Flame-retardant heat-expandable microspheres, waterproof coiled material and preparation method thereof
By applying flame-retardant thermal expansion microspheres with surface carbon modification and phosphorus-containing polymer shells in waterproof rolls, the problem of difficult to take into account both the weight and flame retardancy of traditional PVC waterproof rolls is achieved, and lightweight and high flame retardant is achieved and waterproof coils with good mechanical properties.
Patent Information
- Application Number
- CN202410805635.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Due to its large weight, traditional PVC waterproof coils have inconvenience to construction and transportation. At the same time, their mechanical properties and flame retardant properties are difficult to maintain after reducing weight.
The flame retardant thermal expansion microspheres are used to improve the flame retardancy of microspheres through surface carbon modification, phosphorus-containing polymer shell and internal coating of halogen-free phosphorus-containing flame retardant, and through inorganic carbon materials and The combination of organic carbonaceous agents improves the compatibility of microspheres and resins and reduces the density of waterproof coils.
It significantly improves the flame retardancy and mechanical properties of the waterproof coil, realizes the special performance of lightweight, soft, high elastic and impact resistance, and reduces transportation costs and construction difficulties.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building waterproof materials, and specifically relates to a flame-retardant thermal expansion microsphere, a waterproof coiled material and a preparation method thereof. Background Art
[0002] Polyvinyl chloride (PVC) waterproofing membrane is a high-molecular waterproof material with excellent performance. It is mainly made of polyvinyl chloride resin and filler as raw materials, and is produced with various additives. It has the characteristics of high tensile strength, high elongation, small dimensional change rate, good low-temperature flexibility, strong resistance to root penetration, long service life, etc., and the welding is firm and reliable, environmentally friendly and pollution-free. However, due to its large dead weight, traditional PVC waterproofing membrane brings many inconveniences to construction and transportation.
[0003] In the prior art, there are also some means to lighten the weight of PVC waterproof membranes. For example, when preparing waterproof membranes, a certain amount of foaming agent is added. Although this can reduce the weight of the waterproof membranes, it also damages the mechanical properties of the waterproof membranes, and the flame retardant properties of the membranes are not improved. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a flame retardant heat-expandable microsphere suitable for waterproof roll materials. The flame retardant heat-expandable microspheres are applied to the waterproof roll materials, which not only reduces the weight of the waterproof roll materials, but also maintains the mechanical properties and improves the flame retardancy of the waterproof roll materials.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A flame-retardant heat-expandable microsphere, comprising a core material and a shell coated on the outer periphery of the core material, wherein the core material comprises a hydrocarbon and a liquid phosphorus-containing flame retardant, and the shell is a surface-modified acrylic polymer, wherein the acrylic polymer is obtained by polymerizing a polymerizing monomer, and the shell is obtained by surface-modifying the acrylic polymer using a modifying material;
[0007] The polymerizable monomers include a first polymerizable monomer and a second polymerizable monomer, wherein the first polymerizable monomer is an acrylic acid phosphate monomer, and the second polymerizable monomer is at least one of a nitrile monomer, a carboxyl acrylic acid monomer, and a methacrylic acid ester monomer;
[0008] The modified materials are organic carbon-forming agent, inorganic carbon material and coupling agent.
[0009] In the present invention, the surface of the microspheres is modified by coupling the inorganic carbon material to the surface of the acrylic polymer through a coupling agent, which can increase the carbonization effect and effectively improve the flame retardancy of the microspheres. At the same time, the surface of the microspheres is modified by using an organic carbon-forming agent, which can effectively improve the compatibility of the microspheres with the resin and improve the dispersibility of the microspheres in the resin when the microspheres are applied to the waterproof membrane. While reducing the dead weight of the waterproof membrane, it helps the waterproof membrane to maintain good mechanical properties and give the waterproof membrane a certain flame retardancy.
[0010] According to some implementation aspects of the present invention, the feed mass ratio of the organic carbon-forming agent to the inorganic carbon material is 1:0.5~1.5.
[0011] In some specific embodiments, the organic carbon-forming agent is one or a combination of an organic phosphorus carbon-forming agent, a thermoplastic phenolic resin carbon-forming agent, a polyamide carbon-forming agent, a triazine derivative carbon-forming agent and a hyperbranched macromolecular flame-retardant carbon-forming agent.
[0012] In some specific embodiments, the inorganic carbon material is a nanocarbon material, and the nanocarbon material is one or a combination of carbon nanotubes, graphene, and nanocarbon balls.
[0013] In some specific embodiments, the coupling agent is a silane coupling agent, such as one or a combination of γ-aminopropyltriethoxysilane and γ-methacryloxypropyltrimethoxysilane.
[0014] According to some implementation aspects of the present invention, the feed mass ratio of the first polymerizable monomer to the second polymerizable monomer is 30-50:50-100.
[0015] In some specific embodiments, the acrylic acid phosphate monomer is one or a combination of acrylic acid monophosphate, acrylic acid diphosphate, methacrylic acid monophosphate, methacrylic acid diphosphate, pentabromobenzyl acrylate, methacryloyloxyethyl phosphate, and 2-hydroxyethyl methacrylate phosphate.
[0016] In some specific embodiments, the nitrile monomer is one or a combination of acrylonitrile, methacrylonitrile, chloroacrylonitrile, and ethoxyacrylonitrile.
[0017] In some specific embodiments, the carboxyl acrylic monomer is one or a combination of acrylic acid, methacrylic acid, ethacrylic acid, maleic acid, monoethyl maleate, and monobutyl maleate.
[0018] In some specific embodiments, the methacrylate monomer is one or a combination of methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate, and benzyl methacrylate.
[0019] In some specific embodiments, the mass ratio of the nitrile monomer, the carboxyl acrylic acid monomer, and the methacrylate monomer is 50-100:5-15:20-50.
[0020] According to some implementation aspects of the present invention, the hydrocarbon is a hydrocarbon with a boiling point above 60° C. Further, the hydrocarbon is one or a combination of n-hexane, n-heptane, isooctane, and n-octane.
[0021] In some specific embodiments, the liquid phosphorus-containing flame retardant is one or a combination of tributyl phosphate, dimethyl methyl phosphate, diethyl ethyl phosphate, tricresyl phosphate, tolyl diphenyl phosphate, tri(xylene) phosphate, tri(butoxyethyl) phosphate, bisphenol A-bis(diphenyl phosphate) and resorcinol bis(diphenyl phosphate).
[0022] In some specific embodiments, the mass ratio of the first polymerizable monomer, the hydrocarbon compound and the liquid phosphorus-containing flame retardant is 30-50:30-50:5-30.
[0023] In some specific embodiments, the particle size of the flame retardant heat-expandable microspheres is 30-80 μm.
[0024] According to some implementation aspects of the present invention, the flame-retardant heat-expandable microspheres are prepared by suspension polymerization.
[0025] According to some implementation aspects of the present invention, the flame-retardant heat-expandable microspheres further include a water-dispersible halogen-free flame retardant dispersed in the core material and / or the shell.
[0026] In some specific embodiments, the water-dispersible halogen-free flame retardant is one or a combination of magnesium hydroxide, hydrated magnesium hydroxide, aluminum hydroxide, hydrated aluminum hydroxide, zinc oxide, and magnesium oxide. The addition of a certain amount of water-dispersible halogen-free flame retardant has a certain smoke suppression property.
[0027] In some specific embodiments, the feed mass ratio of the water-dispersible halogen-free flame retardant to the liquid phosphorus-containing flame retardant is 5-20:5-30.
[0028] In some specific embodiments, the raw material formula of the flame retardant heat-expandable microspheres includes, by weight:
[0029] 30~50 parts of hydrocarbons;
[0030] 30-50 parts of the first polymerizable monomer;
[0031] 50-100 parts of the second polymerization monomer;
[0032] 5-20 parts of water-dispersible halogen-free flame retardant;
[0033] 5~30 parts of liquid phosphorus-containing flame retardant.
[0034] The second technical solution adopted by the present invention is a method for preparing the flame-retardant heat-expandable microspheres described above, comprising the following steps:
[0035] (1) uniformly mixing water, a water-dispersible halogen-free flame retardant, an electrolyte and an emulsifier to obtain an aqueous dispersion;
[0036] (2) uniformly mixing the first polymerizable monomer, the second polymerizable monomer, the initiator, the hydrocarbon compound and the liquid phosphorus-containing flame retardant to obtain an oil phase dispersion;
[0037] (3) adding the oil phase dispersion to the aqueous phase dispersion under stirring to obtain a pre-suspension, and then polymerizing under inert gas conditions to obtain microspheres with unmodified surfaces;
[0038] (4) Dispersing the unmodified microspheres in a dispersion of a modified material to obtain the flame-retardant heat-expandable microspheres.
[0039] In some specific embodiments, in step (1), the amount of water is 300-500 parts, the amount of electrolyte is 50-100 parts, and the amount of emulsifier is 0.3-3 parts; in step (2), the amount of initiator is 1-5 parts.
[0040] Furthermore, the electrolyte is sodium chloride or the like; the emulsifier is one or a combination of sodium dodecyl sulfate, polyvinyl alcohol or the like.
[0041] In some specific embodiments, in step (3), the polymerization reaction is carried out at a pressure of 1.5-1.8 MPa and a temperature of 65-80° C., and the polymerization reaction time is 12-24 h.
[0042] In some specific embodiments, in step (4), the dispersion of the modified material comprises the modified material and a dispersion medium, and the dispersion medium is an alcohol solvent, such as methanol, ethanol, or a combination of several thereof.
[0043] In some specific embodiments, in step (4), the surface-unmodified microspheres are added to the dispersion, mixed at high speed, and then kept at 60±10° C. for 24 to 30 h, washed, and filtered to obtain the flame-retardant heat-expandable microspheres.
[0044] In some specific embodiments, in step (4), the mass ratio of the surface-unmodified microspheres to the organic carbon-forming agent is 10-50:1-5. The mass ratio of the surface-unmodified microspheres to the coupling agent is 100:0.1~5.
[0045] The third technical solution adopted by the present invention is: a waterproof roll material, comprising a first resin layer and a second resin layer stacked in sequence, wherein heat-expandable microspheres are added to the first resin layer or the second resin layer, and the heat-expandable microspheres are the flame-retardant heat-expandable microspheres described above or the flame-retardant heat-expandable microspheres prepared by the preparation method of the flame-retardant heat-expandable microspheres described above.
[0046] According to some implementation aspects of the present invention, the feed mass of the heat-expandable microspheres is 0.5-1% of the total mass of the raw materials of the first resin layer or the second resin layer.
[0047] According to some implementation aspects of the present invention, the first resin layer and the second resin layer are PVC resin layers respectively.
[0048] According to some implementation aspects of the present invention, the raw materials of the first resin layer include PVC resin, plasticizer and filler;
[0049] The raw materials of the second resin layer include PVC resin, heat-expandable microspheres, plasticizer and filler;
[0050] In the first resin layer and the second resin layer, the mass ratio of the PVC resin, the plasticizer and the filler is 1:0.2~1:0.1~0.4.
[0051] In some specific embodiments, the raw material formulas of the first resin layer and the second resin layer independently include, by weight:
[0052] PVC resin 80-100 parts;
[0053] Plasticizer 20-80 parts;
[0054] 15-30 parts of filler;
[0055] The second resin layer also includes heat-expandable microspheres in an amount of 0.5 to 1% of the total raw material amount of the second resin layer.
[0056] In some specific embodiments, the thickness ratio of the first resin layer to the second resin layer is 5:1-15.
[0057] In some specific embodiments, the plasticizer is one or a combination of DOP, DINP, DOTP, and epoxidized soybean oil.
[0058] In some specific embodiments, the filler is a combination of one or more of titanium dioxide, calcium carbonate, talc, and clay.
[0059] In some specific embodiments, the raw material formula of the first resin layer and the second resin layer further includes 2 to 6 parts of auxiliary agents, and the auxiliary agents are one or a combination of heat stabilizers and anti-ultraviolet agents.
[0060] Furthermore, the auxiliary agent is 2 to 5 parts of a heat stabilizer and 0.01 to 0.2 parts of an anti-ultraviolet agent.
[0061] The anti-ultraviolet agent is a combination of one or more of an ultraviolet absorber, a light shielding agent, and a hindered amine light stabilizer.
[0062] The fourth technical solution adopted by the present invention: a method for preparing the waterproof coiled material described above, comprising melting the raw material of the first resin layer and the raw material of the second resin layer separately, and co-extruding to obtain the waterproof coiled material.
[0063] In some specific embodiments, the extrusion temperature is 160-180° C. and the screw speed is 140-160 rpm.
[0064] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0065] The flame-retardant heat-expandable microspheres of the present invention have multiple flame-retardant effects through multiple flame-retardant means such as surface carbon modification, a phosphorus-containing polymer shell and an internal coating of a phosphorus-containing flame retardant, and can significantly improve the flame retardancy of the microspheres. Applying the microspheres to waterproof rolls can not only reduce the weight of the waterproof rolls, but also maintain the mechanical properties and improve the flame retardancy of the waterproof rolls.
[0066] Compared with traditional PVC waterproof membrane, the waterproof membrane of the present invention has special properties such as light weight, softness, high elasticity, impact resistance, flame retardancy, etc., and maintains good mechanical properties, and has significant advantages such as low transportation cost and convenient construction. DETAILED DESCRIPTION
[0067] As described in the background art, the existing PCV waterproofing membrane is difficult to solve the contradiction between its own weight and mechanical properties, and the flame retardancy of the membrane has not been improved.
[0068] Heat-expandable microspheres are a type of thermoplastic hollow polymer microspheres. Traditional heat-expandable microspheres are generally composed of a thermoplastic polymer shell and an internal alkane gas. When the microspheres are heated, the gas pressure in the shell increases and the shell softens, causing the volume of the microspheres to increase. After cooling, the shell of the microspheres hardens, and the expansion volume is fixed, causing a significant change in the diameter and volume of the microspheres. After full expansion, the volume of the microspheres can increase by dozens of times. However, general heat-expandable microspheres are flammable due to the presence of internal alkane gas and an organic polymer shell.
[0069] The main concept of the present invention is to redesign a flame-retardant heat-expandable microsphere, and by adopting multiple flame-retardant means such as surface carbon modification, phosphorus-containing polymer shell and internal coating of halogen-free phosphorus-containing flame retardant, the flame-retardant heat-expandable microsphere achieves multiple flame-retardant effects and significantly improves the flame retardancy of the microsphere. In addition, inorganic carbon materials and organic carbon-forming agents are used in combination for surface modification to further improve the flame retardancy, and at the same time, the introduction of organic carbon-forming agents can improve the compatibility of the resin of the waterproof coiled material with the microspheres and improve the dispersibility of the microspheres in the resin.
[0070] A further concept of the present invention is to set the waterproof roll material into a multi-layer structure, and introduce flame-retardant heat-expandable microspheres into one of the layers. On the first hand, the high foaming ratio of the heat-expandable microspheres is utilized to effectively reduce the density of the roll material, thereby achieving the effect of reducing weight and reducing costs. On the second hand, the flame-retardant heat-expandable microspheres are added to one of the layers, and the foaming structure thereof has little effect on the mechanical properties of the roll material, and will not cause a significant decrease in the overall mechanical properties of the waterproof roll material. On the third hand, the flame-retardant heat-expandable microspheres have multiple flame-retardant effects, which improve the decrease in the flame-retardant properties of the roll material due to the generation of internal pores, and can even improve the flame retardancy of the waterproof roll material to a certain extent.
[0071] The technical solution of the present invention is described in detail below in conjunction with specific embodiments so that those skilled in the art can better understand and implement the technical solution of the present invention, but the present invention is not limited to the scope of the examples. Example 1
[0072] The flame-retardant heat-expandable microspheres provided in this embodiment include a core material and a shell coated on the outer periphery of the core material, the core material contains hydrocarbons and liquid phosphorus-containing flame retardants, the shell is a surface-modified acrylic polymer, the acrylic polymer is obtained by polymerizing a polymerizing monomer, and the shell is obtained by modifying the acrylic polymer with a modifying material; wherein the polymerizing monomer includes a first polymerizing monomer and a second polymerizing monomer, the first polymerizing monomer is an acrylic phosphate monomer, and the second polymerizing monomer is a combination of a nitrile monomer, a carboxyl acrylic monomer, and a methacrylate monomer; the modifying material is an organic carbon-forming agent, an inorganic carbon material, and a coupling agent.
[0073] The flame retardant heat-expandable microspheres of this example are prepared by the following method:
[0074] (1) 400 g of water, 10 g of a water-dispersible halogen-free flame retardant, 70 g of an electrolyte and 1.5 g of an emulsifier are mixed uniformly to obtain an aqueous dispersion, wherein the water-dispersible halogen-free flame retardant is magnesium hydroxide, the electrolyte is sodium chloride, and the emulsifier is sodium dodecyl sulfate;
[0075] (2) 40 g of a first polymerizable monomer, 70 g of a second polymerizable monomer, 3 g of an initiator, 40 g of a hydrocarbon, and 20 g of a liquid phosphorus-containing flame retardant are mixed uniformly in a sealed ice-water bath to obtain an oil phase dispersion, wherein the first polymerizable monomer is methyl methacrylate monophosphate, the second polymerizable monomer is a combination of acrylonitrile, acrylic acid, and methyl methacrylate in a mass ratio of 60:10:30, the initiator is benzoyl peroxide, the hydrocarbon is n-hexane, and the liquid phosphorus-containing flame retardant is dimethyl methyl phosphate;
[0076] (3) Under high-speed stirring, the oil phase dispersion was added to the aqueous phase dispersion and mixed evenly to obtain a pre-suspension. After nitrogen was passed through to deoxygenate, a high-pressure (pressure of 1.6 mPa, temperature of 70°C) polymerization reaction was carried out for 20 h. After the reaction was completed, the suspension was filtered and dried at 50°C to obtain microspheres with a particle size of 25 μm.
[0077] (4) 10 g of an organic carbon former, 10 g of a nanocarbon material and 2 g of a silane coupling agent were added to 600 g of a dispersion medium to obtain a dispersion, and the mixture was mixed evenly. Then, 100 g of microspheres were added to the dispersion and mixed evenly. The dispersion was kept at 60 °C for 28 h under high-speed stirring, and the mixture was allowed to stand, washed and filtered to obtain flame-retardant thermally expandable microspheres with a particle size of about 35 μm. The organic carbon former was an organophosphorus carbon former (tricresyl phosphate); the nanocarbon material was a commercially available acidified carbon nanotube (Pioneer Nano, carboxylated multi-walled carbon nanotube aqueous slurry); the silane coupling agent was γ-aminopropyltriethoxysilane; and the dispersion medium was ethanol. Example 2
[0078] The flame retardant heat-expandable microspheres provided in this embodiment are prepared by the same method as in Example 1, except that:
[0079] In step (1), the raw materials are 300 g of water, 5 g of hydrated aluminum hydroxide, 50 g of sodium chloride and 2 g of polyvinyl alcohol;
[0080] In step (2), the raw materials are 50 g of methacryloyloxyethyl phosphate, 100 g of the second polymerization monomer, 3 g of benzoyl peroxide, 50 g of n-heptane and 10 g of toluene diphenyl phosphate, and the second polymerization monomer is a combination of methacrylonitrile, maleic acid and butyl methacrylate in a mass ratio of 50:15:50;
[0081] In step (4), the raw materials are 10 g of an organic carbon-forming agent (triazine macromolecule, Connaught HF-T1020), 5 g of a nanocarbon material (Pioneer Nano, carboxylated multi-walled carbon nanotube aqueous slurry), and 1 g of a silane coupling agent (γ-aminopropyltriethoxysilane).
[0082] Finally, flame-retardant heat-expandable microspheres with a particle size of about 40 μm were obtained. Example 3
[0083] The flame retardant heat-expandable microspheres provided in this embodiment are prepared by the same method as in Example 1, except that:
[0084] In step (1), the raw materials are 500 g of water, 20 g of hydrated aluminum hydroxide, 50 g of sodium chloride and 2 g of polyvinyl alcohol;
[0085] In step (2), the raw materials are 30 g of the first polymerizable monomer, 50 g of the second polymerizable monomer, 3 g of benzoyl peroxide, 30 g of n-heptane and 30 g of bisphenol A-bis(diphenyl phosphate), wherein the first polymerizable monomer is a combination of 2-hydroxyethyl methacrylate phosphate and methacrylate diphosphate in a mass ratio of 1:1; and the second polymerizable monomer is a combination of ethoxyacrylonitrile, ethyl acrylic acid and isopropyl methacrylate in a mass ratio of 100:10:20.
[0086] Finally, flame-retardant heat-expandable microspheres with a particle size of about 30 μm were obtained.
[0087] Comparative Example 1
[0088] The flame retardant heat-expandable microspheres provided in this comparative example are prepared by the same method as in Example 1, except that in step (4), the organic carbon-forming agent is omitted.
[0089] Comparative Example 2
[0090] The flame retardant heat-expandable microspheres provided in this comparative example are prepared by the same method as in Example 1, except that the silane coupling agent and the nano-carbon material are omitted.
[0091] Application Example 1
[0092] The waterproof roll material provided in this example includes a first resin layer and a second resin layer stacked in sequence, and the first resin layer and the second resin layer are PVC resin layers respectively.
[0093] The raw material formulas of the first resin layer and the second resin layer respectively include the following components by weight:
[0094] PVC resin 90 parts;
[0095] DOP plasticizer 50 parts;
[0096] 3 parts of heat stabilizer;
[0097] Calcium carbonate 20 parts;
[0098] 0.1 part of ultraviolet absorber;
[0099] In addition to the above components, the second resin layer also contains the flame retardant heat expandable microspheres of Example 1, and the amount of the flame retardant heat expandable microspheres accounts for 1% of the total amount of raw materials of the second resin layer.
[0100] The waterproof coiled material is prepared by the following method:
[0101] The raw materials of the first resin layer and the second resin layer are respectively added into a twin-screw extruder for melting, extruded through a multi-layer co-extrusion device, and then pulled, calendered and cooled to obtain a waterproof coiled material, wherein the extrusion temperature is 170°C and the screw speed is 150 rpm.
[0102] The thickness of the waterproof coiled material is 1.5 mm, the thickness of the first resin layer is 0.5 mm, and the thickness of the second resin layer is 1 mm.
[0103] Application Example 2
[0104] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that the flame-retardant heat-expandable microspheres of Example 2 are added to the second resin layer, and the amount of the flame-retardant heat-expandable microspheres accounts for 0.5% of the total amount of raw materials in the second resin layer.
[0105] Application Example 3
[0106] The waterproof membrane provided in this example is basically the same as that in Application Example 1, except that:
[0107] The raw material formulas of the first resin layer and the second resin layer respectively include the following components by weight:
[0108] 100 parts of PVC resin;
[0109] DINP plasticizer 80 parts;
[0110] 3 parts of heat stabilizer;
[0111] Calcium carbonate 30 parts;
[0112] 0.1 part of ultraviolet absorber;
[0113] In addition to the above components, the second resin layer also contains the flame retardant heat expandable microspheres of Example 3, and the amount of the flame retardant heat expandable microspheres accounts for 0.8% of the total amount of raw materials of the second resin layer.
[0114] Application Example 4
[0115] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that: the raw material formulas of the first resin layer and the second resin layer respectively include the following components by weight:
[0116] PVC resin 80 parts;
[0117] DINP plasticizer 30 parts;
[0118] 3 parts of heat stabilizer;
[0119] 15 parts of calcium carbonate;
[0120] 0.1 part of ultraviolet absorber;
[0121] In addition to the above components, the second resin layer also contains the flame retardant heat expandable microspheres of Example 1, and the amount of the flame retardant heat expandable microspheres accounts for 1% of the total amount of raw materials of the second resin layer.
[0122] Application Comparative Example 1
[0123] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that the flame-retardant heat-expandable microspheres in the second resin layer are the flame-retardant heat-expandable microspheres of Comparative Example 1.
[0124] Application Comparative Example 2
[0125] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that the flame-retardant heat-expandable microspheres in the second resin layer are the flame-retardant heat-expandable microspheres of Comparative Example 2.
[0126] Application Comparative Example 3
[0127] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that the amount of the flame-retardant heat-expandable microspheres in the second resin layer is 3% of the total amount of raw materials in the second resin layer.
[0128] Application Comparative Example 4
[0129] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that in the second resin layer, a carbonate foaming agent is used instead of flame-retardant heat-expandable microspheres.
[0130] Application Comparative Example 5
[0131] The waterproof roll material provided in this example is basically the same as that in Application Example 1, except that: no flame-retardant heat-expandable microspheres are added to the second resin layer.
[0132] The waterproof membranes of Application Examples 1 to 4 and Comparative Examples 1 to 5 were tested for mechanical properties according to GB 12952-2011, for density according to GB / T 6343-2009, and for flame retardancy according to GB / T 2408-2021 and GB / T 2406. The results are shown in Tables 1 and 2.
[0133]
[0134]
[0135] It can be seen from Table 1 and Table 2 that, by comparing Application Example 1 and Application Comparative Examples 1 to 2, two-component modification of the microsphere surface can further improve the flame retardancy of the coil; by comparing Application Example 1 and Application Comparative Example 3, adding too much expanded microspheres will make the density drop more significantly, but the mechanical properties and flame retardancy drop sharply due to the increase in porosity; by comparing Application Example 1 and Application Comparative Example 4, compared with the inorganic foaming agent, the various properties drop significantly due to the generation of open pores, and it is impossible to simultaneously meet the requirements of density reduction, mechanical properties and flame retardancy.
[0136] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0137] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A waterproof roll material, comprising a first resin layer and a second resin layer stacked in sequence, wherein the first resin layer or the second resin layer contains flame-retardant heat-expandable microspheres, wherein the first resin layer and the second resin layer are PVC resin layers respectively, wherein the flame-retardant heat-expandable microspheres comprise a core material and a shell coated around the core material, wherein the core material comprises hydrocarbons and a liquid phosphorus-containing flame retardant, and wherein: The shell is a surface-modified acrylic polymer, the acrylic polymer is obtained by polymerizing a polymer monomer, and the shell is obtained by surface-modifying the acrylic polymer with a modifying material; The polymerizable monomers include a first polymerizable monomer and a second polymerizable monomer, wherein the first polymerizable monomer is an acrylic acid phosphate monomer, and the second polymerizable monomer is at least one of a nitrile monomer, a carboxyl acrylic acid monomer, and a methacrylic acid ester monomer; The modified materials are organic carbon-forming agent, inorganic carbon material and coupling agent; The mass ratio of the organic carbon-forming agent to the inorganic carbon material is 1:0.5-1.5; The mass of the flame-retardant heat-expandable microspheres is 0.5-1% of the total mass of the raw materials of the first resin layer or the second resin layer.
2. The waterproof coiled material according to claim 1, characterized in that: The raw materials of the first resin layer include PVC resin, plasticizer and filler; The raw materials of the second resin layer include PVC resin, the flame-retardant heat-expandable microspheres, a plasticizer and a filler; In the first resin layer and the second resin layer, the mass ratio of the PVC resin, the plasticizer and the filler is 1:0.2~1:0.1~0.
4.
3. The waterproof coiled material according to claim 2, characterized in that: In parts by weight, the raw material formulas of the first resin layer and the second resin layer independently include: PVC resin 80-100 parts; Plasticizer 20-80 parts; 15-30 parts of filler; The second resin layer further comprises flame-retardant heat-expandable microspheres in an amount of 0.5 to 1% of the total raw material amount of the second resin layer; and / or, The thickness ratio of the first resin layer to the second resin layer is 5:1-15.
4. The waterproof coiled material according to claim 3, characterized in that: The plasticizer is one or a combination of DOP, DINP, DOTP, and epoxidized soybean oil; and / or the filler is one or a combination of titanium dioxide, calcium carbonate, talcum powder, and clay; and / or the raw material formula of the first resin layer and the second resin layer also includes 2 to 6 parts of an auxiliary agent, and the auxiliary agent is one or a combination of a heat stabilizer and an anti-ultraviolet agent.
5. The waterproof coiled material according to claim 1, characterized in that: The organic carbon former is one or a combination of an organic phosphorus carbon former, a thermoplastic phenolic resin carbon former, a polyamide carbon former, a triazine derivative carbon former and a hyperbranched macromolecular flame retardant carbon former.
6. The waterproof coiled material according to claim 1, characterized in that: The inorganic carbon material is a nanocarbon material, and the nanocarbon material is one or a combination of carbon nanotubes, graphene, and nanocarbon balls; and / or, The coupling agent is a silane coupling agent.
7. The waterproof coiled material according to claim 1, characterized in that: The feed mass ratio of the first polymerizable monomer to the second polymerizable monomer is 30-50:50-100.
8. The waterproof coiled material according to claim 1, characterized in that: The acrylic acid phosphate monomer is one or a combination of acrylic acid monophosphate, acrylic acid diphosphate, methacrylic acid monophosphate, methacrylic acid diphosphate, methacryloyloxyethyl phosphate, and 2-hydroxyethyl methacrylate phosphate; and / or, The mass ratio of the nitrile monomer, the carboxyl acrylic acid monomer and the methacrylate monomer is 50-100:5-15:20-50.
9. The waterproof coiled material according to claim 1 or 8, characterized in that: The nitrile monomer is one or a combination of acrylonitrile, methacrylonitrile, chloroacrylonitrile, and ethoxyacrylonitrile; and / or The carboxyl acrylic acid monomer is one or a combination of acrylic acid, methacrylic acid, ethacrylic acid, maleic acid, monoethyl maleate, and monobutyl maleate; and / or, The methacrylate monomer is one or a combination of methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, butyl methacrylate, and benzyl methacrylate.
10. The waterproof coiled material according to claim 1, characterized in that: The hydrocarbon is a hydrocarbon with a boiling point above 60° C.; and / or, The liquid phosphorus-containing flame retardant is one or a combination of tributyl phosphate, dimethyl methyl phosphate, diethyl ethyl phosphate, tricresyl phosphate, diphenyl methyl phosphate, tri(xylene) phosphate, tri(butoxyethyl) phosphate, bisphenol A-bis(diphenyl phosphate) and resorcinol bis(diphenyl phosphate); and / or, The mass ratio of the first polymerizable monomer, the hydrocarbon and the liquid phosphorus-containing flame retardant is 30-50:30-50:5-30.
11. The waterproof coiled material according to any one of claims 1, 5 to 8, and 10, characterized in that: The particle size of the flame retardant heat-expandable microspheres is 30-80 μm.
12. The waterproof coiled material according to any one of claims 1, 5 to 8, and 10, characterized in that: The flame-retardant heat-expandable microspheres are prepared by suspension polymerization; and / or the flame-retardant heat-expandable microspheres further include a water-dispersible halogen-free flame retardant dispersed in the core material and / or the shell.
13. The waterproof coiled material according to claim 12, characterized in that: The water-dispersible halogen-free flame retardant is one or a combination of magnesium hydroxide, hydrated magnesium hydroxide, aluminum hydroxide, hydrated aluminum hydroxide, zinc oxide, and magnesium oxide; and / or, the feed mass ratio of the water-dispersible halogen-free flame retardant to the liquid phosphorus-containing flame retardant is 5~20:5~30.
14. The waterproof coiled material according to claim 1, characterized in that: The flame-retardant heat-expandable microspheres further include a water-dispersible halogen-free flame retardant dispersed in the core material and / or the shell. The preparation method of the flame-retardant heat-expandable microspheres includes the following steps: (1) uniformly mixing water, a water-dispersible halogen-free flame retardant, an electrolyte and an emulsifier to obtain an aqueous dispersion; (2) uniformly mixing the first polymerizable monomer, the second polymerizable monomer, the initiator, the hydrocarbon compound and the liquid phosphorus-containing flame retardant to obtain an oil phase dispersion; (3) adding the oil phase dispersion to the aqueous phase dispersion under stirring to obtain a pre-suspension, and then polymerizing under inert gas conditions to obtain microspheres with unmodified surfaces; (4) Dispersing the unmodified microspheres in a dispersion of a modified material to obtain the flame-retardant heat-expandable microspheres.
15. The waterproof coiled material according to claim 14, characterized in that: In step (4), the dispersion of the modified material comprises the modified material and a dispersion medium, and the dispersion medium is an alcohol solvent; and / or, In step (4), the microspheres with unmodified surfaces are added to the dispersion, mixed evenly, and then kept warm at 60±10° C. for 24 to 30 h, washed, and filtered to obtain the flame-retardant heat-expandable microspheres.
16. A method for preparing the waterproof coiled material according to any one of claims 1 to 15, characterized in that: The preparation method comprises melting the raw material of the first resin layer and the raw material of the second resin layer respectively, and co-extruding to obtain the waterproof coiled material.
Citation Information
Patent Citations
Preparation method of microencapsulated gradient halogen-free flame retardant system
CN102516603A
Production method for over-wide chlorinated polyethylene waterproof coiled material
CN102744860A
Low-pollution flame-retardant thermal expansion microspheres and preparation method thereof
CN108084333A
Thermally expanded microspheres, method
CN115175758A
Waterproof coiled material and preparation method thereof
CN117186569A