Mix it continuously.

[0297] 6. Adjust the solidity of the carrier coating (5) and thicken it with a rheology modifier.

[0298] 7. The final composition of the top support coating is the same as that of reference catalyst 4, containing 1.0 g / in 3 4% La2O3-doped alumina, 1.0 g / in 3 Cerium dioxide-zirconia complex and 6 g / ft 3 The Rh element.

[0299] 8. Then, the carrier coating (7) is applied to the undercoated brick from the outlet side, targeting a dose length of 50%-55%. It is dried with hot air to 80% or more moisture content. Finally, the brick is calcined to obtain the final catalyst product.

[0300] Reference catalyst 5

[0301] The underlying carrier coating is prepared by the following method:

[0302] 1. Grind and prepare a slurry containing 4% La2O3-doped alumina.

[0303] 2. Grind and prepare a slurry containing a mixture of cerium dioxide and zirconium oxide (CZO).

[0304] 3. Mix the two slurries together.

[0305] 4. Add barium hydroxide and palladium nitrate to the slurry (3).

[0306] 5. Adjust the solidity of the carrier coating (4) and thicken it with a rheology modifier.

[0307] 6. The final composition of the underlying carrier coating contains 0.9 g / in 3 La-Al2O3, 0.9 g / in 3 Cerium dioxide-zirconia composite, 300 g / ft 3 Ba element and 36g / ft 3 The Pd element.

[0308] 7. First, coat the substrate with the carrier coating (6) from one side, targeting 50%-55% of the dose length. Dry with hot air to 80% or more moisture content. Then coat the other side of the substrate, targeting 50%-55% of the dose length, followed by drying and calcination.

[0309] The top carrier coating is prepared by the following method:

[0310] 1. Grind and prepare a slurry containing La-stabilized alumina (La-Al2O3).

[0311] 2. Grind and prepare a slurry containing a mixture of cerium dioxide and zirconium oxide (CZO).

[0312] 3. Mix the two slurries together, keeping the weight ratio of La-Al2O3 to CZO at 1:3.

[0313] 4. Add the calculated amount of rhodium nitrate solution to the slurry (3), with a target of 0.4 g / in. 3 La-Al2O3, 1.1 g / in 3 CZO and 4g / ft 3 Rh.

[0314] 5. Increase the pH of the slurry (4) to 6 or 7 with ammonia to obtain a local Rh concentration of 0.15%.

[0315] 6. Adjust the solidity of the carrier coating (5) and thicken it with a rheology modifier.

[0316] 7. The final composition of the top carrier coating contains 1.0 g / in 3 4% La2O3-doped alumina, 1.0 g / in 3 Cerium dioxide-zirconia complex and 6 g / ft 3 The Rh element.

[0317] 8. First, apply the carrier coating (5) to the undercoated brick from one side, targeting a dose length of 50%-55%. Dry with hot air to 80% or more moisture content. Then coat the other side, targeting a dose length of 50%-55%, and then dry and calcine again to obtain the final catalyst.

[0318] Invention catalyst 12 (for example, see Figure 2b )

[0319] The underlying support coating was prepared and coated in the same manner as the reference catalyst 5. Figure 2b (The second catalytic region in the middle).

[0320] Top carrier coating ( Figure 2b The first catalytic region in the sample is prepared by the following method:

[0321] 1. Grind and prepare a slurry containing La-stabilized alumina (La-Al2O3).

[0322] 2. Grind and prepare a slurry containing a mixture of cerium dioxide and zirconium oxide (CZO).

[0323] 3. Mix the two slurries together, keeping the weight ratio of La-Al2O3 to CZO at 1:3.

[0324] 4. Add the calculated amount of rhodium nitrate solution to a portion of the slurry (3), with a target concentration of 0.2 g / in. 3 La-Al2O3, 0.6 g / in 3 CZO and 4g / ft 3 The Rh. The resulting slurry is continuously mixed.

[0325] 5. The pH of the slurry (4) was increased to 6 to 7 with ammonia for Rh hydrolysis, yielding a local Rh concentration of 0.31%. It was then continuously mixed.

[0326] 6. Add 0.2g / in 3 La-Al2O3 slurry and 0.6 g / in 3 An additional amount of slurry 3 of CZO slurry was added to make the total La-Al2O3 and CZO equivalent to the reference catalyst 5 (1.0 g / in). 3 In this carrier coating, Rh is locally concentrated at a concentration of 0.3% on approximately 50% of the mixed La-Al2O3 and CZO carriers, and the remaining portion of the mixed La-Al2O3 and CZO carriers does not contain Rh. This mixture is continuously mixed.

[0327] 7. Adjust the solidity of the carrier coating (5) and thicken it with a rheology modifier.

[0328] 8. The final composition of the top support coating is the same as that of reference catalyst 5, containing 0.4 g / in 3 4% La2O3-doped alumina, 1.1 g / in 3 Cerium dioxide-zirconia complex and 4 g / ft 3 The Rh element.

[0329] 9. First, apply the carrier coating (7) to the undercoated brick from one side, targeting a dose length of 50%-55%. Dry with hot air to 80% or more moisture content. Then coat the other side, targeting a dose length of 50%-55%, and then dry and calcine again to obtain the final catalyst.

[0330] Invention catalyst 13 (see, for example, see Figure 2b )

[0331] The underlying support coating was prepared and coated in the same manner as the reference catalyst 4. Figure 2b (The second catalytic region in the middle).

[0332] Top carrier coating ( Figure 2b The first catalytic region in the sample is prepared by the following method:

[0333] 1. Grind and prepare a slurry containing La-stabilized alumina (La-Al2O3).

[0334] 2. Grind and prepare a slurry containing a mixture of cerium dioxide and zirconium oxide (CZO).

[0335] 3. Mix the two slurries together, keeping the weight ratio of La-Al2O3 to CZO at 1:3.

[0336] 4. Add the calculated amount of rhodium nitrate solution to a portion of the slurry (3), with a target concentration of 0.1 g / in. 3 La-Al2O3, 0.3 g / in 3 CZO and 4g / ft 3 The Rh. The resulting slurry is continuously mixed.

[0337] 5. The pH of the slurry (4) was increased to 6 to 7 with ammonia for Rh hydrolysis, yielding a local Rh concentration of 0.6%. It was then continuously mixed.

[0338] 6. Add 0.3g / in 3 La-Al2O3 slurry and 0.8 g / in 3 An additional amount of slurry 3 of CZO slurry was added to make the total La-Al2O3 and CZO equivalent to the reference catalyst 5 (1.5 g / in). 3In this carrier coating, Rh is locally concentrated at a concentration of 0.6% on approximately 25% of the mixed La-Al2O3 and CZO carrier, and the remainder of the mixed La-Al2O3 and CZO carrier does not contain Rh. This mixture is continuously mixed.

[0339] 7. Adjust the solidity of the carrier coating (5) and thicken it with a rheology modifier.

[0340] 8. The final composition of the top support coating is the same as that of reference catalyst 5, containing 0.4 g / in 3 4% La2O3-doped alumina, 1.2 g / in 3 Cerium dioxide-zirconia complex and 4 g / ft 3 The Rh element.

[0341] 9. First, apply the carrier coating (7) to the undercoated brick from one side, targeting a dose length of 50%-55%. Dry with hot air to 80% or more moisture content. Then coat the other side, targeting a dose length of 50%-55%, and then dry and calcine again to obtain the final catalyst.

[0342] All catalysts are listed in Table 1 along with their corresponding local Rh concentrations, target supports, and total Rh loadings.

[0343] Table 1: Summary of all catalysts

[0344]

[0345] Example 1: FE-EPMA analysis of the interaction between RH and ZR or AL

[0346] Characterizing Rh nanoparticles at very low Rh loadings is a highly challenging task. HRTEM is currently the most commonly used technique. However, due to the extremely fine Rh particle size, identifying these particles is difficult, and the standard deviation (error) is substantial. Furthermore, if Rh is loaded onto CZO, the contrast between Rh and Zr is very close, making it impossible to distinguish Rh particles from the support. H2-TPR is another commonly used technique for measuring Rh-support interactions or the "relative" particle size of Rh. However, both Rh and Ce can be simultaneously reduced by H2, making it impossible to separate them from each other. For CO chemisorption methods, CO can only chemisorb Rh in Rh / Al2O3 and Rh / CzO. 0On unreduced Rh samples, CO absorption is negligible. Typically, the Rh material in the prepared TWC catalyst is in an oxidized state (Rh₂O₃), meaning it is impossible to measure the prepared Rh dispersion by CO chemisorption. Measuring CO chemisorption on Rh / CZO can lead to an overestimation of metal particle dispersion due to the formation of carbonate material even at low temperatures (323 K) on the CeO₂ surface and the possibility of multiple CO molecules adsorbing on the Rh itself. In this invention, an efficient method for detecting Rh on CZO or La-Al₂O₃ supports at very low loadings (0.23% on a single support or 4 g / ft in TWC formulations) has been developed. 3 Dispersion methods.

[0347] The Pearson correlation coefficient (product-moment correlation coefficient) is calculated based on the results of area analysis performed by FE-EPMA, and the Rh-Zr or Rh-Al correlation coefficients are listed in Table 2.

[0348] With 4 g / ft pre-fixed on all CZO carriers 3 The reference catalyst 1 for Rh showed a high coefficient of 0.5, indicating very high Rh dispersion and very fine Rh particles. In contrast, the inventive catalysts 1 and 2 exhibited lower Rh-Zr coefficients than the reference catalyst 1. This means that even with the same total Rh loading, the Rh particle size can be successfully increased by concentrating Rh on a portion of 31% or 15% of the CZO support, respectively. Further increasing the local Rh concentration to 3% by fixing Rh to 7.7% of the total CZO material resulted in a significantly low Rh-Zr coefficient of 0.17. In this case, Rh is over-concentrated and the Rh dispersion is too low. It is assumed that some Rh atoms may not be used due to being buried inside the Rh particles. Figure 28 The concept is illustrated well in the text.

[0349] 4 g / ft of material pre-fixed on a La-Al2O3 support 3 Similar trends in Rh local concentration and Rh-Al Pearson correlation coefficients were observed on the reference catalyst 2 and the inventive catalysts 4, 5, and 6. Locally concentrating Rh to 3% (inventive catalyst 6) by immobilizing Rh on 7.7% of the total La-Al₂O₃ material resulted in a significantly low Rh-Al coefficient of 0.17. In this case, Rh was over-concentrated and the Rh dispersion was too low. It is hypothesized that some Rh atoms may not be used due to being buried inside the Rh particles. In contrast, by concentrating Rh on a 15% La-Al₂O₃ support, inventive catalyst 5 exhibited a reasonable Pearson correlation coefficient of 0.43, presumably leading to optimal Rh nanoparticle size or Rh dispersion.

[0350] When the total Rh load increases to 10 g g / ft 3 At this point, the relationship between the local Rh concentration and the Pearson correlation coefficient becomes much flatter, as demonstrated by reference catalyst 3, inventive catalyst 7, and inventive catalyst 8, where the Pearson correlation coefficient stabilizes between 0.38 and 0.36 as the local Rh concentration increases from 0.46% to 1.86%. This technique is not sensitive enough at high Rh loadings.

[0351] Table 2: Pearson correlation coefficients obtained by EPMA

[0352]

[0353] Example 2: Ignition performance test in engine testing

[0354] All catalysts were bench-aged for 100 hours using a stoichiometric / fuel cutoff aging cycle targeting a catalyst bed peak temperature of 1000°C, and then tested on a gasoline engine. Ignition performance was assessed under typical conditions, with a gas hourly space velocity (VHSV) of 216 K / hr, a temperature ramp of 20°C / min, and an air-fuel ratio (AFR) λ perturbed at 14.56 with an amplitude of 0.5 and a frequency of 1 Hz. The catalyst inlet temperature was then reduced until THC, CO, and NO were reduced. x Conversion rate less than 10%. Stabilize for 2 minutes. Increase catalyst inlet temperature by 20°C per minute until the inlet temperature reaches 500°C. Calculate NO by comparing the concentrations of the feed gas and the catalyst outlet gas. x Conversion rates of CO and THC.

[0355] T 50 This is the temperature at which the conversion rate reaches 50%, and it is commonly used to compare catalytic performance. T 50 The lower the T value, the better the catalyst. The T values ​​for all catalysts... 50 The ignition temperatures are listed in Table 3. This data clearly shows that, compared to reference catalyst 1, both inventive catalyst 1 and inventive catalyst 2 significantly improve ignition performance. These two catalysts exhibit improved ignition performance for NO. x T about 30°C lower 50 For T, where CO is about 33°C lower 50 And for THC that is about 30°C lower 50 Therefore, the optimal size of Rh particles can be more resistant to sintering and migration, resulting in earlier ignition performance. However, over-concentration of Rh in the inventive catalyst 3 begins to degrade catalytic activity, where the conversion of all three contaminants is delayed by about 25°C compared to the inventive catalysts 1 and 2, but is still improved compared to the reference catalyst 1.

[0356] 4 g / ft of material pre-fixed on a La-Al2O3 support 3Similar ignition performance benefits were observed on the reference catalyst 2 and the inventive catalysts 4, 5, and 6. When Rh was locally concentrated on a portion of 31% or 15% of the La-Al2O3 support, the inventive catalysts 4 and 5 clearly showed significantly improved ignition performance compared to the reference catalyst 2, likely due to the optimal size of the Rh particles, which are more resistant to sintering and migration. However, again, the over-concentration of Rh in the inventive catalyst 3 began to reduce the conversion rates of all three contaminants compared to the inventive catalysts 1 and 2, but was still improved compared to the reference catalyst 1.

[0357] Interestingly, when the total Rh load is 10g / ft 3 At that time, compared with reference catalyst 3, the inventive catalyst 7 did not show any benefit in ignition performance. For the ignition test conditions, the Rh particle size / Rh dispersion was probably already at an optimal level in reference catalyst 3 with a local Rh concentration of 0.46%. Further concentrating Rh to 1.86% in the inventive catalyst 8 became detrimental.

[0358] Table 3: Engine bench ignition test results

[0359]

[0360] Example 3: Lamb scan test in engine testing

[0361] All catalysts were aging on an engine bench for 100 hours using a stoichiometric / fuel cutoff aging cycle targeting a catalyst bed peak temperature of 1000°C, and then tested on a gasoline engine. The λ-scan test was typical under the following conditions: gas volume hourly space velocity (VHSV) of 216 K / hr, temperature fixed at 400°C, and the air-fuel ratio (AFR) λ-perturbed by an amplitude of 0.5 during the scan, decreasing from 15.5 to 13.5. THC, CO, and NO were calculated by comparing the concentrations of the feed gas and the gas at the catalyst outlet. x Conversion rate.

[0362] CO and NO x The conversion rate trace is shown in Figure 7 The data clearly indicate that both the inventive catalyst 1 and the inventive catalyst 2 of this invention provide significantly improved NO content across the entire range of λ conditions. x Conversion rate and CO conversion rate. The THC conversion rate trace is shown in... Figure 8 Both Inventive Catalyst 1 and Inventive Catalyst 2 are more active than Reference Catalyst 1, exhibiting higher THC conversion rates across the entire λ condition range. The improved activity of the Inventive Catalysts is believed to be related to the optimal size of the Rh particles, thus making them more resistant to sintering and migration, resulting in performance benefits. However, over-concentration of Rh in Inventive Catalyst 3 begins to degrade catalytic activity, where NO concentration is significantly lower than that of Inventive Catalysts 1 and 2.x The conversion rates of CO and THC decreased significantly, but were still improved compared to reference catalyst 1.

[0363] 4 g / ft of material pre-fixed on a La-Al2O3 support 3 Similar λ-scan performance benefits were observed on Rh reference catalyst 2 and the invented catalysts 4-6. (CO and NO) x The conversion rate trace is shown in Figure 9 The THC conversion trace is shown in the middle. Figure 10 In the middle. When Rh was locally concentrated on a portion of 31% or 15% of the La-Al2O3 support, respectively, the invented catalysts 4 and 5 clearly showed NO across the entire λ range compared to reference catalyst 2. x The significantly improved conversion rates of CO and THC are likely due to the optimal size of the Rh particles, which are more resistant to sintering and migration. However, again, compared to inventive catalysts 4 and 5, the over-concentrated Rh in inventive catalyst 6 begins to reduce the conversion rates of all three contaminants, but is still improved compared to reference catalyst 2.

[0364] When the total load of Rh is 10g / ft 3 At that time, compared with reference catalyst 3, neither the inventive catalyst 7 nor the inventive catalyst 8 showed any benefit in λ-scan performance. CO and NO x The conversion rate trace is shown in Figure 11 The THC conversion trace is shown in the middle. Figure 12 In the λ scan test conditions, the Rh particle size / Rh dispersion was likely already optimal in reference catalyst 3 with a local Rh concentration of 0.46%. Further concentration of Rh in the inventive catalysts 7 or 8 to 0.93% or 1.86% became detrimental to the λ scan test at 400°C.

[0365] Example 4: Thermal RDE Test in Engine Testing

[0366] Targeting a peak catalyst bed temperature of 1000°C, all catalysts were bench-aged for 100 hours using a stoichiometric / fuel cut-off aging cycle. The catalysts were tested using a 2.0L engine bench dynamometer that performed a custom-designed OEM-designed Real-World Driving (RDE) cycle, including acceleration and fuel cut-off conditions representing speed stages in cold city, highway, and hot city conditions. The cycle time from ambient immersion conditions was 2700 seconds, reaching a peak catalyst bed temperature of approximately 650°C and a mass airflow rate of 250 kg / h. A cold RDE test was used as a preconditioning cycle. Subsequently, three hot RDE cycles were repeated, with 5-minute immersion periods in between. The engine was at operating temperature, but the catalyst bed temperature remained hot. The advantage of running the hot RDE with a cold RDE as a precondition is the excellent reproducibility of engine emissions. NO was measured at the catalytic converter location. x The emissions of CO and THC were calculated, and the cumulative mass of each substance throughout the cycle was calculated. The following graph plots and shows the relationship between the average value of three thermal RDE runs and time.

[0367] Figure 13 NO levels during thermal RDE cycles were compared between reference catalyst 1 and inventive catalysts 1-3. x Emissions. The data clearly show that the inventive catalyst 2 of this invention provides the most significant performance improvement compared to reference catalyst 1, which exhibits approximately 5g lower tailpipe NO. x Emissions. The optimal size of Rh particles at a local Rh concentration of 1.5% is therefore the most resistant to sintering and migration, resulting in minimal NO emissions. x Emissions. However, compared to the inventive catalyst 2, less Rh concentration in the inventive catalyst 1 or excessive Rh concentration in the inventive catalyst 3 degrades catalytic activity, resulting in approximately 2.5 or 3.5 g or more of NO. x Emissions are lower than those of reference catalyst 1, but still less. CO and THC emissions are shown in [data missing]. Figure 14 and Figure 15 Compared to reference catalyst 1, both inventive catalyst 1 and inventive catalyst 2 clearly show significantly improved performance, likely due to the optimal size of the Rh particles, which are more resistant to sintering and migration. However, again, compared to inventive catalyst 1, the over-concentrated Rh in inventive catalyst 3 begins to reduce the conversion rates of CO and THC.

[0368] 4 g / ft of material pre-fixed on a La-Al2O3 support 3Similar performance benefits were observed on the reference catalyst 2 and the inventive catalysts 4-6 for Rh. When Rh was locally concentrated on a portion of 31% or 15% of the La-Al2O3 support, respectively, the inventive catalysts 4 and 5 clearly showed significantly improved CO2 concentrations compared to the reference catalyst 2. Figure 17 ) and THC ( Figure 18 Emission control is possible due to the optimal size of the Rh particles, which are more resistant to sintering and migration. However, compared to inventive catalysts 4 and 5, over-concentration of Rh in inventive catalyst 6 begins to degrade performance. Figure 16 As shown, NO for all three Rh concentrate formulations x Emissions controls still offer benefits, but they are not as pronounced as those for CO and THC.

[0369] Surprisingly, when the total Rh load increased to as high as 10g / ft 3 At the same time, compared with reference catalyst 3, the invented catalysts 7 and 8 still showed good performance against CO ( ). Figure 20 ) and THC ( Figure 21 It offers the benefits of emission control, but has NO levels comparable to reference catalyst 3. x ( Figure 19 )emission.

[0370] Example 5: Cold RDE Test in Engine Testing

[0371] Targeting a peak catalyst bed temperature of 1000°C, all catalysts were bench-aged for 100 hours using a stoichiometric / fuel cut-off aging cycle. The catalysts were tested using a 2.0L twin-turbo, 4-cylinder, Eu(VI)b-calibrated bench dynamometer that performed a custom OEM-designed Real-World Driving (RDE) cycle, including acceleration and fuel cut-off conditions representing cold-start city, highway, and hot city speed stages. At a vehicle speed of approximately 140 km / hr and a mass airflow of approximately 400 kg / hr, the cycle time from ambient immersion conditions was 2700 seconds, reaching a peak catalyst temperature of approximately 700°C. NOx, CO, and THC emissions were measured at the post-catalyst location, and the cumulative mass of each substance over the entire cycle was calculated. Each catalyst formulation was tested three times, and the average of the three tests versus time is plotted and shown in the figure below.

[0372] Figure 22 NO during cold RDE cycles of reference catalyst 4 and the invented catalyst 9-11 x Emissions. It is quite clear that the inventive catalyst 10, with its partitioned configuration of 1% Rh concentrated on La-Al2O3 in the rear zone, delivers the lowest NO emissions throughout the entire cold RDE driving cycle. xEmissions. Other formulations, such as the inventive catalyst 9 with a uniform distribution of 1% Rh concentrated on La-Al2O3 in the top layer, or the inventive catalyst 11 with a partitioned configuration but with 1% Rh concentrated on CZO in the back zone, appear to be equivalent to the reference catalyst 4. CO and THC emissions are shown respectively in Figure 23 and Figure 24 In the meantime, although the levels differ slightly, all variants of the Rh allocation are superior to the references for CO or THC emission controls.

[0373] Example 6: WLTC Test in Engine Testing

[0374] Targeting a peak catalyst bed temperature of 1000°C, all catalysts were bench-aged for 100 hours using a stoichiometric / fuel cut-off aging cycle. The catalysts were tested using a 2.0L twin-turbo, 4-cylinder, Eu(VI)b calibrated bench dynamometer performing the World Harmonized Light Vehicles Test Cycle (WLTC), which includes acceleration and fuel cut-off conditions representing urban, rural, highway, and expressway speed stages. At an engine speed of approximately 130 km / h and a mass airflow of approximately 200 kg / h, the cycle time from ambient immersion conditions was 1800 seconds, reaching a peak catalyst temperature of approximately 600°C. NO₂ was measured at the catalyst bed location. x Emissions of CO and THC were measured, and the cumulative mass of each substance over the entire cycle was calculated. Three trials were conducted for each catalyst formulation, and the average value of the three trials versus time is plotted and shown in the figure below.

[0375] Figure 25 NO during WLTC cycle is compared with reference catalyst 4 and the invention catalyst 9-11. x Emissions. Inventive catalyst 10 (with a partitioned configuration of 1% Rh concentrated on La-Al2O3 in the rear zone) and inventive catalyst 11 (with a partitioned configuration of 1% Rh concentrated on CZO in the rear zone) performed equally well, both delivering the lowest NO emissions throughout the WLTC driving cycle. x Emissions. The uniform distribution of 1% Rh concentrated on La-Al2O3 in the inventive catalyst 9 appears to be equivalent to that of the reference catalyst 4. CO and THC emissions are shown respectively in Figure 26 and Figure 27 In the meantime, although the levels differ slightly, all variants of the Rh allocation are superior to the references for CO or THC emission controls.

[0376] Example 7: Vehicle Testing

[0377] Bench-aged samples of the inventive catalysts 12 and 13, as well as the comparative catalyst 5, were tested in a vehicle with a 1.5-liter engine using the Worldwide Light Vehicles Test Procedure (WLTP). Bench aging was performed for 150 hours in the same operation with a 6.1-liter engine using a four-mode aging cycle, with the peak bed temperature of the catalyst reaching approximately 980°C. The results of the vehicle exhaust gas dilution bag data for the bench-aged portion are shown in Table 4. Compared to the comparative catalyst 5, the inventive catalysts 12 and 13 of the present invention exhibit superior activity for THC and NMHC emission control. (For example, see THC and NMHC performance improvements of approximately 11% and 12%, respectively, compared to the comparative catalyst 5).

[0378] Table 4: Emissions Results Based on Vehicle Dilution Bag Data

[0379]

[0380] Example 8: Ignition performance test in engine testing

[0381] The invented catalysts 12 and 13, along with the comparative catalyst 5, were bench-aged on a gasoline engine. Ignition performance was tested under typical conditions, with an exhaust gas velocity of 80 kg / hr, a temperature ramp of 30 °C / min, and an air-fuel ratio (AFR) λ of 14.45. THC and CO conversion rates were calculated by comparing the concentrations of the feed gas and the gas at the catalyst outlet. Prior to engine ignition testing, the invented catalysts 12 and 13, along with the comparative catalyst 5, were bench-aged for 150 hours under the same conditions. Bench aging was performed for 150 hours on a 6.1L engine using a four-mode aging cycle, with the peak bed temperature of the catalyst reaching approximately 980 °C.

[0382] Invented catalysts 12 and 13 and comparative catalyst 5 for HC, CO and NO x T 50 Ignition temperature (T) 50 The temperature at which the conversion rate reaches 50% is shown in Table 5. The data indicate that the invented catalysts 12 and 13 exhibit good performance in reducing HC, CO, and NO. x Improved ignition performance. Compared to comparative catalyst 5 (e.g., NO on inventive catalyst 13) x T of CO and HC 50 (The temperatures were reduced by 13°C, 11°C, and 8°C, respectively).

[0383] Table 5: Engine bench ignition test results

[0384]

[0385] The detailed description above has been provided by way of explanation and illustration and is not intended to limit the scope of the appended claims. Many variations of the presently preferred embodiments shown herein will be apparent to those skilled in the art and remain within the scope of the appended claims and their equivalents.

Claims

1. A catalyst article for treating waste gas, comprising: A substrate, the substrate including an inlet end and an outlet end, having an axial length L; A first catalytic region, the first catalytic region comprising support material particles; At least some of the said support material particles are rhodium-loaded support material particles on which rhodium is loaded, and the concentration of rhodium is from 0.001% to 3.5% by weight based on the weight of the rhodium-loaded support material particles; and the rhodium relative to the first catalytic region is at a concentration of up to 20 g / ft. 3 The load capacity exists. At least some of the carrier material particles are unloaded carrier material particles, and based on the weight of the unloaded carrier material particles, the unloaded carrier material particles have rhodium loaded thereon at a concentration of less than 0.001% by weight.

2. The catalyst article according to claim 1, wherein, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.3% to 3.5% by weight.

3. The catalyst article according to claim 1, wherein, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.4% to 3.0% by weight.

4. The catalyst article according to claim 1, wherein, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.4% to 2.0% by weight.

5. The catalyst article according to claim 1, wherein, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.4% to 1.5% by weight.

6. The catalyst article according to any one of claims 1-5, wherein 5% to 80% of the support material particles in the first catalytic region are rhodium-supported support material particles.

7. The catalyst article according to claim 6, wherein 15% to 35% of the support material particles in the first catalytic region are rhodium-supported support material particles.

8. The catalyst article according to any one of claims 1-5, wherein the carrier material particles comprise alumina and / or a cerium dioxide-zirconia mixed oxide.

9. The catalyst product according to claim 8, wherein the alumina and / or cerium dioxide-zirconia mixed oxide is doped.

10. The catalyst article according to claim 9, wherein the alumina and / or cerium dioxide-zirconia mixed oxide is doped with an oxide of one or more of the following substances: lanthanum, neodymium, yttrium, niobium, praseodymium, hafnium, molybdenum, titanium, vanadium, zinc, cadmium, manganese, iron, copper, calcium, barium, strontium, cesium, magnesium, potassium and sodium.

11. The catalyst article according to claim 9, wherein the alumina and / or cerium dioxide-zirconia mixed oxide is doped with an oxide of one or more of lanthanum, neodymium, and yttrium.

12. The catalyst article according to claim 10 or 11, wherein the dopant is present in the alumina and / or cerium dioxide-zirconia mixed oxide in an amount of 0.001% to 20% by weight.

13. The catalyst article according to claim 10 or 11, wherein the dopant is present in the alumina and / or cerium dioxide-zirconia mixed oxide in an amount of 0.5% to 10% by weight.

14. The catalyst article according to any one of claims 1-5, wherein the support material particles have a density of 0.1 µm to 25 µm. 90 .

15. The catalyst article according to any one of claims 1-5, wherein the support material particles have a density of 0.5 µm to 5 µm. 90 .

16. The catalyst article according to any one of claims 1-5, wherein the support material particles comprise a cerium dioxide-zirconia mixed oxide; and When performing area analysis of the cross-section of the first catalytic region of the catalyst article using FE-EPMA under the conditions of a pixel size of 0.34µm × 0.34µm and a pixel number measured in a 256 × 256 cross-section, the α characteristic X-ray intensity of zirconium (Zr) in cps and the β characteristic X-ray intensity of rhodium (Rh) in cps are measured for each pixel, and the Pearson correlation coefficient calculated using the obtained α and β in each pixel is designated as R. Zr / Rh At that time R Zr / Rh The value ranges from 0.15 to 0.

48.

17. The catalyst article according to claim 16, wherein R Zr / Rh The value is between 0.3 and 0.

45.

18. The catalyst article according to any one of claims 1-5, wherein the rhodium is present at a rate of 1 g / ft relative to the first catalytic region. 3 Up to 20g / ft 3 The capacity exists.

19. The catalyst article according to any one of claims 1-5, wherein the carrier material particles are at a concentration of 0.5 g / in 3 Up to 3g / in 3 The capacity exists.

20. The catalyst article according to any one of claims 1-5, further comprising a second catalytic region.

21. The catalyst article of claim 20, wherein the second catalytic region comprises a second PGM component.

22. The catalyst article of claim 21, wherein the second PGM component is selected from the group consisting of platinum, palladium, rhodium, and mixtures thereof.

23. The catalyst article of claim 20, wherein the second catalytic region further comprises a second OSC material and / or a second inorganic oxide.

24. The catalyst article according to any one of claims 1-5, wherein the first catalytic region extends the axial length L.

25. The catalyst article of claim 20, wherein the second catalytic region extends the axial length L.

26. The catalyst article according to any one of claims 1-5, wherein the first catalytic region is directly supported / deposited on the substrate.

27. The catalyst article of claim 20, wherein the second catalytic region is directly supported / deposited on the substrate.

28. The catalyst article according to claim 20, further comprising a third catalytic region.

29. The catalyst article of claim 28, wherein the third catalytic region comprises a third PGM component.

30. The catalyst article according to claim 29, wherein the third catalytic region further comprises a third OSC material and / or a third inorganic oxide.

31. The catalyst article according to any one of claims 1-5, wherein the first catalytic region further comprises platinum and / or palladium.

32. The catalyst article according to any one of claims 1-5, wherein the catalyst article is used in a three-way catalytic converter.

33. The catalyst article according to any one of claims 1-5, wherein the substrate comprises a wall-flow filter substrate.

34. The catalyst article according to any one of claims 1 to 5, wherein the substrate comprises a flow-through substrate.

35. A method for manufacturing a catalyst article, the method comprising: Provided are rhodium-loaded carrier material particles loaded thereon, wherein the rhodium concentration is from 0.001% to 3.5% by weight based on the weight of the rhodium-loaded carrier material particles. Provide unloaded carrier material particles, which, based on the weight of the unloaded carrier material particles, have rhodium loaded thereon at a concentration of less than 0.001% by weight. A carrier coating comprising the rhodium-loaded carrier material particles and the unloaded carrier material particles is formed; as well as The substrate is coated with the carrier coating to provide a catalyst article, wherein the rhodium relative to the substrate is at a concentration of up to 20 g / ft. 3 The capacity exists.

36. The method of claim 35, wherein, based on the weight of the rhodium-supported material particles, the rhodium-supported material particles have rhodium loaded thereon at a concentration of 0.3% to 3.5% by weight.

37. The method of claim 35 or 36, further comprising adding an adhesive to the carrier coating prior to coating the substrate with the carrier coating.

38. The method of claim 35 or 36, wherein providing the rhodium-loaded carrier material particles comprises loading rhodium onto the carrier material particles using initial wet impregnation.

39. The method of claim 38, wherein providing the rhodium-supported material particles further includes drying and calcining the rhodium-supported material particles.

40. The method according to claim 35 or 36, wherein the catalyst article is any one of claims 1 to 34.

41. A catalyst article, said catalyst article being obtained by or being obtainable by any one of claims 35 to 40.

42. An emission treatment system comprising a catalyst article according to any one of claims 1 to 34 and claim 41.

43. The emission treatment system of claim 42, wherein the emission treatment system is used for a gasoline engine.

44. The emission treatment system of claim 43, wherein the gasoline engine operates under stoichiometric conditions.

45. A method for treating waste gas, the method comprising: Provide a catalyst article according to any one of claims 1 to 34 and claim 41; as well as The catalyst product is brought into contact with the waste gas.

46. ​​The method of claim 45, wherein the exhaust gas originates from a gasoline engine.

47. The method of claim 46, wherein the gasoline engine operates under stoichiometric conditions.

Citation Information

Patent Citations

  • Platinum group metal (PGM) catalysts for automotive emissions treatment

    WO2016123534A1

  • Base metal doped zirconium oxide catalyst support materials

    US20210348534A1