A method for improving the electrical performance of lithium iron phosphate cathode materials through coating
By adding polymethacrylic acid to lithium iron phosphate materials and reacting it with a carbon source to form an ester coating, the problems of low conductivity and high-temperature expansion of lithium iron phosphate were solved, thus improving the electrochemical performance of the battery.
Patent Information
- Application Number
- CN202410264145.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-08
AI Technical Summary
Lithium iron phosphate has low electronic conductivity, which limits its performance in high-power applications. Furthermore, traditional coating agents are difficult to effectively improve its conductivity, leading to volume expansion issues at high temperatures.
By adding polymethyl methacrylate (PMAA) to the slurry, it reacts with the carbon source glucose to form esters, which are then used to coat lithium iron phosphate materials, suppressing high-temperature volume expansion and improving the material's electronic conductivity and ion transport rate.
It effectively suppressed the volume expansion of lithium iron phosphate at high temperatures, improved the electrical performance of the cathode material, and enhanced the overall graphitization reaction performance.
Smart Images

Figure CN118387850B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium-ion battery cathode material technology, and more specifically, to a method for improving the electrical performance of lithium iron phosphate cathode materials through coating. Background Technology
[0002] Lithium iron phosphate (LiFePO4) is an important cathode material for lithium-ion batteries, widely used in electric vehicles and energy storage devices due to its good thermal stability, high safety, and excellent cycle performance. However, the low electronic conductivity of lithium iron phosphate limits its performance in high-power applications to some extent.
[0003] To date, the main methods for modifying LiFePO4 include ion doping, surface coating, morphology control, and the addition of lithium-supplementing materials. LiFePO4 has extremely poor conductivity; however, by coating the surface with structurally stable and high-performance conductive / ion-conducting materials, the electronic and ion conduction between LiFePO4 particles can be improved. LiFePO4 coating modification can control particle size, reduce resistance during lithium-ion migration, improve the overall electronic conductivity and ion transport rate of the material, and further enhance the rate capability and low-temperature performance. Currently, traditional coating agents mainly include carbon materials, metals or metal oxides, and ion-conducting materials, which are difficult to effectively improve the conductivity of lithium iron phosphate and have limited impact on improving the discharge and cycle performance of the material. Furthermore, current power batteries using lithium iron phosphate as the cathode material generally suffer from volume expansion and poor electrical performance.
[0004] In view of the above, this application is hereby submitted. Summary of the Invention
[0005] To address the problems of existing technologies, this invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating. By adding polymethyl methacrylate (PMAA) to the slurry and heating it, PMAA reacts with the carbon source glucose to form esters, which can coat the material. Glucose normally begins to thermally decompose at around 300°C, but the product after reacting with PMAA only begins to thermally decompose at around 500°C. This effectively suppresses the volume expansion of lithium iron phosphate at high temperatures, thereby improving the electrical performance of the cathode material.
[0006] This invention is achieved through the following technical solution:
[0007] In a first aspect, the present invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials by coating, comprising the following steps:
[0008] (1) Lithium source, anhydrous iron phosphate, carbon source, titanium source and pure water are stirred and dispersed for a certain time. The dispersed slurry is put into a sand mill and ground at a certain rate for a certain time. After reaching the specified particle size, the precursor slurry is collected.
[0009] (2) Add the slurry to a mixer and heat it to 60°C. Add a certain amount of polymethyl methacrylate (PMAA) and stir for one hour. Then, connect the resulting slurry to a spray dryer and use a centrifugal spray dryer to obtain the precursor powder.
[0010] (3) The precursor powder was pre-sintered at high temperature in a nitrogen atmosphere, and the sintered sample was crushed by airflow to obtain lithium iron phosphate cathode material.
[0011] This invention improves the electrochemical performance of lithium iron phosphate by adding polymethyl methacrylate (PMAA) to the slurry. PMAA is a polymer with excellent thermal and chemical stability, which can effectively improve the electrochemical performance of lithium iron phosphate materials. By increasing the temperature, PMAA reacts with the carbon source glucose to form esters, which can coat the material. Glucose normally begins to decompose at around 300°C, but the product after reacting with PMAA only begins to decompose at around 500°C. This effectively inhibits the volume expansion of lithium iron phosphate at high temperatures, thereby improving the electrical performance of the cathode material and enhancing the overall graphitization reaction.
[0012] In one specific embodiment, in step (2), the total mass ratio of polymethyl methacrylate to iron phosphate is 0.005-0.012, and the stirring and dispersion time is 1 hour.
[0013] In a specific embodiment, in step (1), the iron-phosphorus molar ratio of the iron phosphate is 0.93 to 0.99, providing iron, phosphorus, and oxygen elements for the lithium iron phosphate material.
[0014] In a specific embodiment, in step (1), the lithium source is one or more of lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, and the molar ratio of lithium ions to iron phosphate is 1.001 to 1.07, providing lithium atoms for the lithium iron phosphate material.
[0015] In a specific embodiment, in step (1), the carbon source is one or more of sucrose, glucose, starch, polyethylene glycol, graphite, carbon nanotubes, and citric acid. The mass ratio of the carbon source to iron phosphate is 0.07 to 0.14, providing carbon elements for the lithium iron phosphate material. After sintering with an appropriate carbon source, a uniform carbon layer will be formed on the outer layer of the lithium iron phosphate material, increasing the electrical conductivity of the lithium iron phosphate material. At the same time, the coated carbon will limit the growth of lithium iron phosphate during the sintering process, and the smaller particles will also enhance the conductivity of the material.
[0016] In a specific embodiment, in step (1), the titanium source is anatase titanium dioxide with a particle size d50 of 5nm-200nm. The mass ratio of the titanium source to iron phosphate is 0.001-0.05. As an additive, it can change the material structure inside lithium iron phosphate during a single sintering process and improve the electrical performance of the material.
[0017] In a specific embodiment, in step (1), the stirring and dispersion time is 0.5 to 1.5 hours, the sand milling time is 1 to 4 hours, the operating speed is 200-1500 rpm, and the specified particle size D50 range is 0.2-0.4 μm.
[0018] In a specific embodiment, in step (2), the inlet temperature of the spray drying is set to 220-250°C, the outlet temperature is set to 90-140°C, and the D50 of the spherical lithium iron phosphate precursor particles obtained by spraying is 3-8 μm.
[0019] In a specific embodiment, in step (3), the first sintering temperature is 700-790℃, the oxygen content in the nitrogen atmosphere furnace is below 70ppm, the temperature is raised to 300℃ at a heating rate of 3℃ / min to 5℃ / min, and then raised to the final temperature at a heating rate of 1℃ / min-2℃ / min, held for 3-5 hours, and then cooled naturally in a nitrogen atmosphere.
[0020] In a specific embodiment, in step (3), the specified particle size distribution D50 of the sintered broken particles is 0.2 to 0.9 μm.
[0021] Secondly, the present invention also provides a lithium iron phosphate cathode material prepared by coating, which is a lithium iron phosphate material prepared by the method of improving the electrical performance of lithium iron phosphate cathode material by coating.
[0022] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0023] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating. By adding polymethyl methacrylate (PMAA) to the slurry, PMAA, a polymer material with excellent thermal and chemical stability, can effectively improve the electrochemical performance of lithium iron phosphate materials. By raising the temperature, PMAA can react with the carbon source glucose to form esters, which can coat the material. Originally, glucose begins to decompose at around 300°C, but after reacting with PMAA, the product only begins to decompose at around 500°C, effectively inhibiting the volume expansion of lithium iron phosphate at high temperatures, thereby improving the electrical performance of the cathode material and enhancing the overall graphitization reaction. Attached Figure Description
[0024] To more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 This is a flowchart of a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, provided in an embodiment of the present invention.
[0026] Figure 2 This is a scanning electron microscope image of the lithium iron phosphate cathode material prepared in Example 1 of the present invention;
[0027] Figure 3 This is a scanning electron microscope image of the lithium iron phosphate cathode material prepared in Example 2 of the present invention;
[0028] Figure 4 This is a scanning electron microscope image of the lithium iron phosphate cathode material prepared in Example 3 of the present invention;
[0029] Figure 5 This is a scanning electron microscope image of the lithium iron phosphate cathode material prepared in Example 4 of the present invention;
[0030] Figure 6 This is a scanning electron microscope image of the lithium iron phosphate cathode material prepared in Example 5 of the present invention;
[0031] Figure 7 The image shows the electrochemical performance test results of the lithium iron phosphate cathode material prepared in Example 1 of this invention. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the embodiments and accompanying drawings. The illustrative embodiments and descriptions of the present invention are only used to explain the present invention and are not intended to limit the present invention.
[0033] In the following description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that these specific details are not necessary to practice the invention. In other embodiments, well-known materials or methods have not been specifically described in order to avoid obscuring the invention.
[0034] Throughout this specification, references to "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in connection with that embodiment or example is included in at least one embodiment of the invention. Therefore, the phrases "an embodiment," "an example," "an example," or "an example" appearing in various places throughout the specification do not necessarily refer to the same embodiment or example. Furthermore, specific features, structures, or characteristics can be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. Moreover, those skilled in the art will understand that the illustrations provided herein are for illustrative purposes and are not necessarily drawn to scale. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0035] In the description of this invention, the terms "front", "rear", "left", "right", "up", "down", "vertical", "horizontal", "high", "low", "inner", and "outer" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limiting the scope of protection of this invention.
[0036] Preparation Example
[0037] like Figure 1 As shown, this embodiment of the invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps:
[0038] (1) Lithium source, anhydrous iron phosphate, carbon source, titanium source and pure water are stirred and dispersed for a certain time. The dispersed slurry is put into a sand mill and ground at a certain rate for a certain time. After reaching the specified particle size, the precursor slurry is collected.
[0039] (2) Add the slurry to a mixer and heat it to 60°C. Add a certain amount of polymethyl methacrylate (PMAA) and stir for one hour. Then, connect the resulting slurry to a spray dryer and use a centrifugal spray dryer to obtain the precursor powder.
[0040] (3) The precursor powder was pre-sintered at high temperature in a nitrogen atmosphere, and the sintered sample was crushed by airflow to obtain lithium iron phosphate cathode material.
[0041] This invention improves the electrochemical performance of lithium iron phosphate by adding polymethyl methacrylate (PMAA) to the slurry. PMAA is a polymer with excellent thermal and chemical stability, which can effectively improve the electrochemical performance of lithium iron phosphate materials. By increasing the temperature, PMAA reacts with the carbon source glucose to form esters, which can coat the material. Glucose normally begins to decompose at around 300°C, but the product after reacting with PMAA only begins to decompose at around 500°C. This effectively inhibits the volume expansion of lithium iron phosphate at high temperatures, thereby improving the electrical performance of the cathode material and enhancing the overall graphitization reaction.
[0042] In one specific embodiment, in step (2), the total mass ratio of polymethyl methacrylate to iron phosphate is 0.005-0.012, and the stirring and dispersion time is 1 hour.
[0043] In a specific embodiment, in step (1), the iron-phosphorus molar ratio of the iron phosphate is 0.93 to 0.99, providing iron, phosphorus, and oxygen elements for the lithium iron phosphate material.
[0044] In a specific embodiment, in step (1), the lithium source is one or more of lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, and the molar ratio of lithium ions to iron phosphate is 1.001 to 1.07, providing lithium atoms for the lithium iron phosphate material.
[0045] In a specific embodiment, in step (1), the carbon source is one or more of sucrose, glucose, starch, polyethylene glycol, graphite, carbon nanotubes, and citric acid. The mass ratio of the carbon source to iron phosphate is 0.07 to 0.14, providing carbon elements for the lithium iron phosphate material. After sintering with an appropriate carbon source, a uniform carbon layer will be formed on the outer layer of the lithium iron phosphate material, increasing the electrical conductivity of the lithium iron phosphate material. At the same time, the coated carbon will limit the growth of lithium iron phosphate during the sintering process, and the smaller particles will also enhance the conductivity of the material.
[0046] In a specific embodiment, in step (1), the titanium source is anatase titanium dioxide with a particle size d50 of 5nm-200nm. The mass ratio of the titanium source to iron phosphate is 0.001-0.05. As an additive, it can change the material structure inside lithium iron phosphate during a single sintering process and improve the electrical performance of the material.
[0047] In a specific embodiment, in step (1), the stirring and dispersion time is 0.5 to 1.5 hours, the sand milling time is 1 to 4 hours, the operating speed is 200-1500 rpm, and the specified particle size D50 range is 0.2-0.4 μm.
[0048] In a specific embodiment, in step (2), the inlet temperature of the spray drying is set to 220-250°C, the outlet temperature is set to 90-140°C, and the D50 of the spherical lithium iron phosphate precursor particles obtained by spraying is 3-8 μm.
[0049] In a specific embodiment, in step (3), the first sintering temperature is 700-790℃, the oxygen content in the nitrogen atmosphere furnace is below 70ppm, the temperature is raised to 300℃ at a heating rate of 3℃ / min to 5℃ / min, and then raised to the final temperature at a heating rate of 1℃ / min-2℃ / min, held for 3-5 hours, and then cooled naturally in a nitrogen atmosphere.
[0050] In a specific embodiment, in step (3), the specified particle size distribution D50 of the sintered broken particles is 0.2 to 0.9 μm.
[0051] Secondly, the present invention also provides a lithium iron phosphate cathode material prepared by coating, which is a lithium iron phosphate material prepared by the method of improving the electrical performance of lithium iron phosphate cathode material by coating.
[0052] Example 1
[0053] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps:
[0054] 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of ferric phosphate, 2.8g of titanium dioxide, and 90g of glucose were added to a stirrer and dispersed for 1 hour. The dispersed slurry was then fed to a sand mill to grind the particles to a D50 of 0.38µm. 5g of polymethyl methacrylate was added to the slurry, and the mixture was heated to 60℃ and stirred for 1 hour. The slurry was then spray-dried to obtain a powder with a D50 of 8.73µm. The powder was then placed in a graphite crucible and sintered once in a box furnace under an inert gas atmosphere at 770℃ for 3.5 hours. The sintered material was then subjected to air jet milling, resulting in a particle size D50 of 0.68µm. Scanning electron microscopy (SEM) results are shown below. Figure 2 As shown, the electrochemical performance test is as follows: Figure 7 As shown.
[0055] Example 2
[0056] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps: 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of iron phosphate, 2.8g of titanium dioxide, and 90g of glucose are added to a stirrer and dispersed for 1 hour. The dispersed slurry is then fed to a sand mill to grind the particles to a D50 of 0.43µm. 7g of polymethyl methacrylate is added to the slurry, and the mixture is heated to 60°C and stirred for 1 hour. The slurry is then spray-dried to obtain powder with a D50 of 9.14µm. The powder is then placed in a graphite crucible and sintered once in a box furnace under an inert gas atmosphere at a sintering temperature of 770°C for 3.5 hours. The sintered material is then subjected to air jet milling, resulting in a particle size D50 of 0.73µm. The scanning electron microscope (SEM) results are shown below. Figure 3 As shown.
[0057] Example 3
[0058] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps:
[0059] 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of ferric phosphate, 2.8g of titanium dioxide, and 90g of glucose were added to a stirrer and dispersed for 1 hour. The dispersed slurry was then fed to a sand mill to grind the particles to a D50 of 0.48µm. 8g of polymethyl methacrylate was added to the slurry, and the mixture was heated to 60℃ and stirred for 1 hour. The slurry was then spray-dried to obtain a powder with a D50 of 9.77µm. The powder was then placed in a graphite crucible and sintered once in a box furnace under an inert gas atmosphere at 770℃ for 3.5 hours. The sintered material was then subjected to air jet milling, and the particle size D50 of the crushed material was 0.79µm. Scanning electron microscopy (SEM) results are shown below. Figure 4 As shown.
[0060] Example 4
[0061] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps:
[0062] 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of ferric phosphate, 2.8g of titanium dioxide, and 90g of glucose were added to a stirrer and dispersed for 1 hour. The dispersed slurry was then fed to a sand mill to grind the particles to a D50 of 0.45µm. 9g of polymethyl methacrylate was added to the slurry, and the mixture was heated to 60℃ and stirred for 1 hour. The slurry was then spray-dried to obtain a powder with a D50 of 9.32µm. The powder was then placed in a graphite crucible and sintered once in a box furnace under an inert gas atmosphere at 770℃ for 3.5 hours. The sintered material was then subjected to air jet milling, and the particle size D50 of the crushed material was 0.75µm. Its scanning electron microscope results are shown below. Figure 5 As shown.
[0063] Example 5
[0064] This invention provides a method for improving the electrical performance of lithium iron phosphate cathode materials through coating, comprising the following steps: 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of iron phosphate, 2.8g of titanium dioxide, and 90g of glucose are added to a stirrer and dispersed for 1 hour. The dispersed slurry is then fed to a sand mill to grind the particles to a D50 of 0.4µm. 12g of polymethyl methacrylate is added to the slurry, and the mixture is heated to 60°C and stirred for 1 hour. The slurry is then spray-dried to obtain powder with a D50 of 9.07µm. The powder is then placed in a graphite crucible and sintered once in a box furnace under an inert gas atmosphere at 770°C for 3.5 hours. The sintered material is then subjected to air jet milling, resulting in a particle size D50 of 0.7µm. The scanning electron microscope (SEM) results are shown below. Figure 6 As shown.
[0065] Comparative Example 1
[0066] This comparative example provides a conventional method for preparing lithium iron phosphate cathode materials using carbon coating, the steps of which are as follows:
[0067] 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of iron phosphate, 2.8g of titanium dioxide, and 90g of glucose were added to a stirrer and stirred and dispersed for 1 hour. The dispersed slurry was then fed to a sand mill to grind the particles to a D50 of 0.4µm. The slurry was then spray-dried to obtain powder with a D50 of 7.5µm. The powder was then placed in a graphite sagger and sintered once in a box furnace under an inert gas atmosphere at a sintering temperature of 770℃ for 10 hours. The sintered material was then subjected to air jet milling, and the particle size D50 of the crushed material was 0.9µm.
[0068] Comparative Example 2
[0069] This comparative example provides a conventional method for preparing lithium iron phosphate cathode materials using carbon coating, the steps of which are as follows:
[0070] 2025.6g of pure water, 257.6g of lithium carbonate, 1000g of iron phosphate, 2.8g of titanium dioxide, and 90g of glucose were added to a stirrer and stirred and dispersed for 1 hour. The dispersed slurry was then fed to a sand mill and ground to a particle size D50 of 0.48µm. The slurry was then spray-dried to obtain a powder with a D50 of 13.7µm. The powder was then placed in a graphite sagger and sintered once in a box furnace under an inert gas atmosphere at a temperature of 780℃ for 10 hours. The sintered material was then subjected to air jet milling, and the particle size D50 of the crushed material was 1.1µm.
[0071] The lithium iron phosphate materials prepared in Examples 1-5 and Comparative Examples 1-2 were assembled into batteries for relevant electrical performance tests. Battery assembly was performed in a glove box under a high-purity argon atmosphere. The prepared positive electrode was used as the positive electrode, lithium foil as the negative electrode, and a 1 mol / L LiPF6 / EC (ethylene carbonate) / DMC (diethyl carbonate) electrolyte (EC and DMC volume ratio 1:1) was used as the electrolyte. A polypropylene microporous membrane was used as the separator. Battery performance was tested using a two-electrode battery testing module. The charge-discharge performance of the positive electrode material was tested on a battery testing system. A constant current charge-discharge regime was adopted, with a charge-discharge voltage range of 2.0-4.2 V. A 1-minute rest period was set before each constant current process. The performance test results are shown in Table 1.
[0072] Table 1
[0073] Preparation process 0.1C initial discharge capacity 1C discharge capacity 5C discharge capacity Example 1 162mAh / g 153mAh / g 137mAh / g Example 2 163mAh / g 154mAh / g 138mAh / g Example 3 166mAh / g 156mAh / g 142mAh / g Example 4 165mAh / g 155mAh / g 140mAh / g Example 5 162mAh / g 152mAh / g 138mAh / g Comparative Example 1 160mAh / g 148mAh / g 134mAh / g Comparative Example 2 159mAh / g 144mAh / g 132mAh / g
[0074] As can be seen from Table 1, Examples 1-5 of the present invention, by adding polymethyl methacrylate to the raw materials, allow PMAA to react with the carbon source glucose during sintering to form esters, thus coating the lithium iron phosphate material. Compared with Comparative Examples 1 and 2, which form physical carbon coating of lithium iron phosphate material through carbon sources, the electrochemical performance is improved. This is because traditional carbon sources, such as glucose, begin to thermally decompose at around 300°C, while the ester products generated after the reaction of glucose and PMAA in the present invention only begin to thermally decompose at around 500°C. This effectively inhibits the volume expansion of lithium iron phosphate at high temperatures, thereby improving the electrical performance of the cathode material and enhancing the overall graphitization reaction.
[0075] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for improving the electrical performance of lithium iron phosphate cathode materials through coating, characterized in that, Includes the following steps: (1) The lithium source, anhydrous iron phosphate, carbon source, titanium source and pure water are mixed, stirred and dispersed and then ground to obtain the precursor slurry; (2) The precursor slurry was stirred and heated and polymethyl methacrylate was added and continuously stirred and dispersed, and then spray dried to obtain the precursor powder; (3) The precursor powder is pre-sintered at high temperature in a nitrogen atmosphere, and then crushed to a specified particle size to obtain lithium iron phosphate cathode material.
2. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (2), the total mass of polymethacrylic acid to the mass ratio of iron phosphate is 0.005-0.012, and the stirring and dispersion time is 1 hour.
3. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (1), the iron-phosphorus molar ratio of the iron phosphate is 0.93 to 0.
99.
4. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (1), the lithium source is one or more of lithium carbonate, lithium nitrate, lithium hydroxide, and lithium acetate, and the molar ratio of the lithium source to iron phosphate is 1.001 to 1.
07.
5. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (1), the carbon source is one or more of sucrose, glucose, starch, polyethylene glycol, graphite, carbon nanotubes, and citric acid, and the mass ratio of the carbon source to iron phosphate is 0.07 to 0.
14.
6. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (1), the titanium source is anatase titanium dioxide, and the mass ratio of the titanium source to iron phosphate is 0.001 to 0.
05.
7. The method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (1), the stirring and dispersing time is 0.5 to 1.5 hours, the sand milling time is 1 to 4 hours, and the operating speed is 200-1500 rpm.
8. A method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (2), the inlet temperature of the spray drying is set to 220-250℃, the outlet temperature is set to 90-140℃, and the D50 of the spherical lithium iron phosphate precursor particles obtained by spraying is 3-8 μm.
9. A method for improving the electrical performance of lithium iron phosphate cathode material by coating according to claim 1, characterized in that, In step (3), the first sintering temperature is 700-790℃, the oxygen content in the nitrogen atmosphere furnace is below 70ppm, the temperature is raised to 300℃ at a heating rate of 3℃ / min to 5℃ / min, and then raised to the final temperature at a heating rate of 1℃ / min-2℃ / min, and held for 3-5h; the specified particle size distribution D50 of the broken particles after sintering is 0.2-0.9um.
10. A lithium iron phosphate cathode material prepared by coating, characterized in that, The lithium iron phosphate material is prepared by the method described in any one of claims 1 to 9, which improves the electrical performance of the lithium iron phosphate cathode material through coating.
Citation Information
Patent Citations
Preparation method for lithium iron phosphate cathode material
CN104300119A