A weather-resistant polyester polyol and its preparation method and application

Weather-resistant polyester polyol is prepared through the copolymerization reaction of polyether-modified MDT silicone resin with dibasic acid and small molecular glycol, which solves the problem of insufficient weather resistance and flexibility of polyester-based polyurethane coatings and achieves high Adhesion, strength and wear resistance, and reduce industrialization costs.

CN118373977BActive Publication Date: 2024-10-22ZHONGSHAN MINGYI CHEM NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410543191.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-04
Publication Date
2024-10-22
Estimated Expiration
2044-05-04

AI Technical Summary

Technical Problem

Existing polyester polyurethane coatings have insufficient weather resistance and flexibility, and have poor compatibility with isocyanates and additives and poor processing performance, resulting in high industrial transformation costs.

Method used

Weather-resistant polyester polyol is prepared by copolymerizing polyether-modified MDT silicone resin with dibasic acid and small-molecule diol. The weather resistance and flexibility are improved by introducing long-chain and branched-chain structures, and is applied in conventional processes. Suitable for the preparation of polyurethane coatings.

Benefits of technology

It significantly improves the weather resistance and flexibility of polyester polyol, improves compatibility with isocyanate and other components, reduces industrialization costs, and achieves high adhesion, strength and wear-resistant polyurethane coating properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004821587010000081
    Figure BDA0004821587010000081
  • Figure BDA0004821587010000091
    Figure BDA0004821587010000091
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and discloses a weather-resistant polyester polyol and a preparation method and application thereof. The preparation method is as follows: adding hydrogen-containing MDT silicone resin and allyl polyether to an organic solvent and mixing them evenly, then adding chloroplatinic acid catalyst, heating to 60-90°C for addition reaction, and obtaining polyether-modified MDT silicone resin; adding polyether-modified MDT silicone resin, dibasic acid and small molecule diol to a reactor, heating and stirring to mix evenly, adding titanate catalyst under nitrogen protection, heating to 180-240°C for insulation reaction, and obtaining weather-resistant polyester polyol. The weather-resistant polyester polyol obtained by the present invention combines the advantages of polysiloxane and polyether polyol, and has the advantages of high strength and adhesion, good weather resistance and flexibility. It can be applied to conventional polyester polyol and polyurethane production process systems, and has low industrialization cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a weather-resistant polyester polyol and a preparation method and application thereof. Background Art

[0002] Polyester polyols are usually products obtained by condensation polymerization of dicarboxylic acids and diols. They are widely used in the preparation of polyester polyurethane coatings and have the advantages of good heat resistance, chemical resistance and high mechanical strength. However, their weather resistance, flexibility, compatibility with components such as isocyanates and additives, and processing performance are slightly inferior to those of polyether polyols.

[0003] Patent CN 109180915 B discloses a liquid polyester polyol for polyurethane coating. Considering the small molecular dibasic acid and diol as the raw materials for synthesizing polyester polyol, the small molecular dibasic acid uses a mixed dibasic acid, and the small molecular diol uses two or more diols, and one of them must contain a branched structure. This ensures that the obtained polyester polyol has a high degree of structural irregularity and asymmetry. The obtained polyester is not easy to crystallize or does not crystallize, and is liquid at room temperature or low temperature, maintaining good fluidity, which is conducive to the preparation of the main agent component in the two-component polyurethane coating and meets the basic requirements of stability, fluidity, etc. However, it cannot solve the problem of insufficient weather resistance and flexibility of polyester polyurethane.

[0004] Silicone materials contain Si-O bonds with high bond energy (422.2 kJ / mol) and rotation barriers close to zero. In addition, the single molecule volume of polysiloxane is large and the cohesive energy density is low. Therefore, it has excellent properties such as resistance to high and low temperatures, resistance to weathering, good flexibility, and good processing fluidity. Therefore, it is an ideal material for polyurethane modified products.

[0005] Li Min et al. (Preparation of Silicone-Modified Waterborne Polyurethane Coatings and Their Antifouling Properties [J], Journal of Functional Polymers, 2021, 34(4): 397-385) disclosed the synthesis of a series of silicone-modified waterborne polyurethane (PU) coatings using toluene diisocyanate (TDI), poly(1,4-butylene adipate) (PCL2000) and hydroxy silicone oil (PDMS) as the main raw materials. The results show that the introduction of PDMS reduces the elastic modulus and glass transition temperature of the PU coating and enhances the hydrophobicity of the coating. However, the direct reaction of PDMS with isocyanate has poor compatibility. In addition, the synthesis steps are complicated, and the process conditions for the synthesis of conventional polyester polyols and polyurethanes are greatly changed, and the cost of industrial transformation is too high. Summary of the invention

[0006] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a method for preparing weather-resistant polyester polyol.

[0007] Another object of the present invention is to provide a weather-resistant polyester polyol prepared by the above method.

[0008] Another object of the present invention is to provide application of the weather-resistant polyester polyol in the preparation of polyurethane coatings.

[0009] The weather-resistant polyester polyol obtained by the present invention combines the advantages of polysiloxane and polyether polyol, and has the advantages of good weather resistance and flexibility. It can directly adopt conventional processes to react with polyacids to prepare polyester polyols, is suitable for the preparation of conventional polyurethane systems, and has low industrialization costs.

[0010] The purpose of the present invention is achieved through the following technical solutions:

[0011] A method for preparing a weather-resistant polyester polyol comprises the following preparation steps:

[0012] (1) Preparation of polyether modified MDT silicone resin:

[0013] The hydrogenated MDT silicone resin and allyl polyether (APEG) are added to an organic solvent and mixed evenly, and then a chloroplatinic acid catalyst is added, and the temperature is raised to 60-90° C. to carry out an addition reaction to obtain a polyether-modified MDT silicone resin;

[0014] (2) Preparation of weather-resistant polyester polyols:

[0015] Add polyether modified MDT silicone resin, dibasic acid and small molecule diol into a reaction kettle, heat and stir to mix, add titanate catalyst under nitrogen protection, heat to 180-240° C. for insulation reaction, and obtain weather-resistant polyester polyol.

[0016] Furthermore, the hydrogen-containing MDT silicone resin in step (1) has a weight average molecular weight (Mw) of 3000 to 8000 g / mol and an active hydrogen content of 0.1% to 0.8% (wt%). It can be prepared by the following method:

[0017] Add dialkoxysilane (D), trialkoxysilane (T) and acid catalyst solution into the reaction kettle, heat to 30-60°C for hydrolysis reaction; then add end-capping agent tetramethyl disiloxane (MM H ), and the temperature is raised to 60-80° C. to carry out copolymerization equilibrium reaction to obtain hydrogenated MDT silicone resin.

[0018] Preferably, the mass ratio of the dialkoxysilane, trialkoxysilane and the end-capping agent tetramethyldisiloxane is 100:10 to 30:10 to 40. The dialkoxysilane can be selected from methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane; the trialkoxysilane can be selected from methyltrimethoxysilane or methyltriethoxysilane.

[0019] Preferably, the acid catalyst solution is hydrochloric acid or sulfuric acid solution, and the hydrolysis reaction time is 1 to 4 hours.

[0020] Preferably, the copolymerization equilibrium reaction time is 2 to 6 hours; after the copolymerization equilibrium reaction is completed, the reaction is allowed to stand for stratification, and the oil phase is vacuum dried at 100 to 140° C. to remove water and low-boiling impurities to obtain a hydrogenated MDT silicone resin.

[0021] Furthermore, the allyl polyether in step (1) is allyl polyethylene glycol with a molecular weight of 500 to 2000 and a hydroxyl value of 25 to 120 mgKOH / g.

[0022] Furthermore, the molar ratio of the amount of the allyl polyether added in step (1) to the active hydrogen content in the hydrogen-containing MDT silicone resin is 0.05 to 0.4:1.

[0023] Furthermore, the organic solvent in step (1) is toluene.

[0024] Furthermore, the addition reaction time in step (1) is 2 to 6 hours, and after the reaction is completed, the organic solvent is removed in vacuo to obtain a polyether-modified MDT silicone resin.

[0025] Furthermore, the dibasic acid in step (2) is an aliphatic dicarboxylic acid or an aromatic dicarboxylic acid. Aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, etc.; aromatic dicarboxylic acids include phthalic acid, isophthalic acid, terephthalic acid, etc.; the small molecule diol is an aliphatic diol having 2 to 6 carbon atoms, such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol or 1,6-hexanediol.

[0026] Furthermore, in step (2), the molar ratio of the dibasic acid to the small molecule diol is 1:1-1.2; and the added amount of the polyether-modified MDT silicone resin is 10%-80% of the total mass of the dibasic acid and the small molecule diol.

[0027] Furthermore, the heat preservation reaction in step (2) refers to firstly heat preservation reaction under closed conditions until the acid value is less than 5 mgKOH / g, and then dehydration reaction by reduced pressure distillation until the acid value is less than 1 mgKOH / g and the hydroxyl value is 40 to 120 mgKOH / g, to obtain weather-resistant polyester polyol.

[0028] A weather-resistant polyester polyol is prepared by the method.

[0029] Application of the above weather-resistant polyester polyol in the preparation of polyurethane coatings.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) The present invention uses polyether-modified MDT silicone resin as a macromolecular polyol to copolymerize with dibasic acid and small molecule diol to prepare polyester polyol, wherein MDT silicone resin introduces long-chain and branched polysiloxane, which significantly improves weather resistance and flexibility. On the one hand, the polyether modification enhances the compatibility and reactivity of MDT silicone resin with dibasic acid and small molecule diol, significantly improving the improvement effect; on the other hand, the introduction of MDT silicone resin-terminated polyether chains makes the obtained polyester polyol contain a large number of polyether chains and polyether terminal hydroxyl groups, which can improve the compatibility with components such as isocyanate and additives in the preparation of polyurethane coatings, and can simultaneously generate a polyether polyurethane structure. The prepared polyurethane coating can simultaneously integrate the high adhesion, high strength, and high wear resistance of polyester polyurethane and the weather resistance and flexibility of polyether polyurethane.

[0032] (2) The polyether-modified MDT silicone resin of the present invention can greatly reduce the crystallinity of the product through the branching effect of the T chain segments, thereby increasing the molecular weight of the polymer and improving its compatibility; at the same time, its branching effect enables the obtained polyether-modified MDT silicone resin to contain a large amount of terminal polyethers, which can improve the reaction activity with dibasic acids while retaining a large amount of unreacted polyether terminal hydroxyl groups for further grafting reaction with raw materials such as isocyanates to obtain a branched polyether-type polyurethane structure, thereby improving the overall performance.

[0033] (3) The polyether-modified MDT silicone resin used in the present invention can be reacted with a polyacid through conventional processes to prepare polyester polyols, and is suitable for the preparation of conventional polyurethane systems without the need to modify the existing industrial process routes. It has the advantages of easy application and low industrialization cost. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0035] Example 1

[0036] A method for preparing a weather-resistant polyester polyol comprises the following preparation steps:

[0037] (1) Preparation of hydrogenated MDT silicone resin:

[0038] 10 kg of dimethyldiethoxysilane, 2 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor, and the temperature was raised to 45 °C for hydrolysis reaction for 2 h; then 3 kg of end-capping agent tetramethyldisiloxane (MM H), the temperature was raised to 75°C for copolymerization equilibrium reaction for 4 hours, and after the reaction was completed, the phase was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.28wt.% by sampling titration method, and the weight average molecular weight was 5520g / mol by GPC.

[0039] (2) Preparation of polyether modified MDT silicone resin:

[0040] Take 5kg of hydrogenated MDT silicone resin and 2.5kg of allyl polyether APEG-800 (hydroxyl value 71mgKOH / g), add them to 5kg of toluene solvent, stir to dissolve and mix, then add 40ml of 3wt% chloroplatinic acid isopropanol solution catalyst, heat to 85°C for addition reaction for 3h, take samples to detect the olefin content, and the reaction is complete. Remove the organic solvent in vacuo to obtain polyether modified MDT silicone resin.

[0041] (3) Preparation of weather-resistant polyester polyols:

[0042] 2kg of polyether-modified MDT silicone resin, 1.18kg of succinic acid, 2.02kg of sebacic acid and 1.98kg of 1,4-butanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% of n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 87.4mgKOH / g when sampling was performed to obtain a weather-resistant polyester polyol.

[0043] Example 2

[0044] A method for preparing a weather-resistant polyester polyol comprises the following preparation steps:

[0045] (1) Preparation of hydrogenated MDT silicone resin:

[0046] 10 kg of methyldiethoxysilane, 3 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor, and the temperature was raised to 55 °C for hydrolysis reaction for 2 h; then 4 kg of end-capping agent tetramethyldisiloxane (MM H ), the temperature was raised to 80°C for copolymerization equilibrium reaction for 4 hours, and after the reaction was completed, the mixture was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.63wt.% by sampling titration method, and the weight average molecular weight was 3850g / mol by GPC.

[0047] (2) Preparation of polyether modified MDT silicone resin:

[0048] Take 5kg of hydrogenated MDT silicone resin and 1.5kg of allyl polyether APEG-500 (hydroxyl value 105mgKOH / g), add them to 5kg of toluene solvent, stir to dissolve and mix, then add 40ml of 3wt% chloroplatinic acid isopropanol solution catalyst, heat to 80°C for addition reaction for 4h, take samples to detect the olefin content, and the reaction is complete. Remove the organic solvent in vacuo to obtain polyether modified MDT silicone resin.

[0049] (3) Preparation of weather-resistant polyester polyols:

[0050] 1kg of polyether-modified MDT silicone resin, 1.18kg of succinic acid, 1.88kg of azelaic acid and 2.45kg of 1,6-hexanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% of n-butyl titanate catalyst was added under nitrogen protection. The temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g. The vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 105.6mgKOH / g when sampling was performed to obtain a weather-resistant polyester polyol.

[0051] Example 3

[0052] A method for preparing a weather-resistant polyester polyol comprises the following preparation steps:

[0053] (1) Preparation of hydrogenated MDT silicone resin:

[0054] 10 kg of dimethyldiethoxysilane, 1 kg of methyltriethoxysilane and 0.5 kg of 1 M sulfuric acid aqueous solution were added to the reactor, and the temperature was raised to 45 °C for hydrolysis reaction for 2 h; then 1 kg of end-capping agent tetramethyldisiloxane (MM H ), the temperature was raised to 75°C for copolymerization equilibrium reaction for 3 hours, and after the reaction was completed, the phase was allowed to stand for stratification, and the oil phase was vacuum dried at 120°C to remove water and low-boiling impurities to obtain hydrogen-containing MDT silicone resin. The active hydrogen content of the hydrogen-containing MDT silicone resin was determined to be 0.12wt.% by sampling titration method, and the weight average molecular weight was 7680g / mol by GPC.

[0055] (2) Preparation of polyether modified MDT silicone resin:

[0056] Take 5kg of hydrogenated MDT silicone resin and 2kg of allyl polyether APEG-1000 (hydroxyl value 52mgKOH / g), add them to 5kg of toluene solvent, stir to dissolve and mix, then add 40ml of 3wt% chloroplatinic acid isopropanol solution catalyst, heat to 85°C for addition reaction for 5h, take samples to detect the olefin content, the reaction is complete, remove the organic solvent in vacuo, and obtain polyether modified MDT silicone resin.

[0057] (3) Preparation of weather-resistant polyester polyols:

[0058] 4kg of polyether-modified MDT silicone resin, 2.92kg of adipic acid, 0.83kg of phthalic acid, 1.52kg of 1,3-propylene glycol, and 0.45kg of 1,4-butanediol were added to a high-pressure reactor, heated, stirred, dissolved, and mixed. A 0.1wt% concentration of n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220°C and sealed for 4 hours. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240°C until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1 hour. The hydroxyl value of the product was 66.5mgKOH / g, and a weather-resistant polyester polyol was obtained.

[0059] Comparative Example 1

[0060] A method for preparing polyester polyol, compared with Example 1, does not add polyether-modified MDT silicone resin, and includes the following preparation steps:

[0061] 1.18kg succinic acid, 2.02kg sebacic acid and 1.98kg 1,4-butanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 110.6mgKOH / g when the sample was tested to obtain polyester polyol.

[0062] Comparative Example 2

[0063] A method for preparing polyester polyol, compared with Example 2, does not add polyether-modified MDT silicone resin, and includes the following preparation steps:

[0064] 1.18kg succinic acid, 1.88kg azelaic acid and 2.45kg 1,6-hexanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220℃ and sealed for 4h, during the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 122.5mgKOH / g when the sample was tested to obtain polyester polyol.

[0065] Comparative Example 3

[0066] A method for preparing a polyester polyol, compared with Example 3, does not add polyether-modified MDT silicone resin, and includes the following preparation steps:

[0067] 2.92kg adipic acid, 0.83kg phthalic acid, 1.52kg 1,3-propylene glycol and 0.45kg 1,4-butanediol were added to a high-pressure reactor, heated, stirred and dissolved, and 0.1wt% n-butyl titanate catalyst was added under nitrogen protection, and the temperature was raised to 220℃ and sealed for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 120.3mgKOH / g, and polyester polyol was obtained.

[0068] Comparative Example 4

[0069] A method for preparing a polyester polyol, compared with Example 1, uses the linear hydroxy silicone oil PDMS disclosed in the literature (Preparation of silicone-modified waterborne polyurethane coating and its antifouling performance [J], Journal of Functional Polymers, 2021, 34(4): 397-385) to replace the polyether-modified MDT silicone resin, comprising the following preparation steps:

[0070] 2kg of hydroxy silicone oil PDMS, 1.18kg of succinic acid, 2.02kg of sebacic acid and 1.98kg of 1,4-butanediol were added to a high-pressure reactor, heated and stirred to dissolve and mix, 0.1wt% of n-butyl titanate catalyst was added under nitrogen protection, the temperature was raised to 220℃ and sealed for reaction for 4h. During the reaction, the acid value in the mixture was tested every half an hour until the acid value in the mixture was less than 5mgKOH / g. Then, the mixture was dehydrated by vacuum distillation at 220-240℃ until the acid value was less than 1mgKOH / g, and the vacuum insulation reaction was continued for 1h. The hydroxyl value of the product was 90.2mgKOH / g when the sample was tested to obtain polyester polyol.

[0071] The polyester polyols obtained in the above Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to performance tests. The test method is as follows: the obtained weather-resistant polyester polyol is dissolved in toluene solvent to prepare a polyester polyol solution with a solid content of 42%, and then the solution is mixed evenly with an HDI trimer curing agent at a molar ratio of hydroxyl to isocyanate of 1:1 to obtain a coating. After the coated object is sizing, coating and curing, the corresponding coating properties are tested or a standard sample of the cured product is prepared to test the corresponding properties. Among them, the adhesion test refers to the standard GB / T5210-2006, and the adhesion substrate uses a hard steel plate; the tensile strength and elongation at break test refer to the standard GB / T 528-2009; the low-temperature flexibility test refers to the standard GB / T 6742-2007, and the test is conditioned for 24 hours at a low temperature of (-30±2)℃ and a relative humidity of (50±5)% before the test; the weather resistance test refers to the standard GB / T 14522-2, and the light source is a UVA-340 fluorescent ultraviolet lamp with an irradiance of 0.89W / m 2 , the tensile strength retention rate and elongation at break retention rate after 600h artificial weathering were tested. The test results are shown in Table 1 below.

[0072] Table 1

[0073]

[0074]

[0075] From the comparison results of Examples 1 to 3 and Comparative Examples 1 to 3 in Table 1, it can be seen that the present invention can improve the strength of the polyurethane material obtained after curing to a certain extent by adding polyether-modified MDT silicone resin to modify the polyester polyol, and can significantly improve its weather resistance and flexibility, and has no obvious adverse effect on the adhesion of the coating film. From the comparison results of Example 1 and Comparative Example 4, it can be seen that after the linear hydroxy silicone oil PDMS is used to replace the polyether-modified MDT silicone resin, the corresponding strength improvement effect and the weather resistance and flexibility improvement effect are significantly reduced, and the coating film adhesion is significantly adversely affected. The reason is that the compatibility and reactivity of the linear hydroxy silicone oil PDMS are relatively low, and it is impossible to generate a branched polyether polyurethane structure, resulting in a reduction in the improvement effect. At the same time, the adhesion is reduced due to the low surface energy characteristics of PDMS and the reduced grafting modification effect.

[0076] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing a weather-resistant polyester polyol, characterized in that: The method comprises the following preparation steps: (1) Preparation of polyether modified MDT silicone resin: The hydrogen-containing MDT silicone resin and the allyl polyether are added to an organic solvent and mixed evenly, and then a chloroplatinic acid catalyst is added, and the temperature is raised to 60-90° C. to carry out an addition reaction to obtain a polyether-modified MDT silicone resin; (2) Preparation of weather-resistant polyester polyols: Add polyether modified MDT silicone resin, dibasic acid and small molecule diol into a reaction kettle, heat and stir to mix, add titanate catalyst under nitrogen protection, heat to 180-240°C for insulation reaction, and obtain weather-resistant polyester polyol; The hydrogen-containing MDT silicone resin in step (1) has a weight average molecular weight of 3000-8000 g / mol and an active hydrogen content of 0.1%-0.8%, and is prepared by the following method: Adding dialkoxysilane, trialkoxysilane and acid catalyst solution into a reaction kettle, heating to 30-60°C for hydrolysis reaction; then adding end-capping agent tetramethyldisiloxane, heating to 60-80°C for copolymerization equilibrium reaction, and obtaining hydrogen-containing MDT silicone resin; The mass ratio of the dialkoxysilane, trialkoxysilane and the end-capping agent tetramethyldisiloxane added is 100:10~30:10~40; the dialkoxysilane is selected from methyldimethoxysilane, methyldiethoxysilane, dimethyldimethoxysilane or dimethyldiethoxysilane; the trialkoxysilane is selected from methyltrimethoxysilane or methyltriethoxysilane; The allyl polyether is allyl polyethylene glycol with a molecular weight of 500-2000 and a hydroxyl value of 25-120 mgKOH / g; the molar ratio of the added amount of the allyl polyether to the active hydrogen content in the hydrogen-containing MDT silicone resin is 0.05-0.4:

1.

2. The method for preparing a weather-resistant polyester polyol according to claim 1, characterized in that: The acid catalyst solution is hydrochloric acid or sulfuric acid solution, the hydrolysis reaction time is 1-4 hours, the copolymerization equilibrium reaction time is 2-6 hours, after the copolymerization equilibrium reaction is completed, the reaction is allowed to stand and the layers are separated, and the oil phase is vacuum dried at 100-140° C. to remove water and low-boiling impurities, thereby obtaining a hydrogenated MDT silicone resin.

3. The method for preparing a weather-resistant polyester polyol according to claim 1, characterized in that: The organic solvent in step (1) is toluene; the addition reaction time is 2 to 6 hours, and after the reaction is completed, the organic solvent is removed in vacuo to obtain a polyether-modified MDT silicone resin.

4. The method for preparing a weather-resistant polyester polyol according to claim 1, characterized in that: The dibasic acid in step (2) is an aliphatic dicarboxylic acid or an aromatic dicarboxylic acid; the aliphatic dicarboxylic acid is at least one of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid; the aromatic dicarboxylic acid is at least one of phthalic acid, isophthalic acid, and terephthalic acid; the small molecule diol is an aliphatic diol having 2 to 6 carbon atoms; the molar ratio of the dibasic acid to the small molecule diol is 1:1 to 1.2; the amount of the polyether-modified MDT silicone resin added is 10% to 80% of the total mass of the dibasic acid and the small molecule diol.

5. The method for preparing a weather-resistant polyester polyol according to claim 1, characterized in that: The heat preservation reaction in step (2) refers to firstly heat preservation reaction under closed conditions until the acid value is less than 5 mgKOH / g, and then dehydration reaction by reduced pressure distillation until the acid value is less than 1 mgKOH / g and the hydroxyl value is 40-120 mgKOH / g, thereby obtaining weather-resistant polyester polyol.

6. A weather-resistant polyester polyol, characterized in that: It is prepared by the method according to any one of claims 1 to 5.

7. Use of the weather-resistant polyester polyol according to claim 6 in the preparation of polyurethane coatings.