Preparation method of amino acid-graphene oxide based clean fracturing fluid high-efficiency temperature resistant agent

By modifying a graphene oxide-based high-efficiency temperature-resistant agent with amino acids to form worm-like micelles and a three-dimensional spider web structure, it solves the problem of reduced viscoelastic properties of polymer fracturing fluids at high temperatures and improves the temperature resistance of clean fracturing fluids. and cost reduction, suitable for a wide range of applications.

CN118344860BActive Publication Date: 2024-10-18JIANGSU OCEAN UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410759891.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-18
Estimated Expiration
2044-06-13

Smart Images

  • Figure CN118344860B_ABST
    Figure CN118344860B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of temperature-resistant agents, and specifically discloses a method for preparing an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent. The method comprises the following steps: firstly, obtaining fluffy graphene oxide by a Hummers method; then, obtaining a graphene oxide acyl chloride intermediate by separating a catalyst and decolorizing by distillation using graphene oxide and N,N-dimethylformamide; then, adding the graphene oxide acyl chloride intermediate into a glass reactor filled with amino acid sodium and ultrapure water; controlling the pH value by controlling the dropping rate of a NaOH solution; and finally obtaining an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent by freeze drying. The invention has a simple synthesis process, is suitable for improving the temperature resistance of a common clean fracturing fluid system, does not need to synthesize a new structure viscoelastic surfactant to match the clean fracturing fluid, improves the strength and stiffness of a three-dimensional spider web bionic network structure in the clean fracturing fluid by a non-covalent bond method, does not affect the gel breaking of the clean fracturing fluid, and protects the formation permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of temperature-resistant agents, and in particular to a method for preparing an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent. Background Art

[0002] Fracturing fluids play a vital role in shale oil and gas production, enhancing flow pathways, improving productivity, delivering proppant, and protecting reservoirs. Compared to other types of fracturing fluids, polymer fracturing fluids exhibit enhanced resistance to heat, salt, and shear, ensuring successful fracturing operations in demanding formation conditions. However, some polymer fracturing fluids may leave significant residue in the formation after use. This residue can block oil and gas flow pathways, reduce formation permeability, and thus affect oil and gas recovery efficiency. Clean fracturing fluids completely break down the gel without the addition of any breakers, forming no filter cake or residue, and fully preserving the conductivity of the propped fractures. Therefore, they are widely used in oil and gas field development. However, the viscoelastic properties of clean fracturing fluids decrease at high temperatures. To ensure sand-carrying and fluid loss resistance, the amount of thickener must be significantly increased, which increases fracturing costs.

[0003] To overcome these issues, researchers are exploring new viscoelastic surfactants to create fracturing fluid systems with enhanced strength and temperature resistance. CN112111263A discloses an amphoteric surfactant prepared by reacting a hydroxyl-containing piperazine compound with an organic acid to produce an amidation product, which is then reacted with a sulfonating agent. A high-temperature stabilizer is also prepared by reacting trimethyl borate with a diamino compound. This clean fracturing fluid, formulated with the amphoteric surfactant and high-temperature stabilizer, exhibits excellent solubility, viscosity-increasing properties, temperature resistance, salt tolerance, and sand-carrying properties, making it suitable for use as a working fluid in high-temperature, high-salinity fracturing operations. However, this technology suffers from the following drawbacks: a complex synthesis process and high costs, making it difficult to commercialize on a large scale.

[0004] 2: Invention patent CN 104927799 A discloses a carbon nanotube composite thickener and its preparation method. The thickening fluid material composition by mass is as follows: 1% to 5% viscoelastic surfactant, 0.05-0.4% modified carbon nanotube particles, 0-8% counterion salt, 0% to 3% additive, and the remaining amount is added with water to 100%. The above components are mixed and stirred according to the proportion to produce a carbon nanotube composite thickener, which can improve the temperature resistance of clean fracturing fluid to a certain extent.

[0005] However, this technology has the following defects: its strengthening operation mechanism only exists in the physical adsorption strengthening method, which cannot meet higher temperature resistance and cannot meet the needs of on-site application promotion.

[0006] 3: Invention patent CN109971451B prepares a nano-crosslinker by grafting a silane coupling agent containing double bonds onto the hydroxyl groups on the surface of graphene oxide, and then grafting polymer chains onto the surface through free radical polymerization. The crosslinking density of the nano-crosslinker to the thickener polymer can be regulated by adjusting the ratio of hydrophilic functional groups to hydrophobic functional groups in the grafted polymer. With the help of the reversibility of the non-covalent bond between the graphene surface modified polymer and the polymer in the fracturing fluid, good shear thinning performance is achieved, which reduces the friction between the fracturing fluid and the pipeline during transportation and reduces energy consumption. At the same time, it can form a stable cross-linked structure after reaching the reservoir fracture to stabilize the suspended proppant. The grafting of ionic polymers containing ring structures can effectively improve the temperature and salt stability of the fracturing fluid.

[0007] However, this technology has the following defects: this method is suitable for polymer fracturing fluid, which effectively improves the temperature and salt stability of the polymer fracturing fluid. However, the nano-crosslinker prepared by grafting polymer chain segments on the surface through free radical polymerization will block the oil and gas flow channels after breaking the gel, reducing the permeability of the formation, thereby affecting the oil and gas collection efficiency.

[0008] Therefore, it can be seen from the above that improving the temperature resistance by synthesizing new viscoelastic surfactants is a complex process and has high costs; improving the temperature resistance by using carbon nanotubes is not effective; and improving the temperature resistance by preparing nano-crosslinkers by grafting polymer chains on the surface of graphene oxide is not suitable for clean fracturing fluids. Therefore, a method for preparing an amino acid-graphene oxide-based high-efficiency temperature-resistant agent for clean fracturing fluids is provided. Summary of the Invention

[0009] The purpose of the present invention is to address the defects of the prior art and provide a method for preparing an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent to solve the problems raised by the above background technology.

[0010] To achieve the above objectives, the present invention provides the following technical solution: a method for preparing an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent, the specific steps of which are as follows:

[0011] S1: Preparation of graphene oxide;

[0012] S11: Add graphite powder and NaNO3 to a large beaker, then slowly add concentrated sulfuric acid and stir with a glass rod. Then, place the beaker in an ice-water bath and slowly add KMnO4 under electromagnetic stirring.

[0013] S12: After KMnO4 is completely added, remove the ice water bath and control the temperature in the water bath to react at 15-20°C for 2-3 hours, then increase the water bath temperature to 40-50°C and continue the reaction for 30-40 minutes;

[0014] S13: Ultrapure water is added to the beaker under rapid stirring and the reaction temperature is controlled at 90-100°C. After the reaction is allowed to proceed for 20-30 minutes, 30% H2O2 is added to reduce the excess KMnO4 until no obvious bubbles escape from the reaction mixture. At this point, the reaction mixture turns bright gold. The hot reaction mixture is filtered, washed several times with ultrapure water, and dried under vacuum at 70-80°C. The resulting brown solid powder is graphite oxide.

[0015] S14: Place an appropriate amount of graphite oxide solid powder in a beaker and dissolve it in ultrapure water. Place the beaker in an ultrasonic cleaner and ultrasonicate for 30-40 minutes. Let it stand and collect the supernatant to obtain a single-layer or a few-layer graphene oxide aqueous solution. Freeze-dry the obtained solution to obtain fluffy graphene oxide.

[0016] S2: Preparation of amino acid-graphene oxide-based clean fracturing fluid with high efficiency and temperature resistance;

[0017] S21: Weigh graphene oxide and catalyst into a three-necked flask, first raise the oil temperature of the thermostatic magnetic stirrer to 60-80°C, then control the oil bath temperature and keep the temperature in the flask relatively constant, slowly and evenly introduce phosgene into the flask through the insertion tube, and introduce phosgene at a rate of 0.1-0.15 L / min for 20-30 minutes, then stop, keep warm for 30-40 minutes, maintain the reaction temperature for 2-2.5 hours, then introduce nitrogen to drive out residual phosgene and hydrogen chloride, separate the catalyst, and then distill and decolorize to obtain the graphene oxide acyl chloride intermediate;

[0018] S22: Add sodium amino acid and ultrapure water to a glass reactor, stir to dissolve, and then add 30 wt. / % NaOH until the pH of the system is 12.0±0.2. Turn on the refrigerated circulating bath to lower the system temperature to 15.0±0.1℃ and adjust the stirring rate to 600-800 rpm. -1 , and then gradually add graphene oxide acyl chloride intermediate within 2-2.5 hours, adjust the drop rate of 30 wt. / % NaOH solution to adjust the system pH to 12.0±0.2, and control the system temperature to 15.0±0.1℃ by adjusting the start and stop of the refrigerated circulation bath. After the addition of acyl chloride is completed, continue to add NaOH solution to maintain the system pH at 12.0±0.2, and react at 15.0±0.1℃ for 3-4 hours, and freeze-dry to obtain amino acid-graphene oxide based clean fracturing fluid with high efficiency and temperature resistance.

[0019] As a preferred technical solution of the present invention, the weight ratio of graphite: NaNO3: concentrated sulfuric acid: KMnO4: ultrapure water: H2O2: graphene oxide in step S1 is 20:10:50:7:100:10:12.

[0020] As a preferred technical solution of the present invention, the catalyst in step S21 is N,N-dimethylformamide.

[0021] As a preferred technical solution of the present invention, the graphene oxide in step S2 : N,N-dimethylformamide :Graphene oxide acyl chloride intermediate : Sodium amino acid : water : The ratio of high-efficiency heat-resistant agent is 200 : 1 : 160 : 80 :60 : 110.

[0022] As a preferred technical solution of the present invention, the sodium amino acid in step S22 is any one of sodium glutamate, sodium glycine, and sodium alanine.

[0023] The invention discloses an application of a high-efficiency heat-resistant agent in preparing a clean fracturing fluid. The clean fracturing fluid comprises: 0.5-2 wt% of a viscoelastic surfactant, 0.5-2 wt% of a viscosity-increasing agent, 0.01-0.03 wt% of a high-efficiency heat-resistant agent, and 95.97-98.99 wt% of water.

[0024] As a preferred technical solution of the present invention, the viscoelastic surfactant includes any one of a cationic surfactant, an anionic surfactant and a zwitterionic surfactant.

[0025] As a preferred technical solution of the present invention, the cationic surfactant is any one of hexadecyldimethylbenzyl ammonium chloride, hexadecyltrimethylammonium chloride and octadecyltrimethylammonium chloride; the anionic surfactant is any one of sodium oleate, fatty acid methyl ester ethoxylate sulfonate and fatty alcohol polyoxyethylene ether sodium sulfate; and the zwitterionic surfactant is any one of hexadecylhydroxypropylsulfobetaine, octadecylhydroxypropylsulfobetaine and erucamidehydroxypropylsulfobetaine.

[0026] As a preferred technical solution of the present invention, the viscosity increasing agent is any one of potassium chloride, sodium chloride, sodium lauryl sulfate, sodium p-toluenesulfonate and sodium salicylate.

[0027] As a preferred technical solution of the present invention, the preparation method of the clean fracturing fluid is as follows:

[0028] Step 1: Thoroughly mix the high-efficiency heat-resistant agent and water using an ultrasonic instrument, and divide the resulting dispersion into two equal parts by weight;

[0029] Step 2: Dissolve the viscoelastic surfactant and the viscosity enhancer fully in two equal-mass solutions prepared in step 1;

[0030] Step 3: Stir the two solutions thoroughly and mix them evenly to obtain an amino acid-graphene oxide-based high-temperature resistant clean fracturing fluid.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. The amino acid-modified graphene oxide of this invention exhibits excellent water solubility and a very high specific surface area. This allows for strong surface electrostatic attraction, triggered by the numerous hydroxyl groups of the graphene oxide itself and the carboxyl groups after amino acid grafting, to adsorb and bind to worm-like micelles formed by the viscoelastic surfactant and thickener. This adsorption and binding can shield the electrostatic repulsion between micelles, increase the effective number, density, and strength of entanglements within the micelle network, and promote cross-linking of the micelles with the amino acid-graphene high-efficiency heat-resistant agent into a tighter three-dimensional spider-web-like network structure. Furthermore, the modified groups (amino acid groups) on the amino acid-graphene high-efficiency heat-resistant agent's molecular structure can provide multiple hydrogen bond receptor sites for the micelle molecules, forming a densely bridging structure with multiple hydrogen bonds, thereby effectively improving the heat resistance and fluid loss resistance of the clean fracturing fluid.

[0033] 2. The invention has a simple synthesis process and is suitable for improving the temperature resistance of common clean fracturing fluid systems. It does not require the synthesis of new viscoelastic surfactants to adapt to it and has a wide range of applications.

[0034] 3. This invention improves the strength and stiffness of the three-dimensional spider web bionic network structure in the clean fracturing fluid by means of non-covalent bonds, does not affect the gel breaking of the clean fracturing fluid, and protects the permeability of the formation. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 : This is a cryo-transmission electron microscopy photograph of the glutamic acid-graphene oxide-based high-temperature resistant cationic clean fracturing fluid of the present invention;

[0036] Figure 2 : This is a cryo-transmission electron microscopy photograph of the glycine-graphene oxide-based high-temperature resistant anionic clean fracturing fluid of the present invention;

[0037] Figure 3 : This is a transmission electron microscope photo of the alanine-graphene oxide-based high-temperature resistant zwitterionic clean fracturing fluid of the present invention; DETAILED DESCRIPTION

[0038] The preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more precise definition of the protection scope of the present invention.

[0039] The amino acid-graphene oxide-based high-temperature resistant clean fracturing fluid prepared by the method of the present invention in the following Examples 1-3 was subjected to a temperature resistance test. The specific method is as follows: the prepared fracturing fluid was placed in a high-temperature and high-pressure rheometer to heat the sample. The rheometer heating rate was maintained at (3±0.2)°C / min, the initial temperature was set to 25°C, the target temperature was set to 80-110°C, and when the target temperature was reached, the shear rate was 170s. -1 The total duration of the shear test was 2 h, and the final viscosity value was recorded.

[0040] Example 1: A method for preparing a glutamic acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent,

[0041] Step (1), preparation of graphene oxide;

[0042] Add 40g of graphite powder and 20g of NaNO₃ to a large beaker. Slowly add 100g of concentrated sulfuric acid and stir thoroughly with a glass rod. Place the beaker in an ice-water bath and slowly add 14g of KMnO₄ while stirring. Once the KMnO₄ is completely added, remove the ice-water bath and allow the mixture to react at 15°C for approximately 2 hours. Then, raise the bath temperature to approximately 45°C and continue reacting for another 30 minutes. 200 g of ultrapure water was added to the beaker under rapid stirring, and the reaction temperature was controlled at about 100°C for about 30 minutes. Then, 20 g of 30% H2O2 was added to reduce the excess KMnO4 until no obvious bubbles escaped from the reaction mixture. At this time, the color of the reaction mixture turned bright golden yellow. The reaction mixture was filtered while hot and washed several times with ultrapure water. It was then dried under vacuum at 70°C. The dried solid powder was placed in a beaker and dissolved in ultrapure water. The beaker was then placed in an ultrasonic cleaner for about 30 minutes of ultrasonic treatment. The solution was allowed to stand and the supernatant was taken to obtain a single-layer or minority-layer graphene oxide aqueous solution. The obtained solution was freeze-dried to obtain 24 g of fluffy graphene oxide.

[0043] In the above steps, the weight ratio of graphite: NaNO3: concentrated sulfuric acid: KMnO4: ultrapure water: H2O2: graphene oxide is 20:10:50:7:100:10:12.

[0044] Step (2), preparation of a high-efficiency temperature-resistant agent for glutamic acid-graphene oxide-based clean fracturing fluid;

[0045] 100 g of graphene oxide and 0.5 g of catalyst (N,N-dimethylformamide) were weighed and added to a three-necked flask. The oil temperature of the constant temperature magnetic stirrer was first raised to 70 ° C, and then the oil bath temperature was controlled to keep the temperature in the flask relatively constant. Phosgene was slowly and evenly introduced into the flask through the insertion tube. Phosgene was introduced at a rate of 0.1 L / min for 20 min and then stopped. The reaction was kept warm for 30 minutes. After maintaining the reaction temperature for 2 hours, nitrogen was introduced to drive out the residual phosgene and hydrogen chloride. After separating the catalyst, 80 g of graphene oxide acyl chloride intermediate was obtained by distillation and decolorization.

[0046] Add 40g of sodium glutamate and 30g of ultrapure water to a glass reactor, stir and dissolve, then add 30 wt. / % NaOH until the pH of the system is 12.0; turn on the refrigerated circulating bath to lower the system temperature to 15°C and adjust the stirring rate to 600 r·min. -1 80g of graphene oxide acyl chloride intermediate was then gradually added over 2 hours. The pH of the system was maintained at 12.0 by adjusting the dripping rate of 30 wt. / % NaOH solution, and the system temperature was controlled at 15.0°C by adjusting the start and stop of the refrigerated circulating bath. After the acyl chloride addition was completed, NaOH solution was continued to be added dropwise to maintain the system pH at 12.0. The reaction was then carried out at 15.0°C for 3.5 hours and freeze-dried to obtain 55g of a glutamic acid-graphene oxide-based clean fracturing fluid with high efficiency and temperature resistance.

[0047] In the above steps, the ratio of graphene oxide: N,N-dimethylformamide: graphene oxide acyl chloride intermediate: sodium glutamate: water: high-efficiency temperature-resistant agent is 200:1: 160: 80: 60:110.

[0048] Step (3), preparation of a cationic high temperature resistant clean fracturing fluid;

[0049] 0.2 g of glutamic acid-graphene oxide-based high-efficiency temperature-resistant agent was thoroughly mixed with 975 g of water using an ultrasonic instrument, and the resulting dispersion was divided into two equal parts by weight; 15 g of hexadecyltrimethylammonium chloride and 10 g of sodium salicylate were fully dissolved in the two equal parts of the solution prepared by the above method; the two solutions were fully stirred and mixed evenly to obtain 1000 g of glutamic acid-graphene oxide-based high-temperature resistant cationic clean fracturing fluid.

[0050] Step (4), cryo-TEM, e.g. Figure 1 As shown;

[0051] from Figure 1 It can be seen that the glutamate-graphene oxide-based high-efficiency heat-resistant agent can increase the effective entanglement number, entanglement density and entanglement strength of micelles in the micelle network, and promote the cross-linking of micelles and high-efficiency heat-resistant agents into a tighter three-dimensional spider web bionic network structure.

[0052] Step (5), 90°C temperature resistance test;

[0053] System Name Final viscosity (mPa·s) Cationic system containing high-efficiency heat-resistant agent 47.2 Cationic system without high-efficiency heat-resistant agent 26.5

[0054] Example 2: A method for preparing a glycine-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent.

[0055] Step (1), preparation of graphene oxide;

[0056] Add 80g of graphite powder and 40g of NaNO₃ to a large beaker. Slowly add 200g of concentrated sulfuric acid and stir thoroughly with a glass rod. Place the beaker in an ice-water bath and slowly add 28g of KMnO₄ while stirring. Once the KMnO₄ is completely added, remove the ice-water bath and allow the mixture to react at 20°C for approximately 2.5 hours. Then, raise the bath temperature to approximately 50°C and continue reacting for another 35 minutes. 400 g of ultrapure water was added to the beaker under rapid stirring, and the reaction temperature was controlled at about 90°C. After reacting for about 20 minutes, 40 g of 30% H2O2 was added to reduce excess KMnO4 until no obvious bubbles escaped from the reaction mixture. At this time, the color of the reaction mixture turned bright golden yellow. The reaction mixture was filtered while hot and washed several times with ultrapure water. It was then dried under vacuum at 80°C. The dried solid powder was placed in a beaker and dissolved in ultrapure water. The beaker was then placed in an ultrasonic cleaner for ultrasonic treatment for about 30 minutes. The mixture was allowed to stand and the supernatant was taken to obtain a single-layer or minority-layer graphene oxide aqueous solution. The obtained solution was freeze-dried to obtain 48 g of fluffy graphene oxide.

[0057] In the above steps, the weight ratio of graphite: NaNO3: concentrated sulfuric acid: KMnO4: ultrapure water: H2O2: graphene oxide is 20:10:50:7:100:10:12.

[0058] Step (2), preparation of a glycine-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent;

[0059] 200 g of graphene oxide and 1 g of catalyst (N,N-dimethylformamide) were weighed and added to a three-necked flask. The oil temperature of the constant temperature magnetic stirrer was first raised to 75 ° C, and then the oil bath temperature was controlled to keep the temperature in the flask relatively constant. Phosgene was slowly and evenly introduced into the flask through the insertion tube. Phosgene was introduced at a rate of 0.1 L / min for 25 min and then stopped. The reaction was kept warm for 40 minutes. After maintaining the reaction temperature for 2 hours, nitrogen was introduced to drive out the residual phosgene and hydrogen chloride. After separating the catalyst, 160 g of graphene oxide acyl chloride intermediate was obtained by distillation and decolorization.

[0060] Add 80g of sodium glycinate and 60g of ultrapure water to a glass reactor, stir and dissolve, then add 30 wt. / % NaOH until the pH of the system is 12.0; turn on the refrigerated circulating bath to lower the system temperature to 15°C and adjust the stirring rate to 700 r·min. -1 160g of graphene oxide acyl chloride intermediate was then gradually added over 2 hours. The pH of the system was maintained at 12.0 by adjusting the dripping rate of 30 wt. / % NaOH solution, and the system temperature was controlled at 15.0°C by adjusting the start and stop of the refrigerated circulating bath. After the acyl chloride addition was completed, NaOH solution was continued to be added dropwise to maintain the system pH at 12.0. The reaction was then carried out at 15.0°C for 3 hours and freeze-dried to obtain 110g of a glycine-graphene oxide-based clean fracturing fluid with high efficiency and temperature resistance.

[0061] In the above steps, the ratio of graphene oxide: N,N-dimethylformamide: graphene oxide acyl chloride intermediate: sodium glycinate: water: high-efficiency temperature-resistant agent is 200:1:160:80:60:110.

[0062] Step (3), preparation of anionic high temperature resistant clean fracturing fluid;

[0063] 0.1 g of glycine-graphene oxide-based high-efficiency temperature-resistant agent was thoroughly mixed with 970 g of water using an ultrasonic instrument, and the resulting dispersion was divided into two equal parts by weight; 10 g of sodium oleate and 20 g of potassium chloride were fully dissolved in the two equal parts of the solution prepared by the above method; the two solutions were fully stirred and mixed to obtain 1000 g of glycine-graphene oxide-based high-temperature resistant anionic clean fracturing fluid.

[0064] Step (4) cryo-TEM, e.g. Figure 2 As shown;

[0065] from Figure 2 It can be seen that the glycine-graphene oxide-based high-efficiency heat-resistant agent can increase the effective entanglement number, entanglement density and entanglement strength of micelles in the micelle network, and promote the cross-linking of micelles and high-efficiency heat-resistant agents into a tighter three-dimensional spider web bionic network structure.

[0066] Step (5), 80°C temperature resistance test;

[0067] System Name Final viscosity (mPa·s) Anion system containing high-efficiency heat-resistant agent 39.5 Anionic system without high-efficiency heat-resistant agent 30.2

[0068] Example 3: A method for preparing an alanine-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent.

[0069] Step (1), preparation of graphene oxide;

[0070] Add 60g of graphite powder and 30g of NaNO₃ to a large beaker. Slowly add 150g of concentrated sulfuric acid and stir thoroughly with a glass rod. Place the beaker in an ice-water bath and slowly add 21g of KMnO₄ while stirring. Once the KMnO₄ is completely added, remove the ice-water bath and allow the mixture to react at 15°C for approximately 2 hours. Then, raise the bath temperature to approximately 45°C and continue reacting for another 30 minutes. 300 g of ultrapure water was added to the beaker under rapid stirring, and the reaction temperature was controlled at about 90°C. After reacting for about 25 minutes, 30 g of 30% H2O2 was added to reduce excess KMnO4 until no obvious bubbles escaped from the reaction mixture. At this time, the color of the reaction mixture turned bright golden yellow. The reaction mixture was filtered while hot and washed several times with ultrapure water. It was then dried under vacuum at 70°C. The dried solid powder was placed in a beaker and dissolved in ultrapure water. The beaker was then placed in an ultrasonic cleaner for ultrasonic treatment for about 30 minutes. The mixture was allowed to stand and the supernatant was taken to obtain a single-layer or minority-layer graphene oxide aqueous solution. The obtained solution was freeze-dried to obtain 36 g of fluffy graphene oxide.

[0071] In the above steps, the weight ratio of graphite: NaNO3: concentrated sulfuric acid: KMnO4: ultrapure water: H2O2: graphene oxide is 20:10:50:7:100:10:12.

[0072] Step (2), preparation of alanine-graphene oxide based clean fracturing fluid high efficiency temperature resistant agent;

[0073] 100 g of graphene oxide and 0.5 g of catalyst (N,N-dimethylformamide) were weighed and added to a three-necked flask. The oil temperature of the constant temperature magnetic stirrer was first raised to 70 ° C, and then the oil bath temperature was controlled to keep the temperature in the flask relatively constant. Phosgene was slowly and evenly introduced into the flask through the insertion tube. Phosgene was introduced at a rate of 0.1 L / min for 20 min and then stopped. The reaction was kept warm for 35 minutes. After maintaining the reaction temperature for 2 hours, nitrogen was introduced to drive out the residual phosgene and hydrogen chloride. After separating the catalyst, 80 g of graphene oxide acyl chloride intermediate was obtained by distillation and decolorization.

[0074] Add 40g of sodium alanine and 30g of ultrapure water to a glass reactor, stir to dissolve, and then add 30 wt. / % NaOH until the pH of the system is 12.0. Turn on the refrigerated circulating bath to lower the system temperature to 15°C and adjust the stirring rate to 600 r·min. -180g of graphene oxide acyl chloride intermediate was then gradually added over 2 hours. The pH of the system was maintained at 12.0 by adjusting the dripping rate of 30 wt. / % NaOH solution, and the system temperature was controlled at 15.0°C by adjusting the start and stop of the refrigerated circulating bath. After the acyl chloride addition was completed, NaOH solution was continued to be added dropwise to maintain the system pH at 12.0. The reaction was then carried out at 15.0°C for 3 hours and freeze-dried to obtain 55g of alanine-graphene oxide-based clean fracturing fluid with high efficiency and temperature resistance.

[0075] In the above steps, the ratio of graphene oxide: N,N-dimethylformamide: graphene oxide acyl chloride intermediate: sodium alanine: water: high-efficiency temperature-resistant agent is 200:1: 160: 80: 60:110.

[0076] Step (3), preparation of a zwitterionic high temperature resistant clean fracturing fluid;

[0077] 0.3 g of alanine-graphene oxide-based high-efficiency temperature-resistant agent was thoroughly mixed with 965 g of water using an ultrasonic instrument, and the resulting dispersion was divided into two equal parts by weight; 20 g of erucamide hydroxypropyl sulfobetaine and 15 g of sodium p-toluenesulfonate were fully dissolved in two equal parts of the solution prepared by the above method; the two solutions were fully stirred and mixed evenly to obtain 1000 g of alanine-graphene oxide-based high-temperature resistant zwitterionic clean fracturing fluid.

[0078] Step (4), cryo-TEM, e.g. Figure 3 As shown;

[0079] from Figure 3 It can be seen that the alanine-graphene oxide-based high-efficiency heat-resistant agent can increase the effective entanglement number, entanglement density and entanglement strength of micelles in the micelle network, and promote the cross-linking of micelles and high-efficiency heat-resistant agents into a tighter three-dimensional spider web bionic network structure.

[0080] Step (5), 110°C temperature resistance test;

[0081] System Name Final viscosity (mPa·s) Zwitterionic system containing high-efficiency temperature-resistant agent 42.4 Zwitterionic system without high-efficiency temperature-resistant agent 19.8

[0082] In Examples 1-3, three types of representative amino acid modified graphene oxide-based high-efficiency heat-resistant agents (glutamic acid-graphene oxide, glycine-graphene oxide, alanine-graphene oxide) were synthesized respectively, and their ability to improve the heat resistance of common clean fracturing fluid systems (cationic, anionic, and zwitterionic) was tested. By analyzing the heat resistance test results of Examples 1-3, it was found that the glutamic acid-graphene oxide-based high-efficiency heat-resistant agent improved the heat resistance of the 90°C cationic clean fracturing fluid system by 78.1%; the glycine-graphene oxide-based high-efficiency heat-resistant agent improved the heat resistance of the 80°C anionic clean fracturing fluid system by 30.8%; and the alanine-graphene oxide-based high-efficiency heat-resistant agent improved the heat resistance of the 110°C zwitterionic clean fracturing fluid system by 114.1%. Figure 1-3 It can be seen that the main reason why the amino acid-graphene oxide-based high-efficiency heat-resistant agent can improve the heat resistance of the clean fracturing fluid system is that it can increase the effective entanglement number, entanglement density, and entanglement strength of the micelles in the micellar network, promoting the cross-linking of the micelles and the high-efficiency heat-resistant agent into a more compact three-dimensional spiderweb biomimetic network structure. Therefore, the advantages of the present invention can be concluded by analyzing the data results of Examples 1-3.

[0083] The above embodiments merely illustrate the implementation methods of the present invention. Although the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention. It should be noted that a person skilled in the art may make various modifications and improvements without departing from the scope of the present invention, and these modifications and improvements fall within the scope of protection of the present invention.

Claims

1. Application of an amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent in the preparation of clean fracturing fluid, characterized in that: The clean fracturing fluid contains: viscoelastic surfactant content 0.5-2 wt%, viscosity enhancer content 0.5-2 wt%, high-efficiency temperature resistant agent content 0.01-0.03 wt%, water content 95.97-98.99 wt%; The viscoelastic surfactant includes any one of a cationic surfactant, an anionic surfactant and a zwitterionic surfactant; The cationic surfactant is any one of hexadecyl dimethyl benzyl ammonium chloride, hexadecyl trimethyl ammonium chloride and octadecyl trimethyl ammonium chloride; the anionic surfactant is any one of sodium oleate, fatty acid methyl ester ethoxylate sulfonate and fatty alcohol polyoxyethylene ether sodium sulfate; the zwitterionic surfactant is any one of hexadecyl hydroxypropyl sulfobetaine, octadecyl hydroxypropyl sulfobetaine and erucamide hydroxypropyl sulfobetaine; The viscosity increasing agent is any one of potassium chloride, sodium chloride, sodium dodecyl sulfate, sodium p-toluenesulfonate and sodium salicylate; The preparation method of amino acid-graphene oxide based clean fracturing fluid high efficiency temperature resistant agent comprises the following specific steps: S1: Preparation of graphene oxide; S11: Add graphite powder and NaNO3 into a large beaker, then slowly add concentrated sulfuric acid and stir evenly with a glass rod, then place the beaker in an ice water bath and slowly add KMnO4 under electromagnetic stirring; S12: After KMnO4 is completely added, remove the ice water bath, and control the temperature in the water bath at 15-20°C to react for 2-3 hours, then raise the water bath temperature to 40-50°C and continue the reaction for 30-40 minutes; S13: Add ultrapure water to the beaker under rapid stirring, and control the reaction temperature to 90-100°C for 20-30 minutes, then add 30% H2O2 to reduce the excess KMnO4 until no obvious bubbles escape from the reaction mixture, and the color of the reaction mixture is bright gold. Filter the reaction mixture while hot, wash it with ultrapure water several times, and dry it under vacuum at 70-80°C. The brown solid powder obtained is graphite oxide; S14: taking an appropriate amount of graphite oxide solid powder and placing it in a beaker, dissolving it in ultrapure water, and then placing the beaker in an ultrasonic cleaner for ultrasonic treatment for 30-40 minutes, letting it stand, taking the upper clear liquid, and obtaining a single layer or a few layers of graphene oxide aqueous solution, and freeze-drying the obtained solution to obtain fluffy graphene oxide; S2: Preparation of amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent; S21: Weigh graphene oxide and catalyst and add them into a three-necked flask. First, raise the oil temperature of the constant temperature magnetic stirrer to 60-80°C, then control the oil bath temperature and keep the temperature in the flask relatively constant, slowly and evenly introduce phosgene into the flask through the insertion tube, introduce phosgene at a rate of 0.1-0.15 L / min for 20-30min and then stop, keep warm for 30-40 minutes, maintain the reaction temperature for 2-2.5 hours, introduce nitrogen to drive out the residual phosgene and hydrogen chloride, separate the catalyst and then distill and decolorize to obtain the graphene oxide acyl chloride intermediate; S22: Add amino acid sodium and ultrapure water to a glass reactor, stir to dissolve, then add 30 wt. / % NaOH until the pH of the system is 12.0±0.2; turn on the refrigerated circulating bath to lower the system temperature to 15.0±0.1℃ and adjust the stirring rate to 600-800r·min -1 , and then gradually add graphene oxide acyl chloride intermediate within 2-2.5h, adjust the dropping rate of 30 wt. / % NaOH solution to make the system pH 12.0±0.2, and control the system temperature to 15.0±0.1℃ by adjusting the start and stop of the refrigerated circulation bath. After the addition of acyl chloride, continue to add NaOH solution to maintain the system pH at 12.0±0.2, and react at 15.0±0.1℃ for 3-4 hours, and freeze-dry to obtain amino acid-graphene oxide based clean fracturing fluid high-efficiency temperature-resistant agent.

2. The use of the amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent according to claim 1 in the preparation of clean fracturing fluid, characterized in that: The weight ratio of graphite: NaNO3: concentrated sulfuric acid: KMnO4: ultrapure water: H2O2: graphene oxide in step S1 is 20:10:50:7:100:10:

12.

3. The use of the amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent according to claim 2 in the preparation of clean fracturing fluid, characterized in that: The catalyst in step S21 is N,N-dimethylformamide.

4. The use of the amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent according to claim 3 in the preparation of clean fracturing fluid, characterized in that: The ratio of graphene oxide: N,N-dimethylformamide: graphene oxide acyl chloride intermediate: amino acid sodium: water: high-efficiency temperature-resistant agent in step S2 is 200: 1: 160: 80: 60:

110.

5. The use of the amino acid-graphene oxide-based clean fracturing fluid high-efficiency temperature-resistant agent according to claim 1 in the preparation of clean fracturing fluid, characterized in that: The amino acid sodium in step S22 is any one of sodium glutamate, sodium glycine, and sodium alanine.

6. The use of the amino acid-graphene oxide based clean fracturing fluid high-efficiency temperature resistant agent according to claim 1 in the preparation of clean fracturing fluid, characterized in that: The preparation method of the clean fracturing fluid is as follows: Step 1: fully mix the high-efficiency temperature-resistant agent and water through an ultrasonic instrument, and divide the resulting dispersion into two equal parts by weight; Step 2: Dissolve the viscoelastic surfactant and the viscosity enhancer fully in two solutions of equal mass prepared in step 1 respectively; Step 3: Stir the two solutions thoroughly and mix them evenly to obtain an amino acid-graphene oxide-based high temperature resistant clean fracturing fluid.

Citation Information

Patent Citations

  • Carbon nano-tube complex thickener and preparation method thereof

    CN104927799A

  • A graphene oxide nano-crosslinking agent for fracturing fluid and its preparation method

    CN109971451B

  • Anionic viscoelastic surfactant and preparation method and application thereof

    CN106634936A

  • Application of amino acid modified graphene oxide in water-base drilling fluid as coating agent

    CN110373165A