A production method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips
Metal magnesium and corundum are produced under vacuum conditions through the pellet heating method of flotation magnesite and waste aluminum chips, combined with electric arc furnace melting, which solves the problems of high cost and complex production of the existing thermite reduction magnesium process, and achieves Efficient, low-cost production of magnesium and corundum improves productivity and economic benefits.
Patent Information
- Application Number
- CN202410833478.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-26
AI Technical Summary
The existing aluminothermic magnesium reduction process has high costs, difficulty in producing high-purity alumina, complex production processes, and high energy consumption, resulting in high production costs for magnesium and corundum.
Flotation magnesite concentrate powder and waste aluminum chips are calcined in a suspension furnace to produce light-burned magnesium oxide powder, and pellets are heated with waste aluminum chips under vacuum conditions to achieve the simultaneous production of metallic magnesium and corundum, using arc The furnace melts into fused corundum, simplifying the process route and improving productivity.
It achieves efficient and low-cost production of metallic magnesium and high-purity corundum, reduces energy consumption and solid waste emissions, improves productivity and economic benefits, and has high process continuity and automation, and is environmentally friendly.
Smart Images

Figure CN118374699B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of non-ferrous light metal smelting and waste resource recycling, and specifically relates to a production method for simultaneously preparing metallic magnesium and corundum. Background Art
[0002] Magnesium is the third largest metal structural material after steel and aluminum, and is also the lightest metal structural material used in engineering so far. The main smelting processes of magnesium are electrolysis and thermal reduction. In the 20th century, 80% of the world's raw magnesium production was produced by electrolysis and 20% by thermal reduction. After the 1990s, the production of raw magnesium by thermal reduction increased rapidly. The thermal reduction method is divided into silicon thermal reduction method, aluminum thermal reduction method, and carbon thermal reduction method. Thermal reduction method of magnesium smelting began in 1913, and it has a history of nearly 100 years.
[0003] Aluminothermic magnesium smelting is a new magnesium smelting technology. This method uses magnesite and dolomite as raw materials and aluminum as a reducing agent to produce magnesium metal. Experimental studies have found that the use of aluminum as a reducing agent in the production of magnesium reduces the reaction temperature, accelerates the reaction speed, shortens the reduction cycle, and increases the purity of crude magnesium. The reduction slag can be used, etc. Due to its high cost, this process method has begun to be used in industry. The products of aluminothermic magnesium smelting are generally magnesium and magnesium-aluminum spinel.
[0004] Magnesium aluminum spinel is made of industrial alumina and light-burned magnesium oxide, which are synthesized by high-temperature sintering or electric melting. The chemical formula of magnesium aluminum spinel is MgO·Al O3, of which the MgO content is 28.2% and the Al2O3 content is 71.8%.
[0005] Patent CN 115807171 A proposes a green and environmentally friendly method for producing magnesium by aluminothermic reduction. Although it produces magnesium and magnesium-aluminum spinel with high purity, the MgO content in magnesium oxide is ≥96%, and the Al content in aluminum powder is ≥99.7%, resulting in high costs.
[0006] Patent CN 116102042 A proposes a method for simultaneously preparing metallic magnesium and alumina-magnesium spinel from magnesite, which uses two calcinations and adds a flocculant, resulting in a low alumina content in the alumina-magnesium spinel.
[0007] Patent CN 116005007 A proposes a method for preparing metallic magnesium and magnesium-aluminum spinel by aluminothermic reduction. Sodium fluoride and magnesium chloride are added to react the main impurities CaO and SiO3 with the additives. However, the remaining additives MgCl2 and NaF during the reduction process, as well as other components (metallic sodium and Na3AlF6) generated by the reaction, will overflow with the magnesium vapor, resulting in a low magnesium content in the finished product. Sodium hydroxide is added to reduce the alumina content.
[0008] At present, the aluminothermic reduction magnesium process cannot produce high-purity alumina. The main types of fused corundum are fused brown corundum and fused white corundum. When using high-alumina bauxite to produce brown corundum, the high-alumina bauxite needs to be pre-burned before fusion to remove the adsorbed water and structural water in it to speed up the fusion process and reduce power consumption. In order to fully reduce and effectively remove impurities during the fusion process, an appropriate amount of anthracite and iron powder needs to be added to the raw materials. When alumina is used to produce white corundum, due to the high purity of the raw materials, there is no need to use a reduction method to separate impurities. The alumina content of fused brown corundum is greater than 94.5%, and the alumina content of white corundum is greater than 98%. The cost of producing fused corundum alone is relatively high. Summary of the invention
[0009] The present invention aims at the shortcomings and deficiencies of the existing magnesium smelting methods, and provides a new method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips. The production method has the characteristics of continuous production process, safety and reliability, can make full use of magnesite resources and waste aluminum chips, can realize automated production, and reduce the physical labor of workers. The metallic magnesium has a high yield, no hazardous waste discharge, and is environmentally friendly. Through the reduction reaction, magnesium vapor and solid corundum slag are generated, and then the corundum slag is melted in an electric arc furnace to form electric fused corundum, which greatly reduces the production cost.
[0010] To achieve the above purpose, the present invention is implemented by adopting such a production method: using flotation magnesite concentrate powder as raw material, producing light-burned magnesium oxide powder by calcining in a suspension furnace, purifying the light-burned magnesium oxide powder by air separation, obtaining magnesium oxide powder with MgO≥97.5%, using waste aluminum chips or aluminum powder as a reducing agent, heating and preheating the pellets, reducing magnesium oxide under vacuum conditions, and simultaneously preparing metallic magnesium and corundum.
[0011] A production method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips comprises the following steps:
[0012] The magnesite ore is crushed into fine powder of 180-200 mesh, and then the fine powder is sent to the flotation machine to remove impurities in the magnesite through flotation to obtain a concentrate powder with a MgO content of ≥47.5%;
[0013] The magnesite concentrate powder after flotation is filtered and dried, and the moisture content of the dried concentrate powder is ≤3%;
[0014] Put the concentrate powder with MgO content ≥ 47.5% into the suspension furnace for calcination, and the calcination temperature is controlled at 900-1000℃;
[0015] The magnesium oxide powder calcined in the suspension furnace is passed through a cyclone separator and gravity air separation to further remove impurities in the magnesium oxide powder, thereby obtaining magnesium oxide powder with a content of MgO ≥ 97.5%;
[0016] Crushing the waste aluminum into particles of 0.1-0.5mm;
[0017] The magnesium oxide powder with a magnesium oxide content of MgO ≥ 97.5% and waste aluminum chips are crushed into waste aluminum chips with a particle size of 0.1-0.5 mm for mixing and batching to obtain a mixed material. The proportion of magnesium oxide and waste aluminum chips is based on the molecular weight ratio of the chemical reaction equation 3MgO+2Al=3Mg+Al2O3;
[0018] Ingredient ratio range: magnesium oxide powder accounts for 68-70%, aluminum powder accounts for 30-32%;
[0019] Grind the prepared materials through a vibration mill to achieve uniformity of the materials and control the particle size within 80-200 meshes;
[0020] The co-ground powder is put into a high-pressure ball press to be pressed into pellets, the average size of the pellets is 20-25mm, and the pressure of the ball press is controlled at 20Mpa;
[0021] The pellets are sent into a microwave heating furnace for heating, and the temperature of the pellets after heating is controlled to be 900°C, so as to shorten the heating time of the pellets in the reduction furnace;
[0022] The preheated pellets are fed into a reduction furnace through an automatic feeding device to undergo a reduction reaction, and magnesium vapor and solid corundum slag are generated through the reduction reaction;
[0023] The magnesium vapor flows into the magnesium crystallizer at the bottom of the reduction furnace, and the condensation temperature of the metal magnesium is 650°C; the magnesium crystallizer is cooled into solid metal magnesium, and the recovery rate of metal magnesium is 99%;
[0024] The Al2O3 content of the produced corundum slag is 96.38%.
[0025] The temperature of the corundum slag is 1000-1100°C, and the size of the corundum slag is greater than 0 and less than or equal to 25mm;
[0026] The vacuum degree in the reduction furnace is controlled at 1-5 Pa, the heating temperature is 1200-1300°C, and the reduction time of each furnace is 6-9 hours;
[0027] The corundum slag produced after reduction in the reduction furnace is automatically discharged from the reduction furnace and directly enters the electric arc furnace through the chute to be melted into fused corundum. The melting temperature of the corundum slag after entering the electric arc furnace is 2100-2300℃. The Al2O3 content of the melted fused corundum is greater than 96.5%, and the particle volume density is greater than 3.80g / cm 3 .
[0028] Preferably, the reduction furnace is a new type of gas reduction furnace with electric auxiliary heating, which includes a reduction tank installed in the gas heating furnace, a central tube installed in the reduction tank, a heat-conducting rib plate installed on the outer surface of the central tube, and the central tube is an electric heater, forming a reduction reaction space of the reduction tank with the central tube being internally heated and the gas heating furnace being externally heated.
[0029] Preferably, a layer of high-temperature aluminum oxide is thermally sprayed on the outer surfaces of the central tube and the heat-conducting ribs.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention is a production method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips. The two independent industrial production processes of vacuum aluminothermic reduction of magnesium and corundum slag are combined into one, so that metallic magnesium and corundum slag can be produced through a single heating process, and the corundum slag is then melted into fused corundum in an electric arc furnace, which simplifies the production process route, reduces energy consumption, and is a continuous production process.
[0032] 2. The present invention adopts a new type of gas-fired vacuum reduction furnace with electric auxiliary heating, which greatly reduces the heat penetration depth of heat conduction in the material, greatly shortens the reduction cycle, and greatly improves productivity; the magnesium crystallizer is arranged at the lower part of the reduction furnace to facilitate the flow and overflow of magnesium vapor.
[0033] 3. The heat utilization rate of the new gas vacuum reduction furnace with electric auxiliary heating of the present invention is increased from about 8-10% of the traditional furnace to more than 60%, which has a good energy-saving effect, and both the economic benefit and the environmental protection benefit are more obvious.
[0034] 4. The present invention provides a production method for simultaneously preparing metallic magnesium and corundum using magnesite and waste aluminum chips. The reduced slag is the primary product of corundum, which realizes the comprehensive utilization of resources, greatly reduces the discharge of solid waste slag, effectively reduces production costs, and improves economic benefits.
[0035] 5. Compared with the existing ferrosilicon reduction magnesium smelting technology, the present invention has a fast reduction reaction speed, high automation, easy operation, low labor intensity, less labor, high magnesium recovery rate, low cost, environmental friendliness, and low carbon dioxide emissions. It has been produced on the actual production line and achieved the expected goal. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention is a process flow chart of a production method for simultaneously preparing metallic magnesium and corundum using magnesite and waste aluminum chips.
[0037] Figure 2 This is the XRD diffraction pattern of the corundum slag of the present invention. DETAILED DESCRIPTION
[0038] The present invention is further described in detail below. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] For the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention.
[0041] See Figure 1 As shown: The technical solution of the production method of the present invention for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips is as follows:
[0042] The magnesite ore with high impurities is crushed into fine powder with a particle size of 180-200 mesh, and then the fine powder is sent to the flotation machine. According to the impurity content of the magnesite, different proportions of flotation agent and water are added. The SiO2 and other impurities in the magnesite are removed by flotation, thereby increasing the MgO content of the magnesite. The MgO of the concentrate powder after flotation is ≥47.5%.
[0043] The magnesite concentrate powder after flotation is filtered and dried to remove moisture from the concentrate powder. The moisture content of the dried concentrate powder is ≤3%.
[0044] The concentrate powder is put into the suspension furnace for calcination, and the calcination temperature is controlled at 900-1000℃. The output is controlled at 30-35t / h. The activity of magnesium oxide powder is ensured.
[0045] The magnesium oxide powder calcined in the suspension furnace passes through a cyclone separator, controls the wind velocity and pressure, and uses gravity air separation to further remove impurities such as SiO2, CaO, Fe2O3, etc. in the magnesium oxide, thereby increasing the MgO content of the magnesium oxide powder. The MgO content of the magnesium oxide powder after air separation is ≥97.5%.
[0046] The waste aluminum chips are crushed into particles of 0.1-0.5mm.
[0047] The magnesium oxide powder with a magnesium oxide content of MgO ≥ 97.5% and waste aluminum chips are crushed into waste aluminum chips with a particle size of 0.1-0.5 mm for mixing and batching to obtain a mixed material. The proportion of magnesium oxide and waste aluminum chips is based on the molecular weight ratio of the chemical reaction equation 3MgO+2Al=3Mg+Al2O3;
[0048] Ingredient ratio range: magnesium oxide powder accounts for 68-70%, and aluminum powder accounts for 30-32%.
[0049] The prepared materials are co-grinded with a vibration mill to achieve uniform material. The particle size is controlled at 80-200 mesh.
[0050] The co-ground powder is fed into a high-pressure ball press and pressed into pellets with an average pellet size of 20-25 mm. The pressure of the ball press is controlled at 20 MPa.
[0051] The pellets are sent into a microwave heating furnace for heating. The temperature of the pellets after heating is controlled to be 900°C and the preheating temperature is maintained so as to shorten the heating time of the pellets in the reduction furnace and improve production efficiency.
[0052] The heated pellets are fed into a reduction furnace through an automatic feeding device to undergo a reduction reaction, and magnesium vapor and solid corundum slag are generated through the reduction reaction;
[0053] The magnesium vapor flows into the magnesium crystallizer at the bottom of the reduction furnace, and the crystallizer temperature is controlled to obtain crystallized magnesium. The condensation temperature of the metal magnesium is 650°C. The magnesium crystallizer is cooled to form solid metal magnesium, and the recovery rate of metal magnesium is 99%.
[0054] The Al2O3 content of the produced corundum slag is 96.38%;
[0055] The temperature of the corundum slag is 1000-1100°C, and the size of the corundum slag is greater than 0 and less than or equal to 25mm;
[0056] The vacuum degree in the reduction furnace is controlled at 1-5 Pa, the heating temperature is 1200-1300°C, and the reduction time of each furnace is 6-9 hours;
[0057] The corundum slag produced after reduction in the reduction furnace is automatically discharged from the reduction furnace and directly enters the electric arc furnace through the chute to be melted into fused corundum. The melting temperature of the corundum slag after entering the electric arc furnace is 2100-2300℃. The Al2O3 content of the melted fused corundum is greater than 96.5%, and the particle volume density is greater than 3.80g / cm 3 .
[0058] Specifically, the reduction furnace is a new type of gas reduction furnace with electric auxiliary heating, which includes a reduction tank installed in the gas heating furnace, a central tube installed in the reduction tank, a heat-conducting rib plate installed on the outer surface of the central tube, and the central tube is an electric heater, forming a reduction reaction space of the reduction tank with the central tube as internal heating and the gas heating furnace as external heating, so as to improve the reaction efficiency.
[0059] Specifically, a layer of high-temperature aluminum oxide is thermally sprayed on the outer surfaces of the central tube and the heat-conducting ribs, so that the material does not adhere to the central tube and the heat-conducting ribs of the reduction furnace.
[0060] Specifically, the heat-conducting tube plate can reduce the heat penetration depth of heat conduction in the material, increase the strength of the central tube, and improve thermal efficiency.
[0061] Experimental data:
[0062] According to the chemical composition of magnesium oxide and aluminum powder: the MgO content of magnesium oxide powder is 97.5%, the active Al content of aluminum powder is 96%, and the weight ratio of molecular weight of aluminum powder is 3MgO+2Al=3Mg+Al2O3. The mass percentage of magnesium oxide and aluminum powder is 69%:31%. The prepared materials are co-grinded to a fineness of 200 mesh by a vibration mill. The experimental press is used to press into pellets with a diameter of 20mm, and the pressure of the press is controlled at 20Mpa. The pellet materials are sent to the vacuum reaction tank in the laboratory and the reduction reaction is carried out according to the prescribed procedures. The heating temperature is 1250℃, the insulation time is 8 hours, and the vacuum degree in the reduction tank is 1Pa. The final experimental results: material magnesium ratio: 2.54; the recovery rate of metal magnesium is 99%; the Mg content of metal magnesium is 99.98%; the Al2O3 content of the produced corundum slag is 96.38%, and the corundum slag is analyzed by X-ray diffraction, see attached Figure 2 The main crystal phase of the mineral is corundum phase (A), and the secondary crystal phases are aluminum magnesium spinel (AM) phase, periclase (M) phase, and calcium hexaaluminate (CA6) phase. It fully meets the chemical composition requirements of fused corundum specified in national standards. Embodiment 1:
[0063] Charge ratio: The mass percentage of calcined magnesium oxide and waste aluminum chips is: 70%, 30%
[0064] Implementation conditions: reduction reaction temperature 1300°C, reduction time 9 hours, vacuum degree 5Pa.
[0065] Implementation results: material-magnesium ratio: 2.8, magnesium recovery rate 98%.
[0066] Reduced magnesium component: contains Mg99.96%.
[0067] The density of treated corundum is 3.80g / cm 3 , containing 95.3% Al2O3 by mass.
[0068] Carbon dioxide emissions: 0.7t / ton of magnesium.
[0069] Solid waste discharge: 0 Embodiment 2:
[0070] Charge ratio: The mass percentage of calcined magnesium oxide and waste aluminum chips is: 69%, 31%
[0071] Implementation conditions: reduction reaction temperature 1300°C, reduction time 8 hours, vacuum degree 5Pa.
[0072] Implementation results: material-magnesium ratio: 2.8, magnesium recovery rate 98%.
[0073] Reduced magnesium component: contains Mg99.94%.
[0074] The density of treated corundum is 3.80g / cm 3 , containing 96% Al2O3 by mass.
[0075] Carbon dioxide emissions: 0.85t / ton of magnesium.
[0076] Solid waste discharge: 0 Embodiment 3:
[0077] Charge ratio: The mass percentage of calcined magnesium oxide and aluminum powder is: 68%, 32%
[0078] Implementation conditions: reduction reaction temperature 1280°C, reduction time 8 hours, vacuum degree 3Pa.
[0079] Implementation results: material-magnesium ratio: 2.8, magnesium recovery rate 98%.
[0080] Reduced magnesium component: contains Mg99.95%.
[0081] The density of treated corundum is 3.80g / cm 3 , containing 96.5% Al2O3 by mass.
[0082] Carbon dioxide emissions: 0.8t / ton of magnesium.
[0083] Solid waste discharge: 0
[0084] Example 4: (Comparative Example: Magnesium Refining by Ferrosilicon Reduction Method)
[0085] Charge ratio: the mass percentage of calcined silicon, ferrosilicon and fluorite powder are: 82%, 15% and 3%.
[0086] Implementation conditions: reduction reaction temperature 1250°C, reduction time 11.5 hours, vacuum degree 3Pa.
[0087] Implementation results: material-magnesium ratio: 6.5, magnesium recovery rate 70%.
[0088] Reduced magnesium component: contains Mg98.9%.
[0089] Carbon dioxide emissions: 17t / ton of magnesium
[0090] Solid waste emission: 5.5t / ton of magnesium.
[0091] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips, characterized in that: The following steps are involved: S1: crush the magnesite ore into fine powder with a particle size of 180-200 mesh, and then send the fine powder into a flotation machine to remove impurities in the magnesite ore through flotation to obtain a concentrate powder with a MgO content of ≥47.5%; S2: The magnesite concentrate powder after flotation is filtered and dried, and the moisture content of the dried concentrate powder is ≤3%; S3: Put the concentrate powder with MgO content ≥47.5% into the suspension furnace for calcination, and the calcination temperature is controlled at 900-1000℃; S4: The magnesium oxide powder produced by calcination in a suspension furnace is passed through a cyclone separator and gravity air separation to further remove impurities in the magnesium oxide powder, thereby obtaining magnesium oxide powder with a MgO content of ≥97.5%; S5: crushing the waste aluminum chips into particles of 0.1-0.5 mm; S6: Mixing magnesium oxide powder with a MgO content of ≥97.5% and waste aluminum chips crushed into a particle size of 0.1-0.5 mm to obtain a mixed material, wherein the ratio of magnesium oxide powder to waste aluminum chips is based on the molecular weight ratio of the chemical reaction equation 3MgO+2Al=3Mg+Al2O3; Ingredient ratio range: magnesium oxide powder accounts for 68-70%, aluminum powder accounts for 30-32%; S7: Grind the prepared materials through a vibration mill to make the materials uniform and control the particle size within 80-200 meshes; S8: Put the co-ground powder into a high-pressure ball press to press into pellets, the average size of the pellets is 20-25 mm, and the pressure of the ball press is controlled at 20 MPa; S9: sending the pellets into a microwave heating furnace for heating, and controlling the temperature of the pellets after heating to be 900° C., so as to shorten the heating time of the pellets in the reduction furnace; S10: feeding the preheated pellets into a reduction furnace through an automatic feeding device to perform a reduction reaction, and generating magnesium vapor and solid corundum slag through the reduction reaction; The magnesium vapor flows into the magnesium crystallizer at the bottom of the reduction furnace. The condensation temperature of the metal magnesium is 650°C. The magnesium crystallizer is cooled to become solid metal magnesium. The recovery rate of metal magnesium is 99%. The Al2O3 content of the produced corundum slag is 96.38%. The temperature of the corundum slag is 1000-1100°C, and the size of the corundum slag is greater than 0 and less than or equal to 25mm; The vacuum degree in the reduction furnace is controlled at 1-5 Pa, the heating temperature is 1200-1300°C, and the reduction time of each furnace is 6-9 hours; S11: The corundum slag produced after reduction in the reduction furnace is automatically discharged from the reduction furnace and directly enters the electric arc furnace through the chute to be melted into fused corundum. The melting temperature of the corundum slag after entering the electric arc furnace is 2100-2300℃. The Al2O3 content of the melted fused corundum is greater than 96.5%, and the particle volume density is greater than 3.80g / cm 3 .
2. The method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips according to claim 1, characterized in that: The reduction furnace is a gas reduction furnace with electric auxiliary heating, which includes a reduction tank installed in the gas heating furnace, a central tube installed in the reduction tank, and a heat-conducting rib plate installed on the outer surface of the central tube. The central tube is an electric heater, forming a reduction reaction space of the reduction tank with the central tube being internally heated and the gas heating furnace being externally heated.
3. The method for simultaneously preparing metallic magnesium and corundum from magnesite and waste aluminum chips according to claim 2, characterized in that: A layer of high-temperature aluminum oxide is thermally sprayed on the outer surfaces of the central tube and the heat-conducting rib plate.