A high wear-resistant material for casters and preparation method thereof
High resistance is prepared by adding graphene powder and polyphenylene sulfide to the nylon material and using coated modified flax fibers and carbon nanotubes, as well as epoxy POSS and konjac glucomannan to form modified POSS enhancement components. The grinding nylon composite material solves the problem of insufficient wear resistance of nylon materials in high friction and high wear environments, and achieves the improvement of the wear resistance and mechanical properties of the materials.
Patent Information
- Application Number
- CN202410435188.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-11
AI Technical Summary
Casters made of nylon materials have poor mechanical properties such as wear resistance, especially in high friction and high wear factory environments, which are difficult to meet long-term use requirements, and may be deformed or damaged under heavy pressure.
Using a highly wear-resistant nylon composite material, the composite fiber wear-resistant components are formed by dispersing graphene powder in the nylon system and adding polyphenylene sulfide to reduce the friction coefficient, while using coated modified flax fibers and carbon nanotubes. And a modified POSS reinforcement component is formed through epoxy POSS and konjac glucomannan, and a high wear-resistant material is prepared in combination with the twin screw extrusion mechanism.
It significantly improves the wear resistance and mechanical properties of the material, extends the service life, ensures that good wear resistance can be maintained under high load conditions, avoids the risk of shedding caused by phase separation, and forms excellent mechanical properties.
Smart Images

Figure CN118344726B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of materials, and in particular to a high wear-resistant material for casters and a preparation method thereof. Background Art
[0002] In daily production and life, it is very common to use carts and other transportation tools to transport goods. The emergence of these transportation tools has provided great convenience for the movement of goods. Since these transportation tools are mainly in direct contact with the ground through casters, the quality of casters has a huge impact on the performance of the transportation tools. Nylon materials have the advantages of strong corrosion resistance, good elasticity, good toughness, high stability, etc., and are not easily affected by external factors. They can cope with various complex terrains and working environments. Therefore, they have become a "universal" material and are often used to make mechanical structural parts such as casters. However, with the continuous application of nylon casters, studies have found that in specific high-friction and high-wear working environments such as factories, the wear resistance of nylon casters is difficult to meet the requirements of long-term use, and the mechanical properties of nylon casters are low. Under high loads or heavy pressure, they may be deformed or damaged, which leads to more limited application of nylon casters in factories and other occasions that need to withstand large impact loads.
[0003] In order to make nylon casters meet the use requirements of special application environments such as factories, the nylon material needs to be enhanced and modified. For this purpose, the patent with publication number CN111040441B discloses a high-hardness and wear-resistant nylon 66 alloy material and a preparation method. In order to improve the wear resistance of the nylon material, graphene powder is dispersed in the nylon system and supplemented with polyphenylene sulfide, which can effectively reduce the friction coefficient of the nylon material and improve the wear resistance of the material. Therefore, the formula of the nylon material can be designed to effectively improve the comprehensive performance of the nylon material such as wear resistance.
[0004] Based on this, the present invention provides a high wear-resistant nylon composite material, which can be used to make casters and expand the application range thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a high wear-resistant material for casters and a preparation method thereof, so as to solve the problem that casters made of nylon material have poor mechanical properties such as wear resistance.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A high wear-resistant material for casters, comprising the following components in parts by weight:
[0008]
[0009] The preparation method of the highly wear-resistant material comprises the following steps:
[0010] Step 1: Prepare the ingredients
[0011] Weigh each raw material according to the corresponding weight parts and set aside;
[0012] Step 2: Mixing
[0013] Put all raw materials into a mixer, control the mixing temperature to 90±5°C, the stirring rate to 500-1000r / min, and mechanically stir and mix for 20-40min to form a mixed material;
[0014] Step 3: Extrusion granulation
[0015] Feed the mixed material into the twin-screw extruder through the feeding hopper, control the temperature of each zone of the extruder as follows: zone 1 230±5℃, zone 240±5℃, zone 3 240±5℃, zone 4 240±5℃, zone 5 250±5℃, zone 6 240±5℃, zone 7 240±5℃, the die head temperature 260±5℃, and set the screw speed to 300-400r / min. After melt extrusion, wait for the masterbatch to cool and then pelletize.
[0016] Specifically, the antioxidant in the component can inhibit the oxidation process of the material, prevent the material from aging during use and causing quality problems. The lubricant added to the component can reduce the friction between the components, facilitating subsequent processing and molding. The inorganic additives added to the component can act as a reinforcing agent. The components are heated, melted and plasticized through a twin-screw extruder, so that they are mixed with each other to finally form a highly wear-resistant material.
[0017] A high wear-resistant material for casters is prepared by adopting the preparation method.
[0018] Furthermore, the composite fiber wear-resistant component is prepared by the following method:
[0019] Step 1: Coating modified flax fiber
[0020] Mixing flax fiber and 75% by volume ethanol to form a uniform dispersion, adding aminopropyl polymethylphenylsiloxane to the dispersion, stirring and mixing at a temperature of 40-50° C. for 1-2 hours, adding a crosslinking agent, continuing to stir for 4-6 hours, separating the fiber material, and obtaining coated modified flax fiber;
[0021] Step 2: Making composite fiber wear-resistant components
[0022] The coated modified flax fiber is dispersed in toluene, and then carbon nanotubes are added. After being dispersed to form a uniform dispersion, heating is turned on, and the mixture is stirred and mixed at a temperature of 90-100°C for 6-12 hours, and then the temperature is reduced and the material is discharged. The material is then ball-milled for 1-2 hours to obtain a composite fiber wear-resistant component.
[0023] Specifically, in step one, since the surface of flax fiber is negatively charged, aminopropyl polymethylphenylsiloxane can be adsorbed through electrostatic action to be coated on the surface of flax fiber. Under the action of the cross-linking agent, the aminopropyl polymethylphenylsiloxane molecules will gradually cross-link and entangle to achieve efficient coating of flax fiber to form coated modified flax fiber. In step two, since the aminopropyl polymethylphenylsiloxane molecular chain contains aromatic benzene rings, under high temperature and ball milling treatment, carbon nanotubes can be fixed on the surface of flax fiber through strong π-π conjugation to form flax fiber loaded with carbon nanotubes, forming a composite fiber wear-resistant component.
[0024] Furthermore, in step 1, the length of the flax fiber is 1-2 mm.
[0025] Furthermore, in step 2, the cross-linking agent is succinaldehyde or glutaraldehyde.
[0026] Furthermore, in step 2, the mass ratio of the coated modified flax fiber to the carbon nanotube is 1:5-10.
[0027] Furthermore, the preparation method of the modified POSS reinforcing component is as follows:
[0028] Disperse epoxy POSS in purified water, turn on heating, wait until the temperature reaches 70-80°C, add konjac glucomannan and phase transfer catalyst, keep warm and stir for 4-8 hours, then cool and discharge, wash and vacuum dry to obtain modified POSS reinforcement component, the whole process is carried out under nitrogen protection.
[0029] Specifically, epoxy POSS can be copolymerized with konjac glucomannan under the action of a phase transfer catalyst. Since epoxy POSS has multiple substituted end groups, the formed modified POSS reinforcement component has a dendritic branched structure.
[0030] Furthermore, the mass ratio of the epoxy POSS to konjac glucomannan is 1:2-3.5.
[0031] Furthermore, the phase transfer catalyst is boron trifluoride ether complex.
[0032] Furthermore, the antioxidant is at least one of antioxidant 1010, antioxidant 1076 or antioxidant 168; the lubricant is calcium stearate or zinc stearate; and the inorganic additive is any one of titanium dioxide, calcium carbonate, talc or bentonite.
[0033] Beneficial effects of the present invention:
[0034] (1) The present invention prepares flax fiber loaded with carbon nanotubes as a wear-resistant component of composite fibers and as an additive to nylon matrix materials. Since there is a polysiloxane interface between the flax fiber and the carbon nanotubes, the polysiloxane interface has good lubricity, and the carbon nanotubes can be made to roll and slide relative to the surface of the flax fiber, thereby forming an effect similar to a "ball" effect, thereby enhancing the wear resistance of the material. Moreover, due to the strong conjugation effect, the carbon nanotubes will not fall off during the sliding process, ensuring that the material can still maintain good wear resistance under long-term friction. In addition, the carbon nanotubes and the flax fiber can form a micro three-dimensional structure, and then be composited with the nylon matrix in a form similar to mortise and tenon, which can effectively reduce the risk of falling off due to phase separation.
[0035] (2) The modified POSS reinforcing component prepared by the present invention has a branched structure, and the organic phase konjac glucomannan molecular chains in the structure can form hydrogen bonds with the nylon matrix, and the extended branched molecular chains can extend into various regions of the matrix material to form an intertwined network structure with the nylon molecular chains, thereby anchoring the POSS in the nylon matrix to form a physical cross-linking core, which plays a good role in dispersing stress and transferring load, so that the prepared material can exhibit excellent mechanical properties.
[0036] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0038] Figure 1 for Figure 1 The scanning electron microscope images of flax fiber and composite fiber wear-resistant components, wherein (A) is flax fiber and (B) is composite fiber wear-resistant component;
[0039] Figure 2 Thermogravimetric analysis diagrams of epoxy POSS and modified POSS reinforcement components. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Example 1
[0042] A high wear-resistant material for casters, comprising the following components in parts by weight:
[0043]
[0044] The preparation method of the highly wear-resistant material comprises the following steps:
[0045] Step 1: Prepare the ingredients
[0046] Weigh each raw material according to the corresponding weight parts and set aside;
[0047] Step 2: Mixing
[0048] Put all raw materials into a mixer, control the mixing temperature to 90°C, the stirring rate to 500r / min, and mechanically stir and mix for 40 minutes to form a mixed material;
[0049] Step 3: Extrusion granulation
[0050] The mixed material is fed into a twin-screw extruder through a feeding hopper, and the temperatures of various zones of the extruder are controlled as follows: zone 1 230°C, zone 2 240°C, zone 3 240°C, zone 4 240°C, zone 5 250°C, zone 6 240°C, zone 7 240°C, the die head temperature is 260°C, and the screw speed is set to 300r / min. After melt extrusion, the masterbatch is cooled and then pelletized.
[0051] Example 2
[0052] A high wear-resistant material for casters, comprising the following components in parts by weight:
[0053]
[0054] The preparation method of the highly wear-resistant material comprises the following steps:
[0055] Step 1: Prepare the ingredients
[0056] Weigh each raw material according to the corresponding weight parts and set aside;
[0057] Step 2: Mixing
[0058] Put all the raw materials into a mixer, control the mixing temperature to 90°C, the stirring rate to 800r / min, and mechanically stir and mix for 30 minutes to form a mixed material;
[0059] Step 3: Extrusion granulation
[0060] The mixed material is fed into a twin-screw extruder through a feeding hopper, and the temperatures of various zones of the extruder are controlled as follows: zone 1 230°C, zone 2 240°C, zone 3 240°C, zone 4 240°C, zone 5 250°C, zone 6 240°C, zone 7 240°C, the die head temperature is 260°C, and the screw speed is set at 400r / min. After melt extrusion, the masterbatch is cooled and then pelletized.
[0061] Example 3
[0062] A high wear-resistant material for casters, comprising the following components in parts by weight:
[0063]
[0064] The preparation method of the highly wear-resistant material comprises the following steps:
[0065] Step 1: Prepare the ingredients
[0066] Weigh each raw material according to the corresponding weight parts and set aside;
[0067] Step 2: Mixing
[0068] Put all the raw materials into a mixer, control the mixing temperature to 90°C, the stirring rate to 1000r / min, and mechanically stir and mix for 20 minutes to form a mixed material;
[0069] Step 3: Extrusion granulation
[0070] The mixed material is fed into a twin-screw extruder through a feeding hopper, and the temperatures of various zones of the extruder are controlled as follows: zone 1 230°C, zone 2 240°C, zone 3 240°C, zone 4 240°C, zone 5 250°C, zone 6 240°C, zone 7 240°C, the die head temperature is 260°C, and the screw speed is set at 400r / min. After melt extrusion, the masterbatch is cooled and then pelletized.
[0071] Comparative Example 1
[0072] A highly wear-resistant material for casters, which is different from Example 2 in that no composite fiber wear-resistant component is added, and the rest is the same as Example 2.
[0073] Comparative Example 2
[0074] A highly wear-resistant material for casters, which is different from Example 2 in that the modified POSS reinforcing component is replaced with epoxy POSS, and the rest is the same as Example 2.
[0075] Comparative Example 3
[0076] A highly wear-resistant material for casters, which is different from Example 2 in that no modified POSS reinforcing component is added, and the rest is the same as Example 2.
[0077] The wear-resistant composite fiber components in the above examples and comparative examples were prepared by the following method:
[0078] Step 1: Coating modified flax fiber
[0079] 6 g of flax fiber with a length of 2 mm and 75% by volume of ethanol were mixed to form a uniform dispersion, 12.5 g of aminopropyl polymethylphenylsiloxane was added to the dispersion, and after stirring for 2 h at a temperature of 50° C., 2.5 g of glutaraldehyde was added, and stirring was continued for 6 h, and the fiber material was separated to obtain coated modified flax fiber;
[0080] Step 2: Making composite fiber wear-resistant components
[0081] 5 g of coated modified flax fiber was dispersed in toluene, and 30 g of carbon nanotubes were added. After being dispersed until a uniform dispersion was formed, heating was turned on, and the mixture was stirred and mixed at 95°C for 9 hours, then cooled and discharged. The mixture was then ball-milled for 2 hours to obtain a composite fiber wear-resistant component.
[0082] Figure 1 The scanning electron microscope images of flax fiber and composite fiber wear-resistant components, where (A) is flax fiber and (B) is composite fiber wear-resistant component. It can be observed that the surface of flax fiber is relatively flat and smooth without obvious protrusions, while the surface of composite fiber wear-resistant component is covered with a large number of protruding needles, presenting a miniature three-dimensional structure. This is due to the carbon nanotubes being loaded on the surface of flax fiber via π-π.
[0083] The preparation method of the modified POSS reinforcing component in the above embodiments and comparative examples is as follows:
[0084] Disperse 3g of epoxy POSS in purified water and start heating. When the temperature reaches 75°C, add 8g of konjac glucomannan and 0.2g of boron trifluoride ether complex. After the addition is completed, keep warm and stir for 6h, then cool and discharge the material. After washing and vacuum drying, the modified POSS reinforcement component can be obtained. The whole process is carried out under nitrogen protection.
[0085] Take the same mass of epoxy POSS and modified POSS reinforcement components and perform thermogravimetric analysis. Figure 2 The thermogravimetric analysis diagram of epoxy POSS and modified POSS reinforcement components is shown in Figure 2. Figure 2 It can be seen that the epoxy POSS structure is stable and an obvious weight loss phenomenon occurs at about 400°C, while the modified POSS reinforcement component has two obvious weight loss stages. The first weight loss occurs at about 200°C, where the weight loss phenomenon is caused by the decomposition of unstable groups in konjac glucomannan, and the second weight loss is caused by the thermal decomposition of the POSS skeleton structure.
[0086] Test Case
[0087] The high wear-resistant materials in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for performance, and the results are recorded in Table 1:
[0088] Table 1 - Test results
[0089]
[0090] Note: The test method for abrasion loss is: the material is injection molded into a block test sample with a specification of 10cm×10cm×8mm, placed on a grinding rotary test bench, and rubbed at a speed of (60±2)r / min. The load is set to 1000g, the grinding wheel is SC10, and the abrasion loss of the test sample is measured after 5000 revolutions. For specific test methods, refer to ASTM D3884.
[0091] The test method of tensile strength refers to GB / T 1040-1992;
[0092] The test method for impact strength refers to GB / T 1843-2008;
[0093] The test method for flexural strength refers to GB / T 9341-2008.
[0094] From the data presented in Table 1, it can be seen that the material containing the composite fiber wear-resistant component and the modified POSS reinforcing component has excellent wear resistance and mechanical properties, while the wear resistance of the material without the fiber wear-resistant component decreases significantly. Similarly, the mechanical properties of the material without the modified POSS reinforcing component decrease significantly, and the material formed by replacing the modified POSS reinforcing component with epoxy POSS may be due to the inability to form a cross-linked network structure, so the mechanical properties are also missing.
[0095] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
[0096] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a highly wear-resistant material for casters, characterized in that: The highly wear-resistant material comprises the following components in parts by weight: Nylon 6 60-70 parts; 3-6 parts of composite fiber wear-resistant component; 2-5 parts of modified POSS reinforcing component; 0.5-1.5 parts of antioxidant; 1-2 parts of lubricant; 5-10 parts of inorganic additives; The preparation method comprises the following steps: Step 1: Prepare the ingredients Weigh each raw material according to the corresponding weight parts and set aside; Step 2: Mixing Put all raw materials into a mixer, control the mixing temperature to 90±5°C, the stirring rate to 500-1000r / min, and mechanically stir and mix for 20-40min to form a mixed material; Step 3: Extrusion granulation Feed the mixed material into the twin-screw extruder through the feeding hopper, melt and extrude it, and cut the masterbatch into pellets after it cools down; The composite fiber wear-resistant component is prepared by the following method: Step 1: Coating modified flax fiber The flax fiber and 75% by volume of ethanol are mixed to form a uniform dispersion, and aminopropyl polymethylphenylsiloxane is added to the dispersion. After stirring and mixing for 1-2 hours at a temperature of 40-50° C., a crosslinking agent is added, and stirring is continued for 4-6 hours. The fiber material is separated to obtain the coated modified flax fiber; Step 2: Making composite fiber wear-resistant components The coated modified flax fiber is dispersed in toluene, and then carbon nanotubes are added. After being dispersed to form a uniform dispersion, heating is turned on, and the mixture is stirred and mixed at a temperature of 90-100° C. for 6-12 hours, and then the temperature is lowered and the mixture is discharged. The mixture is then ball-milled for 1-2 hours to obtain a composite fiber wear-resistant component. The modified POSS reinforcing component is prepared by mixing and prepolymerizing epoxy POSS and konjac glucomannan under the action of a phase transfer catalyst; The mass ratio of the epoxy POSS to the konjac glucomannan is 1:2-3.
5.
2. The method for preparing a highly wear-resistant material for casters according to claim 1, characterized in that: In step 1, the length of the flax fiber is 1-2 mm.
3. The method for preparing a highly wear-resistant material for casters according to claim 1, characterized in that: In step 1, the cross-linking agent is succinaldehyde or glutaraldehyde.
4. The method for preparing a highly wear-resistant material for casters according to claim 1, characterized in that: In step 2, the mass ratio of the coated modified flax fiber to the carbon nanotube is 1:5-10.
5. The method for preparing a highly wear-resistant material for casters according to claim 1, characterized in that: The phase transfer catalyst is boron trifluoride ether complex.
6. The method for preparing a highly wear-resistant material for casters according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010, antioxidant 1076 or antioxidant 168; the lubricant is calcium stearate or zinc stearate; the inorganic additive is any one of titanium dioxide, calcium carbonate, talc or bentonite.
7. A high wear-resistant material for casters, characterized in that: The method is prepared according to claim 1.