A catalyst for decomposing ozone and preparation method thereof

By adhering manganese dioxide and titanium dioxide to the aluminum honeycomb carrier, the preparation process of the ozone decomposition catalyst is simplified, the problems of high cost and secondary pollution in the existing technology are solved, and efficient ozone removal is achieved under high humidity conditions, which is suitable for industrialization. promotion.

CN118356931BActive Publication Date: 2024-10-18SHANGHAI FLORY ENVIRONMENT TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410797502.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-18
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Existing ozone decomposition catalysts have complex preparation processes, high energy consumption, high costs, and secondary pollution problems, which lead to difficulties in market promotion, especially when the humidity is high.

Method used

Aluminum honeycomb is used as a carrier, and manganese dioxide and titanium dioxide are adhered through sodium hydroxymethylcellulose and instant sodium silicate to form a catalyst, which simplifies the process, reduces energy consumption, and improves catalytic efficiency.

Benefits of technology

It achieves low-cost and high-efficiency ozone removal. The catalyst remains efficient even under high humidity conditions and has no secondary pollution and odor. It is suitable for large-scale industrial promotion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118356931B_ABST
    Figure CN118356931B_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst for decomposing ozone and a preparation method thereof, and belongs to the technical field of air purification. The catalyst uses an aluminum honeycomb as a carrier, and the carrier is loaded with manganese dioxide and titanium dioxide. The invention solves the problems of high preparation cost and unstable performance of deozonation catalysts by combining the reasonable ratio of manganese dioxide and titanium dioxide with the characteristics of low production cost, stable performance and firm structure of aluminum honeycombs, and at the same time, there is no secondary pollution in the whole preparation process. The prepared ozone decomposition catalyst can efficiently decompose ozone at room temperature, and can still maintain efficient and excellent ozone decomposition effect under high humidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of air purification, and in particular to a catalyst for decomposing ozone and a preparation method thereof. Background Art

[0002] Ozone pollution in the air will have adverse effects on nature and humans themselves, so it is necessary to remove ozone from the air. Catalytic ozone decomposition technology is currently the most promising ozone removal technology. There are many types of existing ozone decomposition catalysts, but most catalysts are relatively inefficient and need to be replaced after a period of use, which will cause secondary pollution. At the same time, most existing catalysts have low ozone removal efficiency, and there are generally factors in the existing catalyst preparation methods that are not conducive to industrialization. For example:

[0003] CN114618475A discloses a method for preparing a flexible manganese-based catalyst for decomposing ozone, including: aluminum mesh pretreatment, anodizing, high temperature roasting, hydration, boehmite, cerium nitrate impregnation, high temperature roasting, manganese compound loading, vacuum drying, high temperature roasting and other processes. This method has complex preparation process, cumbersome flow, high energy consumption and high cost. At the same time, during the anodizing process of the aluminum mesh, the requirements for the process are relatively strict, the defect rate is high, and the preparation cycle is long. From the aluminum mesh pretreatment to the completion of the manganese compound, the entire cycle requires at least 80 hours. At the same time, the energy consumption during high temperature roasting is very high, which is extremely unfavorable for the marketization of the product.

[0004] CN112138653A discloses a method for preparing a silver-nano-alumina catalyst, comprising: adding a silver nitrate solution to a dispersion of nano-alumina and stirring, and then sequentially performing a rotary evaporation treatment and three heat treatments. In the catalyst described in this scheme, the use of silver ions makes the preparation cost high, and the three heat treatments simultaneously consume a lot of energy.

[0005] The above-mentioned prior arts currently have problems such as complex preparation process, high energy consumption, high cost and secondary pollution, so the price of deozonation catalysts in the market has remained high, which is not conducive to marketization and large-scale application. At the same time, the deozonation catalysts on the market will have a greatly reduced effect of decomposing ozone under high humidity. Therefore, it is very necessary to develop a deozonation catalyst and its preparation method that has a simple preparation process, low energy consumption, low cost, is conducive to large-scale industrial promotion and has good deozonation effect, especially still has good ozone removal effect under high humidity. Summary of the invention

[0006] The purpose of the present invention is to provide a catalyst for decomposing ozone and a preparation method thereof, so as to solve the problems of high cost, high energy consumption and secondary pollution existing in the above-mentioned prior art.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] One of the technical solutions of the present invention is a catalyst for decomposing ozone, which uses an aluminum honeycomb as a carrier, and the carrier is loaded with manganese dioxide and titanium dioxide; the manganese dioxide and titanium dioxide are adhered to the surface of the carrier through sodium hydroxymethyl cellulose and quick-dissolving sodium silicate.

[0009] Titanium dioxide mainly plays the role of dispersing components, which can make the manganese dioxide molecular particles more evenly dispersed, thereby expanding its specific surface area and improving the catalytic efficiency of the catalyst.

[0010] The aluminum honeycomb is an aluminum alloy composite plate with a honeycomb structure. The honeycomb structure is composed of regular hexagonal single rooms, with the room openings all facing downward or facing one side, and arranged symmetrically back to back. One regular hexagonal single room is used as a structural unit. The structural diagram of the aluminum honeycomb is shown in the figure below. Figure 1 shown.

[0011] Furthermore, the side length of the structural unit of the aluminum honeycomb is 1-2 mm, and the thickness of the aluminum honeycomb is 10-20 mm. The thickness refers to the thickness of the aluminum honeycomb panel.

[0012] Furthermore, the wall thickness of the aluminum honeycomb is 0.025 mm.

[0013] Furthermore, the side length of the structural unit of the aluminum honeycomb is preferably 1 mm.

[0014] Furthermore, the manganese dioxide is γ-type manganese dioxide.

[0015] In γ-type manganese dioxide, the pyrolusite [1×1] tunnel and the rhombus ore [1×2] tunnel unit cells grow alternately and disorderly along the c-axis direction, resulting in a large number of defects (such as stacking faults), non-ideal ratios, vacancies, etc. in the crystal, and having good void characteristics and chemical reaction activity. Therefore, γ-type manganese dioxide has the advantages of large specific surface area, good adsorption performance, and high catalytic activity that other crystalline forms of manganese dioxide, such as α-type manganese dioxide and β-type manganese dioxide, cannot match.

[0016] Technical solution 2 of the present invention: A method for preparing the above-mentioned catalyst for decomposing ozone comprises the following steps:

[0017] Instantaneous sodium silicate, sodium hydroxymethyl cellulose, manganese dioxide and titanium dioxide are sequentially added to water and stirred evenly to obtain a precursor solution; an aluminum honeycomb is degreased; the precursor solution is coated on the surface of the aluminum honeycomb after the degreasing treatment, and the aluminum honeycomb with the precursor solution coated on the surface is baked to form a coating on the surface of the aluminum honeycomb, and the coating and baking process are repeated until the weight of the aluminum honeycomb increases by 16±1% (that is, the mass of the coating formed on the surface of the aluminum honeycomb after repeated coating and baking is 16±1% of the mass of the aluminum honeycomb carrier), thereby obtaining the catalyst for decomposing ozone.

[0018] The calculation method of the weight gain of the aluminum honeycomb is: (the mass of the catalyst after baking - the mass of the aluminum honeycomb after degreasing) / the mass of the aluminum honeycomb after degreasing × 100%.

[0019] Furthermore, the specific operation of adding instant sodium silicate, sodium hydroxymethyl cellulose, manganese dioxide and titanium dioxide to water in sequence and stirring evenly to obtain a precursor solution is: first add instant sodium silicate to water and stir for 1 hour to fully dissolve the instant sodium silicate in water; then add sodium hydroxymethyl cellulose and stir for 4 hours to fully dissolve sodium carboxymethyl cellulose; then add titanium dioxide and stir for 2 hours; finally add manganese dioxide and stir for 2 hours.

[0020] Furthermore, calculated by mass ratio, water: instant sodium silicate: sodium hydroxymethyl cellulose: manganese dioxide: titanium dioxide = 10: 0.09-0.11: 0.115-0.130: 1.7-1.9: 0.29-0.33.

[0021] More preferably, the mass ratio is: water: instant sodium silicate: sodium hydroxymethyl cellulose: manganese dioxide: titanium dioxide = 10: 0.1: 0.123: 1.8: 0.31.

[0022] Instant sodium silicate mainly plays a bonding role, and sodium carboxymethyl cellulose mainly plays a thickening role. The ratio of each component in the precursor solution is water: instant sodium silicate: sodium hydroxymethyl cellulose: manganese dioxide: titanium dioxide = 10:0.1:0.123:1.8:0.31, and the best adhesion effect can be achieved. The increase in the ratio of instant sodium silicate will occupy the attachment space of manganese dioxide and titanium dioxide. The decrease in the ratio will cause the firmness to be insufficient, and manganese dioxide and titanium dioxide will easily fall off the surface of the carrier. The increase in the ratio of sodium carboxymethyl cellulose will increase the viscosity of the precursor solution, and it will easily clog in the gaps of the carrier. The decrease in the ratio will make the amount of manganese dioxide and titanium dioxide attached to the carrier at a time too small, and repeated loading is required to achieve the ideal effect.

[0023] Furthermore, the coating formed on the surface of the aluminum honeycomb, i.e., the weight gain, contains 77.2% manganese dioxide by mass, and 13.3% titanium dioxide by mass. The components of the precursor solution are evenly dispersed. When the precursor solution is coated on the carrier aluminum honeycomb, the components are evenly distributed on the aluminum honeycomb. During the baking process, the water in the precursor solution is completely removed, and the fast-dissolving sodium silicate, sodium hydroxymethyl cellulose, manganese dioxide, and titanium dioxide are completely retained. Therefore, the mass proportion of manganese dioxide and titanium dioxide in the coating formed on the surface of the aluminum honeycomb is the proportion of manganese dioxide and titanium dioxide in the sum of the masses of fast-dissolving sodium silicate, sodium hydroxymethyl cellulose, manganese dioxide, and titanium dioxide when preparing the precursor solution.

[0024] Furthermore, the coating is performed by immersion.

[0025] Furthermore, the specific operation of the oil removal treatment is:

[0026] The aluminum honeycomb is soaked in a sodium hydroxide solution, then rinsed with clean water and dried.

[0027] Immersing the aluminum honeycomb in a sodium hydroxide solution can not only remove impurities such as oil stains on the surface of the aluminum honeycomb, but also corrode the surface of the aluminum honeycomb and make it rough. The rough surface is more conducive to the adhesion of manganese dioxide and titanium dioxide.

[0028] Furthermore, the concentration of the sodium hydroxide solution is 0.4 mol / L, and the aluminum honeycomb is immersed in the sodium hydroxide solution for 4 minutes; the specific operation of the drying is: baking at 100° C. for 1 hour to dry the surface of the aluminum honeycomb.

[0029] Furthermore, when the aluminum honeycomb coated with the precursor solution is baked, the baking temperature is 80-100° C. and the baking time is 1-2 hours.

[0030] Furthermore, before baking the aluminum honeycomb with the precursor solution coated on the surface, the process also includes blowing through the holes of the aluminum honeycomb with an air gun.

[0031] The third technical solution of the present invention: application of the above-mentioned ozone decomposition catalyst in decomposing ozone.

[0032] In order for a catalyst to exert its excellent application performance, it needs an economical and practical carrier. At the same time, the production and manufacturing process of the catalyst should be energy-saving and simplified in order to be better promoted and applied. The present invention selects a carrier with low cost, wide application range, and does not require too many pre-treatment processes, and optimizes and adjusts the catalyst production process and formula. Thereby, large-scale, batch, low-cost, and high-efficiency production of the catalyst for decomposing ozone is achieved, and the catalyst prepared by the method of the present invention has a good removal effect on ozone and can be actually promoted and applied.

[0033] The present invention discloses the following technical effects:

[0034] The invention discloses a catalyst for decomposing ozone and a preparation method thereof. Through the reasonable ratio of manganese dioxide and titanium dioxide, combined with the characteristics of low production cost, stable performance and firm structure of aluminum honeycomb, the high preparation cost and unstable performance of the deozonation catalyst are solved, and there is no secondary pollution in the whole preparation process. The prepared catalyst for decomposing ozone can efficiently decompose ozone at room temperature. In the whole catalyst preparation process, the addition of titanium dioxide is very critical. The active sites of manganese-based catalysts are easily occupied by water molecules under high humidity, resulting in inactivation. The addition of titanium dioxide can reduce the adsorption performance of water on the catalyst surface, making manganese dioxide more evenly dispersed, which is more conducive to the decomposition of ozone. Therefore, the addition of titanium dioxide enables the catalyst to maintain high efficiency and excellent decomposition of ozone when the humidity increases to 90%RH. The use of instant sodium silicate can increase the adhesion firmness of manganese dioxide and titanium dioxide on the aluminum honeycomb, so that it is not easy to fall off when it adheres to the surface of the aluminum honeycomb, and there is no odor, no secondary pollution, and no performance change under the long-term action of ozone. Sodium hydroxymethyl cellulose mainly plays the role of thickener in the catalyst preparation process, which can make manganese dioxide and titanium dioxide have a certain viscosity, so that it is easier to adhere to the surface of aluminum honeycomb. In addition, sodium carboxymethyl cellulose can also disperse the components in the precursor solution and make each component evenly distributed on the carrier. The synergistic effect of instant sodium silicate and sodium carboxymethyl cellulose can effectively improve the adhesion stability and uniformity of manganese dioxide and titanium dioxide on the carrier, thereby improving the catalytic performance of the catalyst.

[0035] In the present invention, titanium dioxide is used to modify the manganese-based catalyst, which can effectively improve the activity of the manganese-based catalyst, and the improvement of the ozone removal effect of the manganese-based catalyst is much higher than the case of adding molecular sieves and cerium oxide for modification. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 It is a schematic diagram of the structure of aluminum honeycomb;

[0038] Figure 2 This is a surface SEM image of the aluminum honeycomb after degreasing treatment in Example 1;

[0039] Figure 3 This is a physical picture of the catalyst prepared in Example 1;

[0040] Figure 4 This is the surface SEM image of the catalyst prepared in Example 1. DETAILED DESCRIPTION

[0041] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0042] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0043] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0044] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0045] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0046] In a specific embodiment of the present invention, the time for which the aluminum honeycomb after degreasing treatment is immersed in the precursor solution, and the number of repeated coating and baking are not limited to the present invention and can be adjusted at will as long as the weight gain of the aluminum honeycomb can be 16±1%.

[0047] The raw materials used in the following examples and comparative examples are all common commercially available products, among which:

[0048] The instant sodium silicate used is powdered instant sodium silicate;

[0049] The titanium dioxide used is anatase titanium dioxide with an average particle size of 0.1-0.3 μm at EP grade;

[0050] The titanium dioxide used was gamma manganese dioxide with a particle size of 325 mesh;

[0051] The wall thickness of the aluminum honeycombs used is 0.025 mm.

[0052] Example 1

[0053] The preparation of the catalyst for decomposing ozone is as follows:

[0054] Degreasing the aluminum honeycomb: Soak the aluminum honeycomb (15 mm thick, 1 mm side length of the structural unit, 502 mm long × 312 mm wide, 675 g in weight) in a 0.4 mol / L sodium hydroxide solution for 4 min, then rinse with water and bake in an oven at 100 °C for 1 h to dry the surface of the aluminum honeycomb. The surface SEM image of the aluminum honeycomb after degreasing is shown in Figure 2. Figure 1 As shown by Figure 1 It can be seen that the surface of the aluminum honeycomb is corroded and becomes rough.

[0055] Preparation of precursor solution: first add 0.1 kg of instant sodium silicate to 10 kg of water, stir for 1 hour to fully dissolve the instant sodium silicate in the water; then add 0.123 kg of sodium hydroxymethyl cellulose, stir for 4 hours to fully dissolve the sodium carboxymethyl cellulose; then add 0.31 kg of titanium dioxide, stir for 2 hours; finally add 1.8 kg of γ-type manganese dioxide, stir for 2 hours to obtain a precursor solution;

[0056] Preparation of catalyst: Soak the aluminum honeycomb after degreasing treatment in the above-mentioned precursor solution for 30 seconds, so that the precursor solution is coated on the surface of the aluminum honeycomb, blow through the holes of the aluminum honeycomb with an air gun, and then bake the aluminum honeycomb with the precursor solution coated on the surface to form a coating on the surface of the aluminum honeycomb. Repeat the coating and baking process for a total of 4 times. After the fourth baking, the weight gain of the tested aluminum honeycomb is 108g (16%), and a catalyst for decomposing ozone is obtained (according to calculation, the coating formed on the surface of the aluminum honeycomb, i.e., the mass proportion of manganese dioxide in the weight gain is 77.2%, and the mass proportion of titanium dioxide is 13.3%), i.e., an aluminum honeycomb plate loaded with manganese dioxide and titanium dioxide on the surface; wherein, after each coating of the precursor solution by soaking, the holes of the aluminum honeycomb are blown through with an air gun and then baked. The soaking time is 30 seconds each time, and the baking temperature is 80°C each time. The time for the first three bakings is 1 hour, and the time for the last baking is 2 hours. The actual picture of the catalyst prepared in this embodiment is as follows Figure 2 As shown, the surface SEM image is Figure 3 As shown by Figure 2 and Figure 3It can be seen that a coating is formed on the surface of the aluminum honeycomb, which is evenly loaded with manganese dioxide and titanium dioxide.

[0057] The preparation method of this embodiment was repeated, and the weight gain of the aluminum honeycomb after coating and baking 4 times in each repetition was slightly different. After 200 repetitions, the weight gain of the aluminum honeycomb was statistically obtained to be 16±1%. Three groups of catalysts with weight gains of 16%, 16.2%, and 15.8% were selected for the following performance test.

[0058] Example 2

[0059] Same as Example 1, except that the aluminum honeycomb (thickness 15 mm, side length of the structural unit 1 mm, overall size 502 mm long × 312 mm wide, weight 675 g) is replaced by an aluminum honeycomb (thickness 15 mm, side length of the structural unit 1.5 mm, overall size 502 mm long × 312 mm wide, weight 608 g). The preparation method of this example is repeated three times to obtain three groups of catalysts with weight gains of 16.7%, 16.5%, and 16.2% for the aluminum honeycomb, respectively.

[0060] Example 3

[0061] Same as Example 1, except that the aluminum honeycomb (thickness 15 mm, side length of the structural unit 1 mm, overall size 502 mm long × 312 mm wide, weight 675 g) is replaced by an aluminum honeycomb (thickness 15 mm, side length of the structural unit 1.83 mm, overall size 502 mm long × 312 mm wide, weight 574 g). The preparation method of this example is repeated three times to obtain three groups of catalysts with weight gain of the aluminum honeycomb of 15%, 15.6%, and 15.1%, respectively.

[0062] Example 4

[0063] Same as Example 1, except that the aluminum honeycomb (thickness 15 mm, side length of the structural unit 1 mm, overall size 502 mm long × 312 mm wide, weight 675 g) is replaced by an aluminum honeycomb (thickness 10 mm, side length of the structural unit 1 mm, overall size 502 mm long × 312 mm wide, weight 450 g). The preparation method of this example was repeated three times to obtain three groups of catalysts with aluminum honeycomb weight gains of 16%, 16.7%, and 16.1%, respectively.

[0064] Example 5

[0065] The same as Example 1, except that the aluminum honeycomb (thickness of 15 mm, side length of the structural unit of 1 mm, overall size of 502 mm long × 312 mm wide, weight of 675 g) is replaced by an aluminum honeycomb (thickness of 20 mm, side length of the structural unit of 1 mm, overall size of 502 mm long × 312 mm wide, weight of 900 g). The preparation method of this example is repeated three times to obtain three groups of catalysts with weight gains of 17%, 16.8%, and 16.6% for the aluminum honeycomb, respectively.

[0066] Comparative Example 1

[0067] The same as Example 1, except that titanium dioxide is replaced by molecular sieve of equal mass (3A molecular sieve, diameter 0.4-0.8 mm, bulk density 680 kg / m³). The preparation method of this comparative example is repeated three times to obtain three groups of catalysts with aluminum honeycomb weight gains of 16.2%, 16.4%, and 16.1%, respectively.

[0068] Comparative Example 2

[0069] The same as Example 1, except that titanium dioxide is replaced by an equal mass of cerium oxide. The preparation method of this comparative example is repeated three times to obtain three groups of catalysts with weight gains of aluminum honeycombs of 16.2%, 16.1%, and 16%, respectively.

[0070] Comparative Example 3

[0071] Same as Example 1, except that an equal amount of β-manganese dioxide is used instead of γ-manganese dioxide.

[0072] Comparative Example 4

[0073] Same as Example 1, except that an equal amount of instant sodium silicate is used to replace sodium carboxymethyl cellulose, i.e., the use of sodium carboxymethyl cellulose is omitted, and the amount of instant sodium silicate is increased to 0.223 kg. The preparation method of this comparative example is repeated three times to obtain three groups of catalysts with weight gains of 15.2%, 15.6%, and 15.3% for the aluminum honeycomb, respectively. In this comparative example, the coating on the surface of the aluminum honeycomb, i.e., the weight gain, accounts for 77.2% by mass of manganese dioxide, and the mass of titanium dioxide accounts for 13.3%.

[0074] Test Example 1

[0075] Test of the effect of catalyst on ozone removal:

[0076] Three groups of aluminum honeycomb catalysts (aluminum honeycomb panels with manganese dioxide and titanium dioxide loaded on the surface) prepared by the preparation method of Example 1 with weight gains of 16%, 16.2%, and 15.8%, respectively, and one group of unloaded aluminum honeycomb panels (thickness of 15 mm, side length of structural unit of 1 mm, overall dimensions of 502 mm long × 312 mm wide, weight of 675 g) without any treatment were selected for testing. The test conditions were: temperature of 23°C, humidity of 45%RH, 60%RH, 75%RH, 90%RH, respectively, and wind speed of 1 m / s.

[0077] The test steps are as follows:

[0078] First, place an unloaded aluminum honeycomb panel on a test bench, with a fan and an ozone generator at the front end of the test bench, turn on the fan and ozone generator of the test bench, evenly select 9 points on the unloaded aluminum honeycomb panel, and test the ozone concentration of each point after the unloaded aluminum honeycomb panel, which is recorded as the initial ozone concentration; then replace the unloaded aluminum honeycomb panel with a catalyst (an aluminum honeycomb panel loaded with manganese dioxide and titanium dioxide) prepared by the preparation method of Example 1, and test the ozone concentration after the catalyst at the same point. The ozone removal efficiency of the catalyst is calculated by the formula: ozone removal efficiency = (initial ozone concentration - ozone concentration after the catalyst) / initial ozone concentration × 100%, and then take the average value, which is the ozone removal efficiency of each group of catalysts. Select three groups of catalysts respectively, and repeat the above test three times so that the data is more accurate. The test results are shown in Table 1.

[0079] Table 1

[0080]

[0081] Select three types of ozone removal catalytic plates A, B and C on the market (A is a 150×140×13 ozone removal catalytic plate purchased from Zhejiang Meike Air Purification Technology Co., Ltd., B is a 320×380×13 ozone removal catalytic plate purchased from Guangzhou Shangcheng Filtration Equipment Co., Ltd., and C is a 225×312×15 ozone removal catalytic plate purchased from Elkelly Environmental Protection (Suzhou) Co., Ltd.) and conduct comparative tests under different humidity conditions. The test results are shown in Table 2:

[0082] Table 2

[0083]

[0084] From the above test data, we can see that the ozone removal efficiency of the three catalytic plates A, B and C on the market shows a clear downward trend as the humidity increases. When the humidity reaches 90%RH, the catalytic effect is completely lost.

[0085] Test Example 2

[0086] The ozone removal effects of the catalysts with different sizes of aluminum honeycomb carriers (same thickness, different side lengths of structural units) prepared by the preparation methods of Examples 1-3 were compared as test objects. The size of the unloaded aluminum honeycomb plate (thickness and side length of the structural unit) selected for each catalyst test was consistent with the size of the carrier of the catalyst to be tested, and the test conditions were: temperature 23°C, humidity 60%RH, wind speed 1m / s. The test steps were the same as those of Test Example 1, and the test results are shown in Table 3 (wherein the test data of Example 1 directly adopted the test data at a humidity of 60%RH in Test Example 1, the first group was the group with the largest aluminum honeycomb weight gain among the three groups of catalysts selected in each embodiment, and the third group was the group with the smallest aluminum honeycomb weight gain among the three groups of catalysts selected in each embodiment).

[0087] Table 3

[0088]

[0089] It can be seen from Table 3 that when the thickness of the aluminum honeycomb carrier remains unchanged, the smaller the side length of its structural unit is, the higher the ozone removal efficiency of the obtained catalyst is.

[0090] Test Example 3

[0091] The ozone removal effects of the catalysts with different sizes of aluminum honeycomb carriers (different thicknesses and the same side length of the structural unit) prepared by the preparation methods of Examples 1 and 4-5 were compared as test objects. The size of the unloaded aluminum honeycomb plate (thickness and side length of the structural unit) selected for each catalyst test was consistent with the size of the carrier of the catalyst to be tested, and the test conditions were: temperature 23°C, humidity 60%RH, wind speed 1m / s. The test steps were the same as those of Test Example 1, and the test results are shown in Table 4 (wherein the test data of Example 1 directly adopted the test data at a humidity of 60%RH in Test Example 1, the first group was the group with the largest aluminum honeycomb weight gain among the three groups of catalysts selected in each embodiment, and the third group was the group with the smallest aluminum honeycomb weight gain among the three groups of catalysts selected in each embodiment).

[0092] Table 4

[0093]

[0094] It can be seen from Table 4 that when the side length of the structural unit of the aluminum honeycomb carrier remains unchanged, the thicker the thickness is, the higher the ozone removal efficiency of the obtained catalyst is.

[0095] Test Example 4

[0096] The catalysts prepared by the preparation methods of Example 1 and Comparative Examples 1-4 were used as test objects to compare the ozone removal effects, and the test conditions were: temperature 23°C, humidity 60%RH, and wind speed 1m / s. The test steps were the same as those of Test Example 1, and the test results are shown in Table 5 (wherein the test data of Example 1 directly adopts the test data at a humidity of 60%RH in Test Example 1).

[0097] Table 5

[0098] catalyst Average single removal efficiency (%) Example 1 93.6 Comparative Example 1 48.70 Comparative Example 2 59.71 Comparative Example 3 42.8 Comparative Example 4 54.2

[0099] Test Example 5

[0100] Aging test:

[0101] The catalyst with an aluminum honeycomb weight gain of 16% obtained by the preparation method of Example 1 was aged. The aging method was as follows: first, the catalyst (aluminum honeycomb panel with manganese dioxide and titanium dioxide loaded on the surface) was installed in an air purifier, and then the air purifier was placed in a 3m³ closed environment with an ozone concentration of 1230ppb and the purifier was turned on. At the same time, an ozone generator in the closed space continuously released ozone to ensure that the concentration of ozone in the closed space was constant. After three months of continuous operation, the catalyst was taken out and placed on the test bench for comparative testing. The ozone removal efficiency of the catalyst before and after aging was tested using the test method of Test Example 1. The test conditions were: temperature 23°C, humidity 60%RH, wind speed 1m / s, and the results are shown in Table 6.

[0102] Table 6

[0103]

[0104] It can be seen from Table 6 that after the catalyst was aged for three months, its catalytic performance against ozone did not decay.

[0105] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A catalyst for decomposing ozone, It is characterized in that An aluminum honeycomb is used as a carrier, and manganese dioxide and titanium dioxide are loaded on the carrier; the manganese dioxide and titanium dioxide are adhered to the surface of the carrier through sodium hydroxymethyl cellulose and quick-dissolving sodium silicate; The side length of the structural unit of the aluminum honeycomb is 1-2 mm, and the thickness of the aluminum honeycomb is 10-20 mm; The manganese dioxide is γ-type manganese dioxide; The method for preparing the ozone decomposing catalyst comprises the following steps: Instant sodium silicate, sodium hydroxymethyl cellulose, manganese dioxide and titanium dioxide are sequentially added to water and stirred to obtain a precursor solution; the aluminum honeycomb is degreased; the precursor solution is coated on the surface of the aluminum honeycomb after the degreasing treatment, and the aluminum honeycomb with the precursor solution coated on the surface is baked to form a coating on the surface of the aluminum honeycomb, and the coating and baking processes are repeated until the aluminum honeycomb increases in weight by 16±1%, thereby obtaining the catalyst for decomposing ozone; Calculated by mass ratio, water: instant sodium silicate: sodium hydroxymethyl cellulose: manganese dioxide: titanium dioxide = 10: 0.09-0.11: 0.115-0.130: 1.7-1.9: 0.29-0.

33.

2. The catalyst for decomposing ozone as claimed in claim 1, It is characterized in that The coating is performed by dipping.

3. The catalyst for decomposing ozone as claimed in claim 1, It is characterized in that The specific operation of the oil removal treatment is: The aluminum honeycomb is soaked in a sodium hydroxide solution, then rinsed with clean water and dried.

4. The catalyst for decomposing ozone as claimed in claim 1, It is characterized in that The baking temperature is 80-100° C. and the baking time is 1-2 hours.

5. Use of the ozone decomposing catalyst according to any one of claims 1 to 4 in decomposing ozone.

Citation Information

Patent Citations

  • Catalyst for decomposing ozone and preparation method thereof

    CN112138653A

  • Mixed catalyst and honeycomb using it

    JP2005095804A