Automobile oil pipe and preparation method thereof

By using modified whisker carbon nanotubes with NBR/PVC blend glue in automobile oil pipes, a three-dimensional network structure is formed, which solves the problem of oil pipes cracking during high-temperature vulcanization and molding, reduces the scrap rate and costs , suitable for mass production.

CN118359854BActive Publication Date: 2024-10-08SHIYAN SENXIN AUTOMOTIVE COMPONENTS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410643044.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-08
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

During the high-temperature vulcanization molding process, automobile oil pipes are prone to cracking at corners and reducing sections, resulting in a high scrap rate.

Method used

Modified whisker carbon nanotubes are used in conjunction with NBR/PVC blend rubber to form a three-dimensional network structure in the rubber material for mechanical reinforcement, improve thermal conduction efficiency, and reduce local thermal stress.

Benefits of technology

It significantly reduces the cracking rate of automobile oil pipes, reduces the scrap rate, and reduces the cost of raw materials, making it suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118359854B_ABST
    Figure CN118359854B_ABST
Patent Text Reader

Abstract

The present application discloses an automobile oil pipe and a preparation method thereof, and relates to the field of automobile oil pipe materials. The automobile oil pipe is made of the following components in parts by weight: 80-120 parts of NBR / PVC blended rubber, 1-2 parts of stearic acid, 6-20 parts of modified whisker carbon nanotubes, 4-5 parts of zinc oxide, 3-4.5 parts of antioxidant, 2-3 parts of compatibilizer, 25-40 parts of plasticizer, 40-50 parts of carbon black, 10-20 parts of white carbon black, 1-3 parts of vulcanizing agent, and 4-4.9 parts of accelerator. The present application has the effect of reducing the scrap rate in the production process of automobile oil pipes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of automobile oil pipe materials, and in particular to an automobile oil pipe and a preparation method thereof. Background Art

[0002] Automobile oil pipes are indispensable parts of automobiles, including brake oil pipes, oil return pipes and other oil pipes. In order to adapt to the internal installation space of the automobile, the oil pipes can be divided into special-shaped oil pipes and variable-diameter oil pipes according to their shapes. The shape of the oil pipe is determined by the mandrel used when the rubber is vulcanized at high temperature.

[0003] At present, in order to meet the oil resistance and processing performance of oil pipes, NBR / PVC blended rubber made of nitrile rubber (NBR) and polyvinyl chloride (PVC) is often used as the main type of rubber for making oil pipes.

[0004] However, when manufacturing oil pipes, during the process of vulcanization of rubber materials, special-shaped oil pipes / reduced-diameter oil pipes are prone to cracking at bends / reduced-diameter sections, resulting in a high scrap rate. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the related art, the present application provides an automobile oil pipe and a preparation method thereof.

[0006] On the one hand, the present application provides an automobile oil pipe adopting the following technical solution:

[0007] An automobile oil pipe is made of the following components in parts by weight: 80-120 parts of NBR / PVC blended rubber, 1-2 parts of stearic acid, 6-20 parts of modified whisker carbon nanotubes, 4-5 parts of zinc oxide, 3-4.5 parts of antioxidant, 2-3 parts of compatibilizer, 25-40 parts of plasticizer, 40-50 parts of carbon black, 10-20 parts of white carbon black, 1-3 parts of vulcanizer and 4-4.9 parts of accelerator.

[0008] Preferably, the modified whisker carbon nanotubes are prepared by the following method: adding whisker carbon nanotubes to a formic acid solution of polyamide to obtain a mixed solution, subjecting the mixed solution to ultrasonic oscillation at 35-50°C for 6-9h, and finally washing with ethanol, filtering, and drying to obtain modified whisker carbon nanotubes for use.

[0009] Preferably, the whisker carbon nanotubes are added to a formic acid solution of polyamide to obtain a mixed solution, the mixed solution is subjected to ultrasonic oscillation at 40° C. for 7 hours, and finally washed with ethanol, filtered, and dried to obtain modified whisker carbon nanotubes for use.

[0010] Preferably, the weight ratio of whisker carbon nanotubes to polyamide in the mixed solution is 20-100:1.

[0011] Preferably, the weight ratio of whisker carbon nanotubes to polyamide in the mixed solution is 60:1.

[0012] Preferably, the whisker carbon nanotube has a length of 1-15 μm, an inner diameter of 2-5 nm, and an outer diameter of 20-100 nm.

[0013] Preferably, the polyamide comprises one or more of polyamide 6T / 6, polyamide 6T / 66 and polyamide 6T / 6I.

[0014] Preferably, the polyamide is polyamide 6T / 66.

[0015] Preferably, the NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 0.5-4:1.

[0016] Preferably, the NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 3:2.

[0017] Preferably, the vulcanizing agent includes one or both of sulfur and dicumyl peroxide.

[0018] Preferably, the vulcanizing agent is sulfur.

[0019] Preferably, the plasticizer includes one or more of tributyl citrate, dioctyl phthalate, tri-isooctyl trimellitate and dibutyl sebacate.

[0020] Preferably, the plasticizer is dibutyl sebacate.

[0021] Preferably, the accelerator comprises one or both of dimethyl bisthiocarbonyl disulfide and dimorpholine disulfide.

[0022] Preferably, the accelerator is dithiocarbonyldimethylamine disulfide.

[0023] Preferably, the zinc oxide is zinc oxide whisker.

[0024] Preferably, the zinc oxide is a tetrapod-shaped zinc oxide whisker.

[0025] On the other hand, the present application also provides a method for preparing an automobile oil pipe using the following technical solution:

[0026] A method for preparing an automobile oil pipe comprises the following steps: kneading the components except a vulcanizer and an accelerator to obtain a kneaded product, then kneading the kneaded product, the vulcanizer and the accelerator to obtain a rubber compound, and finally extruding the rubber compound into a tube blank, and vulcanizing the tube blank on a mandrel to obtain the automobile oil pipe.

[0027] In summary, the present application includes at least one of the following beneficial technical effects:

[0028] 1. By adding modified whisker carbon nanotubes, on the one hand, as the content of modified whisker carbon nanotubes in the automobile oil pipe increases, they form a three-dimensional network structure with zinc oxide whiskers in the tube embryo, thereby mechanically reinforcing the tube embryo during the high-temperature vulcanization process when the automobile oil pipe is made. On the other hand, the hollow channel of the modified whisker carbon nanotubes improves the heat conduction efficiency inside the tube embryo, thereby reducing the stress generated by local thermal shrinkage at the bend / diameter-changing section of the tube embryo. Under the combined effect, the cracking rate of the automobile oil pipe is reduced by 80%, and the scrap rate of the automobile oil pipe in the production process is reduced;

[0029] 2. The unique aspect ratio of modified whisker carbon nanotubes improves the uniformity of dispersion of modified whisker carbon nanotubes in the rubber compound, which is conducive to the formation of a three-dimensional network structure and is also conducive to heat conduction in the tube embryo, reducing the possibility of local thermal stress concentration at the bend / diameter section of the tube embryo;

[0030] 3. Using easily available and low-cost whisker carbon nanotubes as fillers can reduce the scrap rate of automobile oil pipes during the production process while also reducing the raw material cost of automobile oil pipes, which is conducive to the large-scale production of automobile oil pipes. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0032] Figure 1 It is a schematic diagram used in this application to show the turning point / diameter-changing section of the automobile oil pipe. DETAILED DESCRIPTION

[0033] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.

[0034] The raw materials used in the embodiments and comparative examples can all be obtained commercially. In the embodiments and comparative examples of the present application, the carbon black is N550 carbon black, the antioxidant is antioxidant 1010, the compatibilizer is maleic anhydride grafted ABS, the vulcanizing agent is sulfur, the accelerator is accelerator TMTD (dithiocarbonyl dimethylamine disulfide), and the plasticizer is dibutyl sebacate.

[0035] Example 1

[0036] Example 1 of the present application provides an automobile oil pipe, which is prepared by the following steps:

[0037] a. Modification of whisker carbon nanotubes: dissolve 10 g of polyamide in 1000 mL of formic acid, slowly add 600 g of whisker carbon nanotubes under stirring to obtain a mixed solution, then place the mixed solution under ultrasonic oscillation at 40° C. for 7 h, finally wash with ethanol, filter, and dry to obtain modified whisker carbon nanotubes for use.

[0038] b. Internal mixing: put the NBR / PVC blend into an internal mixer and plasticize for 60 seconds, then add stearic acid, modified whisker carbon nanotubes, four-needle zinc oxide whiskers, antioxidant and compatibilizer, lower the top plug for 60 seconds, raise the top plug to add white carbon black and half of the carbon black, lower the top plug for 80 seconds, raise the top plug to add half of the plasticizer, lower the top plug for 90 seconds, add the remaining carbon black, lower the top plug for 80 seconds, add the remaining plasticizer, lower the top plug and mix to 140°C for rubber discharge to obtain the internal mixing product.

[0039] c. Open mixing: add the internal mixing product into the open mixing mill, add the vulcanizer and accelerator after rolling, pass the mixture through the mixing mill for 2 times and tamp the mixture for 5 times, produce sheets, and leave the sheets for 24 hours to obtain the rubber compound.

[0040] d. Extrusion vulcanization: use an extruder to extrude the rubber into a tube embryo, put the tube embryo on the mandrel and vulcanize it at 150℃ for 30 minutes to obtain the automobile oil pipe. Figure 1 .

[0041] In the embodiment of the present application, 100 parts of NBR / PVC blended rubber, 6 parts of modified whisker carbon nanotubes, 1.5 parts of stearic acid, 4.5 parts of zinc oxide, 45 parts of carbon black, 15 parts of white carbon black, 30 parts of plasticizer, 4 parts of antioxidant, 2.5 parts of compatibilizer, 2 parts of vulcanizer, and 4.5 parts of accelerator; the NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 3:2; the whisker carbon nanotubes used to prepare the modified whisker carbon nanotubes have a length of 1-15 μm, an inner diameter of 2-5 nm, and an outer diameter of 20-100 nm; the particle size of the four-needle zinc oxide whisker is 0.5-5 μm; the polyamide is polyamide 6T / 66, and the number average molecular weight is 24000 g / mol.

[0042] Example 2

[0043] Example 2 of the present application provides an automobile oil pipe. The difference between Example 2 and Example 1 is that in Example 2, the weight parts of each component are as follows: 100 parts of NBR / PVC blend rubber, 12 parts of modified whisker carbon nanotubes, 1.5 parts of stearic acid, 4.5 parts of four-needle zinc oxide whiskers, 45 parts of carbon black, 15 parts of white carbon black, 30 parts of plasticizer, 4 parts of antioxidant, 2.5 parts of compatibilizer, 2 parts of vulcanizer, and 4.5 parts of accelerator.

[0044] Example 3

[0045] Example 3 of the present application provides an automobile oil pipe. The difference between Example 3 and Example 1 is that in Example 2, the weight parts of each component are as follows: 100 parts of NBR / PVC blend rubber, 20 parts of modified whisker carbon nanotubes, 1.5 parts of stearic acid, 4.5 parts of four-needle zinc oxide whiskers, 45 parts of carbon black, 15 parts of white carbon black, 30 parts of plasticizer, 4 parts of antioxidant, 2.5 parts of compatibilizer, 2 parts of vulcanizer, and 4.5 parts of accelerator.

[0046] Example 4

[0047] Example 4 of the present application provides an automobile oil pipe. The difference between Example 4 and Example 2 is that in Example 4, the modification steps of the whisker carbon nanotubes are as follows: 10g of polyamide is dissolved in 1000mL of formic acid, 200g of whisker carbon nanotubes are slowly added under stirring, and then ultrasonically oscillated at 40°C for 7h, and finally washed with ethanol, filtered, and dried to obtain modified whisker carbon nanotubes for use.

[0048] Example 5

[0049] Example 5 of the present application provides an automobile oil pipe. The difference between Example 5 and Example 2 is that in Example 5, the modification steps of the whisker carbon nanotubes are as follows: 10g of polyamide is dissolved in 1000mL of formic acid, 1000g of whisker carbon nanotubes are slowly added under stirring, and then ultrasonically oscillated at 40°C for 7h, and finally washed with ethanol, filtered, and dried to obtain modified whisker carbon nanotubes for use.

[0050] Example 6

[0051] Example 6 of the present application provides an automobile oil pipe. The difference between Example 6 and Example 2 is that in Example 6, when modifying the whisker carbon nanotubes, the polyamide used is polyamide 6T / 6 with a number average molecular weight of 23000 g / mol.

[0052] Example 7

[0053] Example 7 of the present application provides an automobile oil pipe. The difference between Example 7 and Example 2 is that in Example 7, when modifying the whisker carbon nanotubes, the polyamide used is polyamide 6T / 6I, and the number average molecular weight is 26000 g / mol.

[0054] Comparative Example 1

[0055] Comparative Example 1 provides an automobile oil pipe, which is prepared by the following steps:

[0056] Internal mixing: put the NBR / PVC blend into an internal mixer and plasticize for 60 seconds, then add stearic acid, whisker carbon nanotubes, four-needle zinc oxide whiskers, antioxidant and compatibilizer, lower the top plug pressure for 60 seconds, raise the top plug to add white carbon black and half of the carbon black, lower the top plug pressure for 80 seconds, raise the top plug to add half of the plasticizer, lower the top plug for 90 seconds, add the remaining carbon black, lower the top plug for 80 seconds, add the remaining plasticizer, lower the top plug and mix to 140°C for rubber discharge to obtain the internal mixing product.

[0057] Open mixing, add the internal mixing product into the open mixing mill, add the vulcanizer and accelerator after rolling, thin pass 2 times, tamp the rubber 5 times, make a sheet, leave it for 24 hours, and get the rubber compound.

[0058] Extrusion vulcanization: use an extruder to extrude the rubber into a tube embryo, put the tube embryo on a mandrel and vulcanize it at 150°C for 30 minutes to obtain an automobile oil pipe.

[0059] In this comparative example, there are 100 parts of NBR / PVC blended rubber, 6 parts of whisker carbon nanotubes, 1.5 parts of stearic acid, 4.5 parts of tetrapod-shaped zinc oxide whiskers, 45 parts of carbon black, 15 parts of white carbon black, 30 parts of plasticizer, 4 parts of antioxidant, 2.5 parts of compatibilizer, 2 parts of vulcanizer, and 4.5 parts of accelerator; the NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 3:2; the whisker carbon nanotubes have a length of 1-15 μm, an inner diameter of 2-5 nm, and an outer diameter of 20-100 nm.

[0060] Comparative Example 2

[0061] Comparative Example 2 provides an automobile oil pipe, which is prepared by the following steps:

[0062] Internal mixing: put the NBR / PVC blend into an internal mixer and plasticize for 60 seconds, then add stearic acid, zinc oxide, antioxidant and compatibilizer, lower the top plug for 60 seconds, raise the top plug to add white carbon black and half of the carbon black, lower the top plug for 80 seconds, raise the top plug to add half of the plasticizer, lower the top plug for 90 seconds, add the remaining carbon black, lower the top plug for 80 seconds, add the remaining plasticizer, lower the top plug and mix to 140°C for rubber discharge to obtain the internal mixing product.

[0063] Open mixing, add the internal mixing product into the open mixing mill, add the vulcanizer and accelerator after rolling, thin pass 2 times, tamp the rubber 5 times, make a sheet, leave it for 24 hours, and get the rubber compound.

[0064] Extrusion vulcanization: use an extruder to extrude the rubber into a tube embryo, put the tube embryo on a mandrel and vulcanize it at 150°C for 30 minutes to obtain an automobile oil pipe.

[0065] In this comparative example, NBR / PVC blended rubber is 100 parts, stearic acid is 1.5 parts, tetrapod-shaped zinc oxide whiskers are 4.5 parts, carbon black is 45 parts, white carbon black is 15 parts, plasticizer is 30 parts, antioxidant is 4 parts, compatibilizer is 2.5 parts, vulcanizer is 2 parts, and accelerator is 4.5 parts; NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 3:2.

[0066] Comparative Example 3

[0067] Comparative Example 3 provides an automobile oil pipe. The difference between Comparative Example 3 and Example 2 is that: in the process of preparing the automobile oil pipe, Comparative Example 3 uses modified multi-walled carbon nanotubes to replace the modified whisker carbon nanotubes, and the modified multi-walled carbon nanotubes are prepared by the following steps: 10g of polyamide is dissolved in 1000mL of formic acid, 600g of multi-walled carbon nanotubes are slowly added under stirring to obtain a mixed solution, and then the mixed solution is placed at 40°C for ultrasonic oscillation for 7h, and finally washed with ethanol, filtered, and dried to obtain the modified multi-walled carbon nanotubes for use.

[0068] Comparative Example 4

[0069] Comparative Example 4 provides an automobile oil pipe. The difference between Comparative Example 4 and Example 2 is that in the process of preparing the automobile oil pipe, zinc oxide is used to replace the four-needle zinc oxide whiskers.

[0070] Test and Inspection

[0071] (1) The automobile oil pipes prepared in Examples 1-7 and Comparative Examples 1-4 were tested for tensile strength at 150° C. using an electronic tensile testing machine. The test results are shown in Table 1.

[0072] (2) Take 500 automobile oil pipes prepared in Examples 1-7 and Comparative Examples 1-4 respectively, and count the number of oil pipes at the bends.

[0073] / Cracking rate of the variable diameter section. The test results are shown in Table 1.

[0074] Table 1:

[0075]

[0076]

[0077] Results Analysis

[0078] The present application is described in detail below in conjunction with the experimental data provided in Table 1.

[0079] The cracking rate of the automobile oil pipe provided in Examples 1-3 is as low as less than 1%, and the tensile strength at 150°C is as high as 13 MPa or more, indicating that the automobile oil pipe provided in Examples 1-3 also has good tensile strength under high temperature conditions, and the pipe embryo has good anti-cracking effect during high-temperature vulcanization.

[0080] With reference to Example 2, Examples 4 and 5 reflect the effect of the weight ratio of whisker carbon nanotubes and polyamide on the cracking rate and tensile strength of the obtained automobile oil pipe when the whisker carbon nanotubes are modified. The high-temperature tensile strength of the automobile oil pipe provided by Example 2 is higher than the high-temperature tensile strength of the automobile oil pipes provided by Examples 4 and 5, while the cracking rate of the automobile oil pipe provided by Example 2 is lower than the cracking rate of the automobile oil pipes provided by Examples 4 and 5, indicating that when the whisker carbon nanotubes are modified by polyamide, the weight ratio of polyamide to whisker carbon nanotubes is 1:60, which is beneficial to improving the high-temperature tensile strength of the obtained automobile oil pipe and reducing the cracking rate. Analysis may be because when the weight ratio of polyamide to whisker carbon nanotubes is 1:60, the combination effect of the modified whisker carbon nanotubes and other components is better. Compared with Example 1, although the content of modified whisker carbon nanotubes in Example 3 is increased, the 150°C tensile strength is slightly reduced. Analysis shows that the increase in the content of modified whisker carbon nanotubes causes gaps to appear at the interface between the modified whisker carbon nanotubes and other components, resulting in a decrease in mechanical strength. However, the cracking rate of the automobile oil pipe provided by Example 3 is still lower than that of the automobile oil pipe provided by Example 1, indicating that the increase in the content of modified whisker carbon nanotubes makes it possible to produce a three-dimensional network structure, which is particularly important for reducing the cracking rate of the turning points / diameter-changing sections of the tube embryo during the vulcanization process.

[0081] With reference to Example 2, Examples 6 and 7 reflect the effect of the polyamide type on the cracking rate and tensile strength of the obtained automobile oil pipe when the whisker carbon nanotubes are modified. The high-temperature tensile strength of the automobile oil pipe provided by Example 2 is higher than that of the automobile oil pipes provided by Examples 6 and 7, while the cracking rate of the automobile oil pipe provided by Example 2 is lower than that of the automobile oil pipes provided by Examples 6 and 7. The selection of polyamide 6T / 66 is conducive to improving the high-temperature tensile strength of the obtained automobile oil pipe and reducing the cracking rate at the bend / diameter-changing section.

[0082] Referring to Example 2 and Comparative Examples 1-4, although whisker carbon nanotubes were used in Comparative Example 1, the cracking rate of the automobile oil pipe provided by Comparative Example 1 was still more than 8% without polyamide modification. Analysis showed that this may be due to the fact that gaps were easily formed at the interface between the unmodified whisker carbon nanotubes and other components in the tube embryo, resulting in weaker heat conduction effect and reinforcement effect than the automobile oil pipe provided by Example 2. While in Comparative Example 2, without the use of whisker carbon nanotubes and modified whisker carbon nanotubes, the cracking rate reached more than 15%, and the cracking rate of the automobile oil pipe provided by Examples 1-7 was reduced by 85%-95% compared with the cracking rate of the automobile oil pipe provided by Comparative Example 2. In Comparative Example 3, the whisker carbon nanotubes are replaced with multi-walled carbon nanotubes. It is found that in Comparative Example 4, the tetrapod-shaped zinc oxide whiskers are replaced with zinc oxide. Combined with Example 2 and Comparative Examples 2-4, it can be seen that the cracking rate of the automobile oil pipe prepared in Example 2 using tetrapod-shaped zinc oxide whiskers and whisker carbon nanotubes is much lower than that of the automobile oil pipes of Comparative Examples 2-4, indicating that the use of tetrapod-shaped zinc oxide whiskers and whisker carbon nanotubes together has a synergistic effect in reducing the cracking rate of the turning / diameter-changing section of the automobile oil pipe.

[0083] The performance of the automobile oil pipe of Example 2 was tested. Among its conventional performance, the hardness was 72, which was greater than 70; the tensile strength was 13.88MPa, which was greater than 10MPa; the tensile elongation was 372.7%, which was greater than 250%; in the hot air aging performance, after being treated at 125°C for 72h, the hardness changed to +7, the tensile strength decreased by 8.71%, the tensile elongation decreased by -19.2%, and the compression deformation was 35.5%; the volume change rate of resistance to liquid C at room temperature was 2%, the volume change rate of resistance to oil No. 3 was 3.5%, and the adhesion strength was 1.8KN / m; ozone resistance: no cracks were observed at twice the magnification under the conditions of 100pphm×50°C×144h; low temperature bending resistance: no cracks were observed under the conditions of -40°C×70h after injecting liquid C and plugging both ends. All the above test indicators were qualified.

[0084] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An automobile oil pipe, characterized in that: The invention is made of the following components in parts by weight: 80-120 parts of NBR / PVC blended rubber, 1-2 parts of stearic acid, 6-20 parts of modified whisker carbon nanotubes, 4-5 parts of zinc oxide whiskers, 3-4.5 parts of antioxidant, 2-3 parts of compatibilizer, 25-40 parts of plasticizer, 40-50 parts of carbon black, 10-20 parts of white carbon black, 1-3 parts of vulcanizer, and 4-4.9 parts of accelerator. The modified whisker carbon nanotubes are prepared by the following method: adding whisker carbon nanotubes to a formic acid solution of polyamide to obtain a mixed solution, placing the mixed solution under ultrasonic vibration at 35-50° C. for 6-9 hours, and finally washing with ethanol, filtering, and drying to obtain modified whisker carbon nanotubes for use; The weight ratio of whisker carbon nanotubes to polyamide in the mixed solution is 20-100:1; The whisker carbon nanotube has a length of 1-15 μm, an inner diameter of 2-5 nm, and an outer diameter of 20-100 nm.

2. The automobile oil pipe according to claim 1, characterized in that: The polyamide includes one or more of polyamide 6T / 6, polyamide 6T / 66 and polyamide 6T / 6I.

3. The automobile oil pipe according to claim 1, characterized in that: The NBR / PVC blended rubber is made of NBR and PVC in a weight ratio of 0.1-9:

1.

4. The automobile oil pipe according to claim 1, characterized in that: The vulcanizing agent includes one or both of sulfur and dicumyl peroxide.

5. The automobile oil pipe according to claim 1, characterized in that: The plasticizer includes one or more of tributyl citrate, dioctyl phthalate, tri-isooctyl trimellitate and dibutyl sebacate.

6. The automobile oil pipe according to claim 1, characterized in that: The accelerator includes one or both of dimethyl dithiocarbonyl disulfide and dimorpholine disulfide.

7. A method for preparing an automobile oil pipe according to any one of claims 1 to 6, characterized in that: The following steps are involved: The components except the vulcanizer and the accelerator are subjected to internal kneading to obtain a internal kneading product, and then the internal kneading product, the vulcanizer and the accelerator are subjected to open kneading to obtain a rubber compound, and finally the rubber compound is extruded into a tube blank, and the tube blank is put on a mandrel for vulcanization to obtain the automobile oil pipe.