Method and device for co-producing synthesis gas and carbon nanotubes by methane dry reforming reaction

By using a Ni-based catalyst with an alumina carrier and a quartz wool-metal casing structure in the methane dry reforming reaction, the problems of catalyst carbon deposition and low H2/CO ratio were solved, and efficient carbon nanotube separation and The high H2/CO ratio of syngas is suitable for normal pressure conditions.

CN118373413BActive Publication Date: 2024-10-18ZHEJIANG UNIV OF TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410840683.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-18
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

In the methane dry reforming reaction, Ni-based catalysts are easily deactivated due to carbon deposition, and the H2/CO ratio of the generated syngas is usually lower than 1, making it difficult to apply directly.

Method used

Ni-based catalysts and alumina or alumina-silica are used as carriers, and quartz wool and metal casing structures are set up in the reaction tube to form an upper layer of quartz wool, a catalyst layer and a lower layer of quartz wool, and roughened surfaces are attached to the metal casing. On the surface, high space velocity conditions are used to grow carbon nanotubes and take them away from the catalyst surface to increase the H2/CO ratio.

Benefits of technology

It effectively avoids catalyst deactivation, improves the H2/CO ratio of syngas, realizes efficient separation of carbon nanotubes and direct application of syngas, and the reaction can be carried out under normal pressure, avoiding the need for high-pressure equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118373413B_ABST
    Figure CN118373413B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and device for co-producing synthesis gas and carbon nanotubes by dry reforming reaction of methane. The device used in the method includes a reaction tube as shown in the figure; the catalyst used in the method is a Ni-based catalyst; the method includes: introducing a reaction raw gas composed of CH4, CO2 and carrier gas from the air inlet of the reaction tube, performing a methane dry reforming reaction under high reaction space velocity conditions, collecting synthesis gas through the gas outlet of the reaction tube, and collecting carbon nanotubes on the surface of a metal sleeve lower than the lower quartz wool. The present invention not only avoids the deactivation caused by carbon deposition covering the reaction active centers on the surface of the Ni-based catalyst, but also can obtain carbon nanotubes with higher economic value; at the same time, the H2 / CO ratio in the obtained synthesis gas exceeds 1.0, which is more conducive to the subsequent direct application of the synthesis gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method and a device for co-producing synthesis gas (CO+H2) and carbon nanotubes by utilizing a methane dry reforming reaction. Background Art

[0002] The dry reforming of methane (DRM) reaction has attracted widespread interest and high attention from scientists and industrial circles in various countries because it can use CH4 and CO2 as reactants to reduce greenhouse gas emissions and produce synthesis gas (CO+H2, a series of important chemical products such as long-chain hydrocarbons and methanol can be prepared using synthesis gas as raw materials).

[0003] After extensive research, it was found that the methane dry reforming reaction is a complex reaction system, which includes the following reactions:

[0004] ; (1-1)

[0005] ; (1-2)

[0006] ; (1-3)

[0007] ; (1-4)

[0008] ; (1-5)

[0009] In the application field of methane dry reforming reaction, CN113955742A discloses a process for preparing carbon nanotubes by carbon dioxide-methane reforming technology. The catalyst used in the process is a nanotube with a diameter of 15-20 × 10 -15 The invention discloses a honeycomb solid cobalt-based catalyst of mm, wherein the catalyst is synthesized by a co-impregnation method, with alumina as a carrier, cobalt as an active component, and any one of the oxides of rare earth metals yttrium and cerium as an additive. The process prepares carbon nanotubes and generates synthesis gas in the catalyst bed of the reforming reactor, wherein the dry reforming reaction temperature is 800°C and the pressure is 0.7MPa. In addition, the generated carbon nanotubes are attached to the surface of the catalyst, so ultrasonic separation is required in the separation device. Therefore, the CO2-CH4 dry reforming technology for preparing carbon nanotubes described in the patent requires equipment that is resistant to both high pressure and high temperature, and there is a problem of catalyst deactivation due to incomplete separation of the catalyst and the carbon nanotubes.

[0010] According to a large number of literature reports, Ni-based catalysts have been widely used in DRM reactions due to their low cost and relatively high catalytic activity. However, Ni-based catalysts are often deactivated due to sintering and carbon deposition during the reaction. At the same time, due to the presence of the reverse water gas shift reaction (1-3), the H2 / CO ratio in the DRM reaction product is usually lower than 1, which brings inconvenience to the direct use of the synthesis gas generated by the DRM reaction (for example: directly applied to the Fischer-Tropsch synthesis reaction, 2n H2+ n CO – n(CH2)+nH2O). Therefore, how to inhibit the side reactions (1-4) and (1-5) that cause carbon deposition during the DRM reaction and improve the anti-carbon deposition performance of Ni-based DRM catalysts and the product H2 / CO ratio is one of the current focuses of related research fields.

[0011] CN114249300A discloses the application of a specific microstructure alumina supported Ni-based catalyst in plasma catalytic methane dry reforming to produce synthesis gas. This patent improves the anti-sintering ability of Ni active centers by regulating the microstructure of the catalyst, and couples plasma with a specific microstructure catalyst to improve the reaction performance and energy efficiency of low-temperature methane dry reforming to produce synthesis gas. However, this technical solution does not generate carbon nanotubes. Summary of the invention

[0012] The object of the present invention is to provide a method and apparatus for co-producing synthesis gas and carbon nanotubes by means of methane dry reforming reaction, so as to make it easier to separate the catalyst and the carbon nanotubes, thereby avoiding deactivation caused by carbon deposits covering the reaction active centers on the surface of the Ni-based catalyst, and at the same time improving the H2 / CO ratio of the synthesis gas.

[0013] The technical solution of the present invention is described in detail below.

[0014] In a first aspect, the present invention provides a method for co-producing synthesis gas and carbon nanotubes by dry reforming reaction of methane, wherein the device used in the method comprises a reaction tube, wherein the upper end and the lower end of the reaction tube are respectively provided with an air inlet and an air outlet, wherein the interior of the reaction tube is sequentially filled with quartz wool-catalyst-quartz wool from top to bottom to form an upper layer of quartz wool, a catalyst layer and a lower layer of quartz wool, wherein the upper layer of quartz wool and the lower layer of quartz wool fix the catalyst layer inside the reaction tube, and wherein the reaction tube further comprises a metal sleeve, wherein the metal sleeve passes through the three-layer structure of quartz wool-catalyst-quartz wool, and the head of the metal sleeve is higher than the upper layer of quartz wool, the tail of the metal sleeve is lower than the lower layer of quartz wool, and the metal sleeve lower than the lower layer of quartz wool has a rough surface;

[0015] The catalyst used in the method is a Ni-based catalyst, which is composed of metal Ni particles and an oxide carrier, the loading amount of the metal Ni particles is 10-15wt%, the particle size of the metal Ni particles is 6-8 nanometers, and the oxide carrier is aluminum oxide, silicon oxide, or an aluminum oxide-silicon oxide mixture;

[0016] The method comprises: introducing a reaction raw gas consisting of CH4, CO2 and a carrier gas from the gas inlet of a reaction tube, and reacting the reaction raw gas at a reaction space velocity of at least 230,000 cm 3 g -1 h -1 The methane dry reforming reaction is carried out under the conditions of , the synthesis gas is collected through the gas outlet of the reaction tube, and the carbon nanotubes are collected on the surface of the metal sleeve below the lower layer of quartz wool.

[0017] In the method of co-producing synthesis gas and carbon nanotubes by methane dry reforming reaction of the present invention, the carbon formed by CH4 cracking or CO disproportionation reaction during the reaction process will first dissolve on the metal Ni surface to form a nickel carbide intermediate (Ni3C), and then the carbon will continue to diffuse and deposit to form filamentous carbon nanotubes. When the filamentous carbon nanotubes grow toward the outside of the metal particles (attached to Ni particles), the metal Ni species can be separated from the metal Ni particles. This separation will neither cause a change in the size of the metal Ni particles nor significantly reduce or block the reaction active sites. During the reaction, due to the use of a higher space velocity condition, the metal Ni particles wrapped in the carbon tube will be carried away from the catalyst surface by the gas. Under the condition of installing the metal sleeve, the carbon tube containing the metal Ni particles carried away from the catalyst surface by the gas is adsorbed by the rough metal sleeve surface under the lower quartz wool due to magnetism, and the CO molecules in the tail gas are further disproportionated in the part with suitable temperature, thereby causing CO to decrease, so that H2 / CO>1. It can be understood by those skilled in the art that the longer the length of the rough metal sleeve under the lower quartz wool, the more helpful it is to adsorb the carbon tube containing the metal Ni particles.

[0018] Preferably, the metal Ni particles in the Ni-based catalyst are spherical. Preferably, the loading amount of the metal Ni particles in the Ni-based catalyst is 10wt%. Preferably, the oxide carrier is alumina, and the alumina has a cylindrical pore structure. It is further preferred that the specific surface area of ​​the alumina is 200-220 m 2 g -1 , pore volume is 0.5-0.7 cm 3 g -1 , pore size is 10-12 nm.

[0019] The Ni-based catalyst of the present invention can be prepared by the following method: preparing a nickel salt into a nickel salt solution; uniformly dropping the nickel salt solution onto an oxide support, drying after sufficient impregnation, and then calcining at a high temperature in an air atmosphere, obtaining a calcined product after cooling, and reducing the calcined product to obtain a Ni-based catalyst.

[0020] The loading amount of the metal Ni particles in the present invention is based on the assumption that the Ni element in the nickel salt is completely loaded onto the oxide support to form metal Ni particles during the preparation process. The loading amount of the metal Ni particles = m Ni / (m Ni +m 氧化物载体 )×100%.

[0021] Preferably, in the preparation of the Ni-based catalyst, the impregnation conditions are: standing at room temperature for 1-3 h.

[0022] Preferably, in the preparation of the Ni-based catalyst, the nickel salt solution is an ethanol solution of nickel nitrate.

[0023] Preferably, in the preparation of the Ni-based catalyst, the drying conditions are: drying at 95-105° C. for 10-14 h.

[0024] Preferably, in the preparation of the Ni-based catalyst, the high temperature calcination conditions are: heating to 390-410° C. at a rate of 9-11° C. / min, and calcining in an air atmosphere for 4-6 h.

[0025] Preferably, in the preparation of the Ni-based catalyst, the specific surface area of ​​the calcined product is 160-180 m 2 g -1 , pore diameter is 10-12 nm, pore volume is 0.4-0.6 cm 3 g -1 .

[0026] Preferably, in the preparation of the Ni-based catalyst, the reduction conditions are: reduction at 690-710° C. for 1-3 h in a hydrogen atmosphere.

[0027] Preferably, the metal sleeve is a stainless steel sleeve.

[0028] In the present invention, the rough surface of the metal sleeve can be obtained by sandpaper grinding.

[0029] Preferably, the carrier gas in the reaction raw gas is nitrogen, wherein the gas molar ratio CH4:CO2=1:1.

[0030] Preferably, the reaction temperature of the methane dry reforming reaction is 680-710° C., and the reaction pressure is normal pressure.

[0031] Preferably, the reaction space velocity is 230000-260000 cm 3 g -1 h -1 .

[0032] In a second aspect, the present invention provides a device for co-producing synthesis gas and carbon nanotubes through methane dry reforming reaction, the device comprising a reaction tube, the upper and lower ends of the reaction tube being respectively provided with an air inlet and an air outlet, the constant temperature zone inside the reaction tube being sequentially filled with quartz wool-catalyst-quartz wool from top to bottom to form an upper layer of quartz wool, a catalyst layer and a lower layer of quartz wool, the upper layer of quartz wool and the lower layer of quartz wool fixing the catalyst layer inside the reaction tube, the reaction tube further comprising a metal sleeve, the metal sleeve passing through the three layers of quartz wool-catalyst-quartz wool, and the head of the metal sleeve being higher than the upper layer of quartz wool and the metal sleeve being lower than the lower layer of quartz wool having a rough surface.

[0033] Furthermore, the device also includes a heater to heat the reaction tube.

[0034] Furthermore, the device also includes a thermocouple, which is fixed in the metal sleeve to measure the temperature in the reaction tube.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] (1) The present invention comprehensively optimizes the catalyst, reactor structure and reaction process parameters, so that in the DRM reaction process, not only synthesis gas (H2+CO) and carbon nanotubes with high economic value are co-produced, but also the catalyst and carbon nanotubes are easy to separate, thereby avoiding deactivation caused by carbon deposition covering the reaction active centers on the surface of the Ni-based catalyst; at the same time, the H2 / CO ratio in the obtained synthesis gas exceeds 1.0, which is more conducive to the subsequent direct application of the synthesis gas.

[0037] (2) The present invention optimizes the structure of the Ni-based catalyst, so that it not only has good catalytic performance for methane dry reforming reaction, but also can generate filamentous carbon nanotubes on its surface. The filamentous carbon nanotubes are easily carried away from the catalyst surface by the gas, thereby avoiding the deactivation of the catalyst due to carbon deposition covering the reaction active centers on the surface of the Ni-based catalyst.

[0038] (3) The methane dry reforming reaction of the present invention can be carried out at normal pressure without the need to use high-pressure resistant equipment.

[0039] (4) The device for co-producing synthesis gas and carbon nanotubes by methane dry reforming reaction provided by the present invention is simple in design but highly efficient. By providing a metal sleeve, not only carbon nanotubes with high economic value are obtained, but also the H2 / CO ratio in the obtained synthesis gas exceeds 1.0, which is more conducive to the subsequent direct application of the synthesis gas. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 : XRD pattern (X-ray diffraction pattern) of the Ni-based catalyst prepared in Example 1.

[0041] Figure 2 : TEM image (transmission electron microscope image) of the Ni-based catalyst prepared in Example 1.

[0042] Figure 3 : Diagram of the reaction tube structure containing a stainless steel sleeve, wherein 1-air inlet, 2-air outlet, 3-stainless steel sleeve, 4-upper layer of quartz wool, 5-catalyst layer, 6-lower layer of quartz wool, 7-carbon nanotubes.

[0043] Figure 4 : The variation of H2 / CO ratio in the tail gas of Example 2 with reaction time (Ni-based catalyst under hydrogen atmosphere, after 700 o C reduction, using a reaction tube with a stainless steel cannula).

[0044] Figure 5 : TEM image of carbon nanotubes.

[0045] Figure 6 : Ni of Ni catalyst after 5h reaction 2p XPS diagram (X-ray photoelectron spectroscopy).

[0046] Figure 7 : TEM image of Ni catalyst after 5 h of reaction.

[0047] Figure 8 : HAADF-STEM image (high-angle annular dark field image of scanning transmission electron microscope) of Ni catalyst after 5h of reaction and EDS mapping (energy dispersive X-ray spectroscopy mapping) of C, O, Al and Ni.

[0048] Fig. 9 : Diagram of the reaction tube structure without a stainless steel sleeve, wherein 1-air inlet, 2-air outlet, 4-upper layer of quartz wool, 5-catalyst layer, 6-lower layer of quartz wool.

[0049] Fig.10 : Comparative Example 1: The ratio of H2 / CO in the tail gas changes with the reaction time (Ni-based catalyst under hydrogen atmosphere, after 700 o C reduction, using a reaction tube without a stainless steel sleeve).

[0050] Fig.11 : A graph showing the variation of the H2 / CO ratio in the reaction tail gas with reaction time in Comparative Example 2 (the Ni-based catalyst is not reduced, and a reaction tube containing a stainless steel sleeve is used). DETAILED DESCRIPTION

[0051] The technical solution of the present invention is further described below with specific embodiments, but the protection scope of the present invention is not limited by the following embodiments.

[0052] A device for co-producing synthesis gas and carbon nanotubes by dry reforming of methane comprises a reaction tube, such as Figure 3 As shown, the upper end and the lower end of the reaction tube are respectively provided with an air inlet 1 and an air outlet 2, and the interior of the reaction tube is filled in the order of quartz wool-catalyst-quartz wool from top to bottom to form an upper quartz wool 4, a catalyst layer 5 and a lower quartz wool 6. The upper quartz wool 4 and the lower quartz wool 6 fix the catalyst layer 5 inside the reaction tube. The reaction tube also contains a stainless steel sleeve 3, which passes through the three layers of upper quartz wool 4-catalyst layer 5-lower quartz wool 6, and the head of the stainless steel sleeve 3 is higher than the upper quartz wool 4, and the stainless steel sleeve lower than the lower quartz wool 6 has a rough surface.

[0053] Furthermore, the device also includes a heater to heat the reaction tube.

[0054] Furthermore, the device also includes a thermocouple, which is fixed in the stainless steel sleeve to measure the temperature in the reaction tube.

[0055] Embodiment 1:

[0056] First, weigh ~1.1 g Ni(NO3)2ˑ6H2O and dissolve it in an appropriate amount of ethanol (excessive impregnation, no less than 10 ml) to form a nickel nitrate solution. Weigh 2 g Al2O3 carrier (Alfa Aesa, with a cylindrical pore structure and a specific surface area of ​​~211.6 m 2 g -1 , with a pore volume of ~0.61 cm 3 g -1 , pore size is ~11.6 nm), the nickel nitrate solution is evenly added to the Al2O3 carrier, then placed at room temperature for 2 h, dried in an oven (100 °C) for 12 h, taken out, placed in a muffle furnace, heated to 400 °C at a rate of 10 °C / min, and calcined in air for 5 h to obtain a calcined product. The specific surface area of ​​the calcined product is ~172 m 2 g -1 , the pore volume is ~0.5 cm 3 g -1, the pore size is ~11.7 nm. The calcined product was reduced at 700 ° C in a hydrogen atmosphere for 2 h and then cooled to room temperature to obtain a Ni-based catalyst (metal Ni loading is 10 wt.%). In order to characterize the Ni-based catalyst, 1% O2 / Ar was introduced for passivation treatment for 1 h. After the passivation treatment, the Ni-based catalyst was analyzed by TEM and X-ray diffraction (XRD) respectively for the catalyst crystal phase, grain size and morphology. Figure 1 As shown in the figure, the diffraction peaks at 2θ ≈ 44.5°, 52° and 76° can be attributed to the Ni (111), (200), and (220) crystal planes, respectively. According to the Scherrer equation, the particle size of the metal Ni particles in the Ni-based catalyst is about 7 nm. Figure 2 As shown, the Ni-based catalyst mainly contains spherical Ni particles with an average particle size of about 8 nm.

[0057] Embodiment 2:

[0058] The fillers are sequentially loaded into the reactor in the order of quartz wool, Ni-based catalyst, and quartz wool. Figure 3 In the reaction tube shown, the Ni-based catalyst actually loaded here is the calcined product obtained in Example 1. Before the reaction, it is necessary to use hydrogen reduction at 700°C for 2 h to obtain the Ni-based catalyst of the present invention. Then the reaction is carried out at 700°C. The composition of the reaction raw gas is: CH4: CO2: N2 = 46 mol%: 46 mol%: 8 mol%; reaction pressure: normal pressure; reaction space velocity is 240000 cm 3 g -1 h -1 . CH4, CO2, and CO gases were analyzed online for qualitative and quantitative analysis by Shimadzu GC-2014ATF, and the chromatographic carrier gas was high-purity He. CH4, CO2, CO, and N2 in the tail gas were separated by TDX-01 packed columns and detected by thermal conductivity detector (TCD). H2 in the tail gas was analyzed online for qualitative and quantitative analysis by Agilent 6890N, and the chromatographic carrier gas was high-purity Ar. H2 in the tail gas was separated by Porapak Q and 5A packed columns and detected by thermal conductivity detector (TCD). Figure 4 It shows that after the reaction at 700℃, the H2 / CO ratio in the tail gas can exceed 1.0. In addition, after 5 hours of reaction, the surface of the stainless steel sleeve in the reaction tube (see Figure 3 ) collected about 0.5 g of carbon nanotubes (see Figure 5 ). Figure 6 Ni is the Ni-based catalyst after 5 hours of reaction. 2p XPS picture. Figure 6It can be seen that the Ni catalyst after the reaction has corresponding XPS peaks at electron binding energies of about ~853.4 eV, ~857.0 eV, ~870.7 eV, and ~874.5 eV. According to literature reports [J. Hao, GF Zhang, YT Zhang, etal., Electrochimica Acta 320 (2019) 134631; JF Moulder, WF Stickle, PE Sobol, KD Bomben, Nickel, in: J. Chastain (Ed.), Handbook of X-rayPhotoelectron Spectroscopy, Perkin-Elmer Corporation, Minnesota, 1992, pp.84–85], the peaks at around ~853.4 eV and 870.7 eV can be attributed to the Ni of nickel carbide. 2p3 / 2 and Ni 2p1 / 2 The peaks at ~857.0 eV and 874.5 eV can be attributed to Ni 2p3 / 2 and Ni 2p1 / 2 The peaks with binding energies around ~862.7 eV and 880.8 eV belong to their satellite peaks. Combining the above data, it can be seen that nickel carbide species exist in the Ni catalyst after the reaction. Figure 7 and 8 The TEM and EDX-mapping images of the catalyst after 5 hours of reaction. Figure 7 As can be seen from (a), the Ni catalyst after the reaction mainly contains spherical particles. According to the particle size distribution statistics, the average particle size is about ~8 nm, which indicates that the particles did not sinter during the reaction. The crystal form of the particles was further analyzed by HRTEM. Figure 7 As shown in (c), the lattice fringe spacing of the spherical particles is 2.30 Å, corresponding to the Ni3C (100) crystal plane [L. He, Journal of Magnetism and Magnetic Materials, 322 (2010) 1991-1993], which indicates that Ni3C particles exist in the catalyst. In addition, TEM analysis further revealed that a large number of tubular or filamentous carbon species appeared on the surface of the catalyst sample ( Figure 7 (b)). From Figure 8It can be found that in addition to the catalyst particle agglomerates (see the red rectangular area in the figure), there is also an obvious tubular carbon species in the sample (see the white arrow in the figure). Element mapping analysis shows that O and Al elements exist in the entire analysis area, while Ni element only corresponds to the white bright spot in the analysis area. By analogy, the white bright spot in the tubular carbon species in the figure also corresponds to the Ni species. On the other hand, ICP-MS analysis of the catalyst after 5 hours of reaction showed that the metal Ni content in the catalyst was 5.3 wt.%. The above analysis results show that carbon nanotubes are generated outside the catalyst particle agglomerates, and metal Ni (white bright spot) is attached to the surface of the carbon nanotubes, so Ni is separated from the carrier surface.

[0059] Combined with the above characterization analysis, during the reaction process, the carbon formed by the cracking of CH4 or the disproportionation reaction of CO will first dissolve on the surface of the metal Ni to form the intermediate Ni3C, and then the carbon will continue to diffuse and deposit to form filamentary carbon nanotubes. When the carbon nanotubes grow toward the outside of the metal particles (attaching Ni particles), the metal Ni species can be separated from the metal Ni particles. This separation will neither cause a change in the size of the metal Ni particles nor significantly reduce or block the reaction active sites. During the reaction, due to the use of a higher space velocity condition, this part of the metal Ni particles encapsulated in the carbon tubes will be carried away from the catalyst surface by the gas, so the metal Ni content in the catalyst will decrease after the reaction, but the metal Ni particle size in the catalyst has not changed. When using such as Figure 3 When the reaction tube shown in the figure is installed with a metal sleeve, the carbon tube containing metallic Ni species carried away from the catalyst surface by the gas is adsorbed by the metal sleeve due to magnetism, and the CO molecules in the exhaust gas undergo a disproportionation reaction at the appropriate temperature, resulting in the H2 / CO ratio of the catalyst exceeding 1.0 ( Figure 4 ).

[0060] Comparative Example 1:

[0061] The fillers are sequentially loaded into the reactor in the order of quartz wool, Ni-based catalyst, and quartz wool. Fig. 9 In the reaction tube shown, the Ni-based catalyst actually loaded here is the calcined product obtained in Example 1. Before the reaction, it is necessary to use hydrogen reduction at 700°C for 2 h to obtain the Ni-based catalyst of the present invention. Then the reaction is carried out at 700°C. The composition of the reaction raw gas is: CH4: CO2: N2 = 46 mol%: 46 mol%: 8 mol%; reaction pressure: normal pressure; reaction space velocity is 240000 cm 3 g -1 h -1. CH4, CO2, and CO gases were analyzed online for qualitative and quantitative analysis by Shimadzu GC-2014ATF, and the chromatographic carrier gas was high-purity He. CH4, CO2, CO, and N2 in the tail gas were separated by TDX-01 packed columns and detected by thermal conductivity detector (TCD). H2 in the tail gas was analyzed online for qualitative and quantitative analysis by Agilent 6890N, and the chromatographic carrier gas was high-purity Ar. H2 in the tail gas was separated by Porapak Q and 5A packed columns and detected by thermal conductivity detector (TCD). Fig.10 It shows that after the reaction at 700°C, the H2 / CO ratio in the tail gas is lower than 1 (~0.92). Since the stainless steel sleeve is not installed in the reaction tube, the carbon nanotubes are not collected. By comparing Example 1 with Comparative Example 1, it is shown that the internal components in the reaction tube play an important role in collecting the carbon nanotubes formed during the reaction and improving the H2 / CO ratio.

[0062] Comparative Example 2:

[0063] The fillers are sequentially loaded into the reactor in the order of quartz wool, Ni-based catalyst, and quartz wool. Figure 3 In the reaction tube shown, the Ni-based catalyst actually loaded here is the calcined product obtained in Example 1. Before the reaction, the Ni-based catalyst was not subjected to reduction pretreatment under hydrogen atmosphere, but directly reacted at 700°C. The reaction raw gas composition was: CH4: CO2: N2 = 46 mol%: 46 mol%: 8 mol%; reaction pressure: normal pressure; reaction space velocity was 240000 cm 3 g -1 h -1 . CH4, CO2, and CO gases were analyzed online for qualitative and quantitative analysis by Shimadzu GC-2014ATF, and the chromatographic carrier gas was high-purity He. CH4, CO2, CO, and N2 in the tail gas were separated by TDX-01 packed columns and detected by thermal conductivity detector (TCD). H2 in the tail gas was analyzed online for qualitative and quantitative analysis by Agilent 6890N, and the chromatographic carrier gas was high-purity Ar. H2 in the tail gas was separated by Porapak Q and 5A packed columns and detected by thermal conductivity detector (TCD). Fig.11 It shows that after the reaction at 700°C, the H2 / CO ratio in the tail gas is lower than 0.7. At the same time, even if the stainless steel sleeve is installed, no carbon nanotubes are collected. By comparing Example 1 and Comparative Example 2, it is shown that the use of 700°C hydrogen pretreatment has an important effect on the co-production of synthesis gas and carbon nanotubes during the reaction process. At the same time, it also shows that the structure and properties of the Ni-based catalyst have an important influence on the co-production of synthesis gas and carbon nanotubes during the reaction process.

Claims

1. A method for co-producing synthesis gas and carbon nanotubes by dry reforming of methane, characterized in that: The device used in the method comprises a reaction tube, wherein the upper end and the lower end of the reaction tube are respectively provided with an air inlet and an air outlet, wherein the interior of the reaction tube is sequentially filled with quartz wool-catalyst-quartz wool from top to bottom to form an upper layer of quartz wool, a catalyst layer and a lower layer of quartz wool, wherein the upper layer of quartz wool and the lower layer of quartz wool fix the catalyst layer inside the reaction tube, and wherein the reaction tube further comprises a metal sleeve, wherein the metal sleeve passes through the three-layer structure of quartz wool-catalyst-quartz wool, and wherein the head of the metal sleeve is higher than the upper layer of quartz wool, the tail of the metal sleeve is lower than the lower layer of quartz wool, and the metal sleeve lower than the lower layer of quartz wool has a rough surface; The catalyst used in the method is a Ni-based catalyst, which is composed of metal Ni particles and an oxide carrier, the loading amount of the metal Ni particles is 10-15wt%, the particle size of the metal Ni particles is 6-8 nanometers, and the oxide carrier is aluminum oxide, silicon oxide, or an aluminum oxide-silicon oxide mixture; The method comprises: introducing a reaction raw gas consisting of CH4, CO2 and a carrier gas from the gas inlet of a reaction tube, and reacting the reaction raw gas at a reaction space velocity of at least 230,000 cm 3 g -1 h -1 Under the condition of installing a metal sleeve, the carbon nanotubes containing metal Ni particles carried away from the catalyst surface by the gas are adsorbed by the rough metal sleeve surface under the lower quartz wool due to magnetism, and the carbon nanotubes are collected on the metal sleeve surface below the lower quartz wool.

2. The method according to claim 1, characterized in that: The metal Ni particles in the Ni-based catalyst are spherical.

3. The method according to claim 1, characterized in that: The oxide support is aluminum oxide, and the aluminum oxide has a cylindrical pore structure.

4. The method according to claim 3, characterized in that: The specific surface area of ​​the alumina is 200-220 m 2 g -1 , pore volume is 0.5-0.7 cm 3 g -1 , pore size is 10-12 nm.

5. The method according to any one of claims 1 to 4, characterized in that: The Ni-based catalyst is prepared by the following method: preparing a nickel salt into a nickel salt solution; uniformly dropping the nickel salt solution onto an oxide carrier, drying after sufficient impregnation, and then calcining at a high temperature in an air atmosphere, obtaining a calcined product after cooling, and reducing the calcined product to obtain a Ni-based catalyst.

6. The method according to any one of claims 1 to 4, characterized in that: The metal sleeve is a stainless steel sleeve.

7. The method according to any one of claims 1 to 4, characterized in that: The carrier gas in the reaction raw material gas is nitrogen, wherein the gas molar ratio of CH4:CO2 is 1:

1.

8. The method according to any one of claims 1 to 4, characterized in that: The reaction temperature of the methane dry reforming reaction is 680-710° C., and the reaction pressure is normal pressure.

9. The method according to any one of claims 1 to 4, characterized in that: The reaction space velocity is 230000-260000 cm 3 g -1 h -1 .

10. A device for the method of co-producing synthesis gas and carbon nanotubes by dry reforming reaction of methane as claimed in claim 1, characterized in that: The device includes a reaction tube, the upper end and the lower end of the reaction tube are respectively provided with an air inlet and an air outlet, the constant temperature zone inside the reaction tube is filled in sequence from top to bottom in the order of quartz wool-catalyst-quartz wool to form an upper layer of quartz wool, a catalyst layer and a lower layer of quartz wool, the upper layer of quartz wool and the lower layer of quartz wool fix the catalyst layer inside the reaction tube, the reaction tube also contains a metal sleeve, the metal sleeve passes through the three layers of quartz wool-catalyst-quartz wool, and the head of the metal sleeve is higher than the upper layer of quartz wool, and the metal sleeve below the lower layer of quartz wool has a rough surface.

Citation Information

Patent Citations

  • Process for preparing carbon nanotube by carbon dioxide-methane reforming technology

    CN113955742A

  • Application of alumina-loaded Ni catalyst with specific microstructure in preparation of synthesis gas by plasma catalytic methane dry reforming

    CN114249300A

  • Method for producing Nano carbon tubes continuously and equipment

    CN101049927A

  • Method for preparing synthesis gas from carbon dioxide-containing natural gas or methane

    CN101905865A

  • Reaction system for catalyzing CO2 to be converted into carbon nano tube through cascade reaction, preparation method, carbon nano tube and application of carbon nano tube

    CN118217888A