A method for regenerating a post-treatment catalyst after failure
By using a combined cleaning agent of strong alkali, flocculant and surfactant, combined with ultrasonic treatment and drying technology, toxic silicon species in the diesel engine after-treatment catalyst are removed, and by spraying precious metal solution, the problem of catalyst failure is solved and achieved Significant improvement in catalytic performance.
Patent Information
- Application Number
- CN202410818766.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The existing technology is difficult to effectively remove the performance degradation problem caused by silicon poisoning in the diesel engine after-treatment catalyst. In particular, it is difficult to ensure that the entire catalyst surface can be blown over and remove the carbon deposit and oil mixture, and high-temperature roasting cannot completely remove the S element, resulting in catalyst Invalid.
A combination of cleaning agents including strong alkali, flocculants and surfactants are used, and the precious metal solution is sprayed after ultrasonic treatment and drying to remove toxic silicon species in the catalyst and restore the catalytic performance.
It achieves efficient removal of toxic silicon species in the catalyst, restores the catalytic performance to a fresh state in a short time, is simple to operate, has a high silicon removal rate, and significantly improves the catalytic performance.
Smart Images

Figure CN118371275B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst regeneration, and in particular relates to a method for regenerating a post-processing catalyst that has failed. Background Art
[0002] The diesel engine aftertreatment system that meets the National VI emission requirements is composed of catalytic units such as DOC, DPF, SCR and ASC. Each component will deteriorate or even fail to varying degrees during actual use. Studies have shown that high-temperature misfires, chemical poisoning and impurity blockages such as ash are the main factors causing the above phenomenon. In the study of failure regeneration of aftertreatment catalysts, high-temperature misfires are irreversible for the degradation of catalyst performance. Chemical elements such as alkali metals Ca, Na and non-metallic P and S are common factors that cause the performance of aftertreatment catalysts to decline; the P element is mainly distributed on the surface of the catalyst coating, and P decreases from the surface of the coating to the inside of the coating. Acid washing can remove some phosphorus-containing species; S is mainly distributed in the catalyst coating close to the carrier, and S increases from the surface to the inside of the coating, and can be removed by high-temperature roasting. Ash and other particulate impurities, the current existing technology uses manual high-pressure air gun blowing regeneration technology, which has many shortcomings: first, manual blowing is difficult to ensure that the entire surface can be blown, and it is inevitable that some areas will be forgotten to blow; even if the surface is blown, it is difficult to ensure the blowing time to achieve a certain effect; second, when the DPF fails, a large amount of carbon deposits and oil stains are accumulated inside, and it is difficult to effectively blow out the accumulated mixture with simple high-pressure blowing.
[0003] The national standard does not set a limit on the silicon content of oil products. There are frequent cases of post-processing silicon poisoning caused by customers using low-quality fuel. Silicon-containing species cover the surface of the catalyst coating, causing the catalyst performance to decline or even deactivate. There is no relevant technology for the research on the regeneration method of post-processing catalyst failure caused by silicon. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for regenerating a post-processed catalyst, which can remove harmful silicon species in the poisoned catalyst and, after spraying a precious metal solution, make the catalytic performance of the regenerated catalyst close to that of a fresh catalyst.
[0005] The present invention provides a method for regenerating a post-processing catalyst after failure, comprising the following steps:
[0006] The cleaning agent and the poisoned catalyst are mixed, ultrasonically treated, washed until neutral, and dried to obtain a sample;
[0007] The cleaning agent includes a strong alkali, a flocculant and a surfactant;
[0008] The strong base is selected from sodium hydroxide and / or potassium hydroxide; the flocculant is selected from one or more of polyaluminium chloride, polyaluminium sulfate, polyferric chloride and polyferric sulfate; the surfactant is selected from one or more of disodium lauryl sulfosuccinate, polyethylene glycol ether, polyethylene glycol sulfate, polyoxyethylene ethyl ether and ethylhexyl alcohol;
[0009] The sample is sprayed with a noble metal solution to obtain a regenerated catalyst.
[0010] Preferably, the mass ratio of the strong base, flocculant and surfactant is 100:(1~20):(0.5~15).
[0011] Preferably, the power of the ultrasonic treatment is 100-2400 W, and the time of the ultrasonic treatment is 1-10 h.
[0012] Preferably, the drying temperature is 80-100° C., and the drying time is 5-10 hours.
[0013] Preferably, the poisoned catalyst is at least one of a silicon-poisoned DOC and a silicon-poisoned DPF.
[0014] Preferably, the noble metal solution is selected from a platinum salt-palladium salt mixed solution with a mass ratio of 2 to 11:1.
[0015] Preferably, the cleaning agent further comprises a color developer;
[0016] The color developer is β-carotene;
[0017] The developer accounts for 0.5-3 wt % of the strong base.
[0018] Preferably, the cleaning agent also includes an antifreeze agent;
[0019] The antifreeze agent is one or more of ethylene glycol, propylene glycol and glycerol;
[0020] The antifreeze agent accounts for 0.1-30wt% of the strong base.
[0021] The present invention provides a method for post-processing catalyst failure regeneration, comprising the following steps: mixing a cleaning agent and a poisoned catalyst, ultrasonically treating, washing to neutrality, and drying to obtain a sample; the cleaning agent comprises a strong base, a flocculant, and a surfactant; the strong base is selected from sodium hydroxide and / or potassium hydroxide; the flocculant is selected from one or more of polyaluminium chloride, polyaluminium sulfate, polyferric chloride, and polyferric sulfate; the surfactant is selected from one or more of disodium lauryl sulfosuccinate, polyethylene glycol ether, polyethylene glycol sulfate, polyoxyethylene ethyl ether, and ethylhexyl alcohol; spraying a precious metal solution on the sample to obtain a regenerated catalyst. The above method uses a cleaning agent of a specific composition, that is, a specific type of strong base, flocculant, and surfactant that work together to effectively remove toxic silicon species in the poisoned catalyst, which is time-consuming, simple to operate, and has a high silicon removal rate; after cleaning, the precious metal solution is sprayed, so that the catalytic performance of the regenerated catalyst is close to that of the fresh state. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a comparison chart of DOC performance of Example 1 of the present invention and Comparative Examples 1-7. DETAILED DESCRIPTION
[0023] The present invention provides a method for regenerating a post-processing catalyst after failure, comprising the following steps:
[0024] The cleaning agent and the poisoned catalyst are mixed, ultrasonically treated, washed until neutral, and dried to obtain a sample;
[0025] The cleaning agent includes a strong alkali, a flocculant and a surfactant;
[0026] The strong base is selected from sodium hydroxide and / or potassium hydroxide; the flocculant is selected from one or more of polyaluminium chloride, polyaluminium sulfate, polyferric chloride and polyferric sulfate; the surfactant is selected from one or more of disodium lauryl sulfosuccinate, polyethylene glycol ether, polyethylene glycol sulfate, polyoxyethylene ethyl ether and ethylhexyl alcohol;
[0027] The sample is sprayed with a noble metal solution to obtain a regenerated catalyst.
[0028] The present invention mixes a cleaning agent and a poisoned catalyst, performs ultrasonic treatment, washes until neutral, and dries to obtain a sample. The present invention uses a cleaning agent to remove poisonous silicon materials in the poisoned catalyst. Specifically, a strong base, a surfactant, and a flocculant work together to effectively remove poisonous silicon species in the poisoned catalyst. The process is short in time, simple in operation, and has a high silicon removal rate. The catalytic performance of the regenerated catalyst after cleaning is close to that of the fresh state.
[0029] The strong base in the cleaning agent of the present invention is selected from sodium hydroxide and / or potassium hydroxide; in a specific embodiment, the strong base is a sodium hydroxide aqueous solution and / or a potassium hydroxide aqueous solution; specifically, the molar ratio of sodium hydroxide in the sodium hydroxide aqueous solution to the volume ratio of water is 0.5 mol:3 L; the molar ratio of potassium hydroxide in the potassium hydroxide aqueous solution to the volume ratio of water is 0.5 mol:3 L. - Can react with SiO2: SiO2+OH - →SiO3 2- +H2O to form soluble silicates; in the process of forming soluble silicates, the above-mentioned specific types of flocculants and surfactants fully remove the oily substances in the poisoned catalyst, increase the contact area, expose the toxic silicon substances, make them easier to remove, and improve the removal efficiency.
[0030] The present invention has specific selections for the types of flocculants and surfactants. Not all types of flocculants and surfactants can act with strong alkali to achieve good removal effects on silicon in silicon-poisoned catalysts. The applicant has obtained through a large number of screenings that the above types of flocculants and surfactants can act together with strong alkali, making the silicon removal effect more excellent.
[0031] The flocculant described in the present invention is selected from one or more of polyaluminium chloride, polyaluminium sulfate, polyferric chloride and polyferric sulfate; preferably polyaluminium sulfate or polyferric chloride. The surfactant described in the present invention is selected from one or more of lauryl sulfosuccinate monoester, polyethylene glycol ether, polyethylene glycol sulfate, polyoxyethylene ethyl ether and ethylhexyl alcohol, preferably polyethylene glycol sulfate or polyoxyethylene ethyl ether. The mass ratio of the strong base, flocculant and surfactant described in the present invention is 100:(1~20):(0.5~15), preferably 100:(1~10):(1~10), more preferably 100:(1~5):(3~7). In a specific embodiment, the mass ratio of the strong base, flocculant and surfactant is 100:1.5:5.
[0032] The cleaning agent used in the present invention preferably also includes a color developer; the color developer is β-carotene; the color developer accounts for 0.5~3wt% of the strong base; specifically, the color developer accounts for 0.5wt%, 1.0wt%, 1.5wt%, 2.0wt%, 2.5wt% or 3wt% of the strong base.
[0033] The cleaning agent used in the present invention preferably also includes an antifreeze agent; the antifreeze agent is one or more of ethylene glycol, propylene glycol and glycerol; the antifreeze agent accounts for 0.1~30wt% of the strong base; specifically, the antifreeze agent accounts for 1 wt%, 2wt%, 3 wt%, 4wt%, 5wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt%, 10 wt%, 11wt%, 15 wt%, 20 wt%, 25 wt%, 28 wt%, 29 wt%, or 30 wt% of the strong base.
[0034] The power of the ultrasonic treatment in the present invention is 100-2400W, and the time of the ultrasonic treatment is 1-10h; in a specific embodiment, the power of the ultrasonic treatment is 300W or 700W; the time of the ultrasonic treatment is 1h, 3h or 5h.
[0035] The present invention removes poisonous silicon species such as silicon oxide and silicate by washing, so that the silicon-containing materials in the regenerated catalyst are greatly reduced and the catalytic performance is restored. The present invention preferably uses water for washing to neutrality; specifically, deionized water is used for washing to neutrality.
[0036] After obtaining the sample, the present invention sprays the sample with a precious metal solution to obtain a regenerated catalyst. In order to restore the catalytic performance of the regenerated catalyst as much as possible, the present invention uses the above-mentioned cleaning agent for cleaning and then continues to spray the precious metal solution. The experimental results show that the catalytic performance of the regenerated catalyst is close to that of the fresh state.
[0037] The poisoned catalyst treated by the present invention is at least one of silicon-poisoned DOC and silicon-poisoned DPF, and the precious metal solution is selected from a platinum salt-palladium salt mixed solution with a mass ratio of 2 to 11:1; in a specific embodiment, the precious metal solution is a platinum salt-palladium salt mixed solution with a mass ratio of 5:1. It can be seen from the embodiments and comparative examples of the present invention that spraying the precious metal solution significantly improves the catalytic performance of the regenerated catalyst.
[0038] In order to further illustrate the present invention, a method for regenerating a post-treatment catalyst provided by the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0039] Example 1
[0040] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0041] Step 2: Add 1.5 wt% polyaluminium sulfate.
[0042] Step 3: Add 5 wt% of polyethylene glycol sulfate.
[0043] Step 4: Add 0.5 wt% β-carotene aqueous solution.
[0044] Step 5: Add 3 wt % of propylene glycol and stir evenly to obtain cleaning agent A-1.
[0045] Step 6: Take 2L of cleaning agent A-1, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an oven at 80℃ for 6 hours.
[0046] Step 7: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0047] Comparative Example 1
[0048] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0049] Step 2: Add 5 wt% of disodium lauryl sulfosuccinate.
[0050] Step 3: Add 0.5 wt% β-carotene aqueous solution.
[0051] Step 4: Add 3 wt% of ethylene glycol and stir evenly to obtain cleaning agent B.
[0052] Step 5: Take 2L of cleaning agent B, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80℃ oven for 6 hours.
[0053] Step 6: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0054] Comparative Example 2
[0055] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0056] Step 2: Add 1.5wt% polyferric chloride.
[0057] Step 3: Add 0.5 wt% β-carotene aqueous solution.
[0058] Step 4: Add 3 wt% of ethylene glycol and stir evenly to obtain cleaning agent C.
[0059] Step 5: Take 2L of cleaning agent C, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80℃ oven for 6 hours.
[0060] Step 6: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0061] Comparative Example 3
[0062] Step 1: Dissolve 0.5 mol potassium hydroxide in 3 L of deionized water and stir at room temperature.
[0063] Step 2: Add 1.5wt% polyaluminium chloride.
[0064] Step 3: Add 5 wt% of disodium lauryl sulfosuccinate.
[0065] Step 4: Add 3 wt% of ethylene glycol and stir evenly to obtain cleaning agent D.
[0066] Step 5: Take 2L of cleaning agent D, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80℃ oven for 6 hours.
[0067] Step 6: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0068] Comparative Example 4
[0069] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0070] Step 2: Add 1.5wt% polyaluminium chloride.
[0071] Step 3: Add 5 wt% of disodium lauryl sulfosuccinate.
[0072] Step 4: Add 0.5% β-carotene aqueous solution and stir evenly to obtain cleaning agent E.
[0073] Step 5: Take 2L of cleaning agent E, heat it to 80℃, put in the silicon-poisoned DOC, adjust the power of the ultrasonic machine to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an oven at 80℃ for 6 hours.
[0074] Step 6: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0075] Comparative Example 5
[0076] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0077] Step 2: Add 1.5wt% polyaluminium chloride.
[0078] Step 3: Add 5 wt% of disodium lauryl sulfosuccinate.
[0079] Step 4: Add 0.5% β-carotene aqueous solution.
[0080] Step 5: Add 3 wt % of ethylene glycol and stir evenly to obtain cleaning agent F.
[0081] Step 6: Take 2L of cleaning agent F, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80℃ oven for 6 hours.
[0082] Comparative Example 6
[0083] Step 1: Add 1.5 wt% polyaluminium chloride to 3 L of deionized water.
[0084] Step 2: Add 5 wt% of polyethylene glycol ether.
[0085] Step 3: Add 0.5 wt% β-carotene aqueous solution.
[0086] Step 4: Add 3 wt% of ethylene glycol and stir evenly to obtain cleaning agent G.
[0087] Step 5: Take 2L of cleaning agent G, heat it to 80℃, put in the silicon-poisoned DOC, adjust the power of the ultrasonic machine to 1500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an oven at 80℃ for 6 hours.
[0088] Step 6: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0089] Comparative Example 7
[0090] Step 1: Do not use cleaning agents for cleaning. Just follow the method of dealing with failed parts on the market and use an air gun to blow for 2 hours, setting the gas pressure to 0.4MPa.
[0091] Step 2: Add soluble platinum and palladium salts to an aqueous solution at a weight ratio of 25:1 between platinum and palladium, and spray a 2 wt % noble metal solution on the purged DOC sample.
[0092] The performance test results show that the uncleaned catalyst contains toxic silicon species and has low DOC efficiency. The T50 of HC and the T90 of CO are 345°C and 358°C respectively, the maximum conversion rate of HC is 73%, and the NO conversion rate is only 1.8%. The performance of the DOC after cleaning and regeneration in the embodiment is significantly restored. The T50, T90 of HC and the T90 of CO are 177°C, 459°C and 168°C respectively. The maximum conversion rate of HC is 99%, and the NO conversion rate is as high as 48.8%. The performance of the catalyst after cleaning is close to the level of the fresh state. The cleaning agent of Comparative Example 1 does not add flocculants, and the cleaning effect is worse than that of the embodiment. The T50, T90 of HC and the T90 of CO are 196°C, 488°C and 203°C respectively. The maximum conversion rate of HC is 89%, and the NO conversion rate is 41%. The cleaning agent of Comparative Example 2 does not add surfactant, and the cleaning effect is slightly worse than that of the embodiment. The T50, T90 of HC and T90 of CO are 189°C, 476°C and 177°C, respectively. The maximum conversion rate of HC is 95%, and the NO conversion rate is 45%. The cleaning agent of Comparative Example 3 does not add β-carotene aqueous solution, and the cleaning effect is not much different from that of the embodiment. The T50, T90 of HC and T90 of CO are 175°C, 456°C and 172°C, respectively. The maximum conversion rate of HC is 96%, and the NO conversion rate is 46%. The cleaning agent of Comparative Example 4 does not add any of the components of ethylene glycol, propylene glycol, and glycerol, and the cleaning effect is not much different from that of the embodiment. The T50, T90 of HC and T90 of CO are 176°C, 453°C and 175°C, respectively. The maximum conversion rate of HC is 95%, and the NO conversion rate is 47%. In the cleaning operation of Comparative Example 5, no precious metal spraying was performed, and the cleaning effect was worse than that of the embodiment. The T50, T90 of HC and T90 of CO were 188°C, 466°C and 175°C, respectively, and the maximum conversion rate of HC was 83%, and the NO conversion rate was 40%. In the cleaning operation of Comparative Example 6, no sodium hydroxide or potassium hydroxide was added, and the cleaning effect was even worse. The T50, T90 of HC and T90 of CO were 310°C, 563°C and 266°C, respectively, and the maximum conversion rate of HC was 77%, and the NO conversion rate was only 20%. In the regeneration operation of Comparative Example 7, no cleaning agent was used, and regeneration was performed by spraying precious metal solution after purging. The regeneration effect was the worst. The T50 of HC and T90 of CO were 340°C and 341°C, respectively, and the maximum conversion rate of HC was 25%, and the NO conversion rate was only 8%.
[0093] The above results show that sodium hydroxide and potassium hydroxide are the main silicon removal components, and the synergistic effect between them and flocculants and surfactants makes the removal effect of silicon elements more excellent. β-carotene aqueous solution and ethylene glycol, propylene glycol, and glycerol have little effect on the effect of cleaning agents. Spraying of precious metal solutions can improve catalyst performance, but the improvement effect is limited. Purge regeneration operation cannot remove silicon-containing harmful substances, and spraying of precious metal solutions still has very limited catalyst performance recovery.
[0094] Comparative Example 8
[0095] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0096] Step 2: Add 1.5wt% of polysilicate aluminum ferric.
[0097] Step 3: Add 5 wt% of polyethylene glycol sulfate.
[0098] Step 4: Add 0.5 wt% β-carotene aqueous solution.
[0099] Step 5: Add 3 wt % of propylene glycol and stir evenly to obtain cleaning agent H.
[0100] Step 6: Take 2L of cleaning agent H, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80℃ oven for 6 hours.
[0101] Step 7: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0102] The performance test results show that in comparative example 8, in which polysilicate aluminum iron is used as a flocculant to prepare cleaning agent H, the DOC efficiency after cleaning and regeneration is lower than that of example 1. The T90 of HC and CO are 496°C and 268°C, respectively, the maximum conversion rate of HC is 85%, and the conversion rate of NO is 28%.
[0103] Comparative Example 9
[0104] Step 1: Dissolve 0.5 mol sodium hydroxide in 3 L of deionized water and stir at room temperature.
[0105] Step 2: Add 1.5wt% polyferric chloride.
[0106] Step 3: Add 5 wt% of γ-aminopropyltriethoxysilane.
[0107] Step 4: Add 0.5 wt% β-carotene aqueous solution.
[0108] Step 5: Add 3 wt % of propylene glycol and stir evenly to obtain cleaning agent I.
[0109] Step 6: Take 2L of cleaning agent I, heat it to 80°C, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an 80°C oven for 6 hours.
[0110] Step 7: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0111] The performance test results show that in comparative example 9, cleaning agent I is prepared with γ-aminopropyltriethoxysilane as a surfactant, and the DOC efficiency after cleaning and regeneration is lower than that of example 1. The T90 of HC and CO are 486°C and 248°C, respectively, the maximum conversion rate of HC is 89%, and the conversion rate of NO is 26%. The above results show that when flocculants and surfactants outside the scope of protection of this patent are used, the DOC performance after cleaning and regeneration is not significantly improved.
[0112] Table 1 DOC performance after treatment with different cleaning agents and regeneration processes
[0113]
[0114] Example 2
[0115] Step 1: Dissolve 0.5 mol potassium hydroxide in 3 L of deionized water and stir at room temperature.
[0116] Step 2: Add 1.5wt% polyferric chloride.
[0117] Step 3: Add 5 wt% of polyoxyethylene ethyl ether.
[0118] Step 4: Add 0.5 wt% β-carotene aqueous solution.
[0119] Step 5: Add 3 wt % of propylene glycol and stir evenly to obtain cleaning agent A-2.
[0120] Step 6: Take 2L of cleaning agent A-2, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 700W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an oven at 80℃ for 4 hours.
[0121] Step 7: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0122] Example 3
[0123] Step 1: Dissolve 0.5 mol potassium hydroxide in 3 L of deionized water and stir at room temperature.
[0124] Step 2: Add 1.5 wt% polyaluminium sulfate.
[0125] Step 3: Add 5 wt% of polyoxyethylene ethyl ether.
[0126] Step 4: Add 0.5 wt% β-carotene aqueous solution.
[0127] Step 5: Add 3 wt % of propylene glycol and stir evenly to obtain cleaning agent A-3.
[0128] Step 6: Take 2L of cleaning agent A-3, heat it to 80℃, put in the silicon-poisoned DOC, adjust the ultrasonic machine power to 500W for 2 hours, then wash with 5L of deionized water until neutral, and dry in an oven at 80℃ for 6 hours.
[0129] Step 7: Add soluble platinum and palladium salts to the aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 2 wt% of the precious metal solution on the dried DOC sample.
[0130] The performance test results show that the DOC efficiency of Example 2 after cleaning and regeneration is equivalent to that of Example 1. The T90 of HC and CO are 453°C and 176°C, respectively, the maximum conversion rate of HC is 98%, and the conversion rate of NO is 48%. The DOC efficiency of Example 3 after cleaning and regeneration is equivalent to that of Example 1. The T90 of HC and CO are 456°C and 179°C, respectively, the maximum conversion rate of HC is 97.8%, and the conversion rate of NO is 96%. The above results show that the cleaning agents prepared by different combinations of desiliconizers, flocculants and surfactants involved in the present invention all have good desiliconization efficiency, and the DOC performance is significantly improved after cleaning and regeneration.
[0131] The present invention is applicable to but not limited to the cleaning and regeneration of silicon-poisoned DOC, DPF and other diesel engine post-treatment catalysts. Now, examples and comparative examples are used to illustrate that the cleaning and regeneration method of the present invention can achieve the performance recovery of silicon-poisoned DPF.
[0132] Example 4: Cleaning and regeneration of DPF
[0133] Step 1: Take 2L of cleaning agent A, heat it to 80℃, put it into the silicon-poisoned DPF, adjust the ultrasonic machine power to 500W for 2 hours, then wash it with 5L of deionized water until it is neutral, and dry it in an 80℃ oven for 6 hours.
[0134] Step 2: Add soluble platinum and palladium salts to an aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 0.1 wt% of the precious metal solution on the purged DPF sample.
[0135] Comparative Example 10: Purge regeneration of DPF
[0136] Step 1: Do not use cleaning agents for cleaning. Just follow the method of dealing with failed parts on the market and use an air gun to blow for 2 hours, setting the gas pressure to 0.4MPa.
[0137] Step 2: Add soluble platinum and palladium salts to an aqueous solution at a weight ratio of 5:1 between platinum and palladium, and spray 0.1 wt% of the precious metal solution on the purged DPF sample.
[0138] Performance test results show that the unwashed catalyst contains toxic silicon species. The laboratory back pressure tester measured the DPF back pressure as high as 26.55mbar, PN 23 Emissions 2.1E+13mg kWh -1 The performance of DPF in Example 4 after cleaning and regeneration is close to that of fresh state, with a back pressure of 13.33 mbar, which is equivalent to the level of normal parts, and the PN capture efficiency is significantly restored. The performance of DPF in Example 10 is improved to a certain extent, but the performance is far from meeting the emission requirements.
[0139] Table 2 DPF performance after different regeneration processes
[0140]
[0141] The silicon removal agent, flocculant and surfactant of the present invention work together to achieve efficient removal of silicon-containing harmful substances and significantly improve the performance of silicon-poisoned and failed parts. The cleaning and regeneration differences of different flocculants and surfactants are now explained through examples.
[0142] As can be seen from the above embodiments, the present invention provides a method for post-processing catalyst failure regeneration, comprising the following steps: mixing a cleaning agent and a poisoned catalyst, ultrasonically treating, washing to neutrality, and drying to obtain a sample; the cleaning agent comprises a strong base, a flocculant, and a surfactant; the strong base is selected from sodium hydroxide and / or potassium hydroxide; the flocculant is selected from one or more of polyaluminium chloride, polyaluminium sulfate, polyferric chloride, and polyferric sulfate; the surfactant is selected from one or more of disodium lauryl sulfosuccinate, polyethylene glycol ether, polyethylene glycol sulfate, polyoxyethylene ethyl ether, and ethylhexyl alcohol; spraying a precious metal solution on the sample to obtain a regenerated catalyst. The above method uses a cleaning agent of a specific composition, that is, a specific type of strong base, flocculant, and surfactant that work together to effectively remove toxic silicon species in the poisoned catalyst, which is time-consuming, simple to operate, and has a high silicon removal rate; after cleaning, the precious metal solution is sprayed, so that the catalytic performance of the regenerated catalyst is close to that of the fresh state.
[0143] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for regenerating a post-processing catalyst after failure. It is characterized in that The following steps are involved: The cleaning agent and the silicon-poisoned catalyst are mixed, subjected to ultrasonic treatment, washed to neutrality, and dried to obtain a sample; the silicon-poisoned catalyst is at least one of a silicon-poisoned DOC and a silicon-poisoned DPF; The cleaning agent comprises a strong base, a flocculant and a surfactant; the mass ratio of the strong base, the flocculant and the surfactant is 100:(1-20):(0.5-15); The strong base is selected from sodium hydroxide and / or potassium hydroxide; the flocculant is selected from polyaluminium sulfate or polyferric chloride; the surfactant is selected from polyethylene glycol sulfate or polyoxyethylene ethyl ether; The sample is sprayed with a noble metal solution to obtain a regenerated catalyst.
2. The method according to claim 1, It is characterized in that The power of the ultrasonic treatment is 100-2400W, and the time of the ultrasonic treatment is 1-10h.
3. The method according to claim 1, It is characterized in that The drying temperature is 80-100° C., and the drying time is 5-10 hours.
4. The method according to claim 1, It is characterized in that The noble metal solution is selected from a platinum salt-palladium salt mixed solution with a mass ratio of 2 to 11:
1.
5. The method according to claim 1, It is characterized in that The cleaning agent also includes a color developer; The color developer is β-carotene; The developer accounts for 0.5-3 wt % of the strong base.
6. The method according to claim 1, It is characterized in that The cleaning agent also includes antifreeze; The antifreeze agent is one or more of ethylene glycol, propylene glycol and glycerol; The antifreeze agent accounts for 0.1-30wt% of the strong base.
Citation Information
Patent Citations
Regeneration method of sulfur-poisoned selective catalytic reduction (SCR) denitrification catalyst
CN104028315A
Regeneration method for inactivated selective catalytic reduction (SCR) denitration catalyst
CN105080622A
DPF coating structure and preparation method thereof
CN116850707A
Regeneration cleaning agent and regeneration method for arsenic poisoning denitration catalyst
CN117065806A
Method for regenerating solid catalyst
JP2007326069A