Screen surface coating and preparation method thereof
By using composite coatings of polymethyl methacrylate, fluorocarbon resin, nanosilicon dioxide or nanotitanium dioxide on the surface of the photovoltaic module screen, the problem of easy aging and falling off of existing coatings is solved, and high weather resistance is achieved and self-repair performance, extending service life and maintaining the performance stability of photovoltaic modules.
Patent Information
- Application Number
- CN202411209363.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing photovoltaic module screen surface coatings are susceptible to environmental factors to aging and shedding during long-term use, and have limited weather resistance, especially in extreme climate conditions, showing poor performance and service life.
Using composite coatings of polymethyl methacrylate, fluorocarbon resin, nanosilicon dioxide or nanotitanium dioxide, rare earth oxides, multi-wall carbon nanotubes and self-healing microcapsules, through specific surface treatment processes and ultraviolet light The curing method forms a coating with excellent hydrophobic, wear-resistant, anti-aging and self-healing properties.
It significantly improves the hydrophobic properties, weather resistance and wear resistance of the coating, extends the service life of the screen, and maintains the performance stability of the photovoltaic module and the clarity of the printing pattern under extreme conditions.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of screen printing, in particular to a screen printing surface coating and a preparation method thereof. Background Art
[0002] With the rapid development of modern technology, screens, as key optoelectronic equipment components, play an increasingly important role in communications, reconnaissance, navigation and other fields. Screens for photovoltaic modules usually refer to mesh templates used to print specific patterns (such as electrodes, insulation layers, etc.) on the surface of photovoltaic cells during the manufacturing process of photovoltaic cells. These screens are made of fine metal wires or synthetic materials with precise mesh structures and pattern designs to ensure accuracy and consistency of printing.
[0003] Screen surface coating plays a key role in photovoltaic manufacturing, aiming to improve the performance, weather resistance and durability of photovoltaic modules. The specific functions are: 1. Protect the screen: The coating can protect the screen from damage by environmental factors such as chemical corrosion, mechanical wear and ultraviolet radiation, and extend the service life of the screen.
[0004] 2. Improve printing quality: The coating can improve the surface properties of the screen, such as improving wettability, reducing the friction coefficient, etc., thereby improving the clarity and consistency of the printed pattern.
[0005] 3. Enhanced functionality: Certain functional coatings (such as anti-reflective coatings, insulating coatings, etc.) can give the screen additional performance, further improving the photoelectric conversion efficiency and safety of photovoltaic modules.
[0006] The surface coatings currently used for photovoltaic module screens still have the following shortcomings: 1. During long-term use, the performance of some coating materials may change due to environmental factors (such as ultraviolet rays, high temperature, humidity, etc.), resulting in aging and peeling of the coating.
[0007] 2. Limited weather resistance: Although many coatings claim to have excellent weather resistance, the weather resistance of the coating may be challenged under extreme climatic conditions, such as strong UV radiation, extreme temperature fluctuations, etc., thus affecting the overall performance and service life of the photovoltaic module. Summary of the invention
[0008] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a screen surface coating and a preparation method thereof to solve the above technical problems.
[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: A screen surface coating, the composition by weight is as follows: 20-40 parts of polymethyl methacrylate, 3-8 parts of fluorocarbon resin, 1.2-3.6 parts of silicon nitride, 0.2-0.5 parts of aluminum oxide, 0.01-0.02 parts of rare earth oxide, 0.01-0.03 parts of nanoparticles, 0.001-0.003 parts of carbon nanotubes, 0.01-0.03 parts of self-repairing microcapsules, 0.02-0.03 parts of ultraviolet absorbers, 0.03-0.06 parts of antioxidants, and 0.003-0.006 parts of antistatic agents.
[0010] Nano silicon dioxide particles have low surface energy and can effectively reduce the wettability of the coating surface, making the coating show excellent hydrophobic properties. In addition, nano silicon dioxide can also improve the hardness, wear resistance and anti-aging properties of the coating. In addition to photocatalytic properties, nano titanium dioxide can also obtain hydrophobic properties through a specific surface treatment process. This nano material can form a dense hydrophobic layer on the surface of the coating, effectively blocking the penetration of moisture and oil. The coating prepared by compounding nano silicon dioxide or nano titanium dioxide with fluorocarbon resin in the present invention has both excellent hydrophobic and oleophobic properties and good weather resistance and wear resistance.
[0011] The microcapsule self-repairing material of the present invention, when the coating is damaged, the capsules rupture to release the repairing agent, and the repairing agent undergoes a polymerization reaction under the action of a catalyst or external conditions (such as temperature and humidity) to fill the damaged area and achieve self-repair.
[0012] Rare earth oxides have good optical properties and chemical stability, and can be used to improve the light transmittance, anti-reflection and weather resistance of coatings. They can be combined with fluorocarbon resins to form composites, thereby having higher light absorption efficiency and better thermal stability.
[0013] The invention adds multi-walled carbon nanotubes to improve the mechanical properties and thermal stability of the screen.
[0014] Furthermore, the rare earth oxide is selected from one of cerium oxide and lanthanum oxide.
[0015] Furthermore, the nanoparticles are selected from one of nano-titanium dioxide and nano-silicon dioxide.
[0016] Furthermore, the shell layer of the self-repairing microcapsule is urea-formaldehyde resin, and the core material is epoxy resin or polyurethane.
[0017] Furthermore, the ultraviolet absorber is selected from one of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,4-dihydroxybenzophenone, and 2-hydroxy-4-methoxybenzophenone.
[0018] Furthermore, the antioxidant is selected from one of butylated hydroxytoluene and butylated hydroxyanisole.
[0019] Furthermore, the antistatic agent is amide phosphate.
[0020] Furthermore, the carbon nanotubes are multi-walled carbon nanotubes with 2-50 layers and an average interlayer spacing of 0.34±0.02 nm.
[0021] A method for preparing a screen surface coating, the preparation method comprising the following steps: S1 Coating composition preparation: 1) dissolving polymethyl methacrylate and fluorocarbon resin in xylene solvent, pre-dispersing silicon nitride and aluminum oxide nanoparticles in toluene solvent, and then mixing and stirring the two; 2) Add rare earth oxides and carbon nanotubes and continue stirring to mix; 3) adding self-repairing microcapsules, ultraviolet absorbers, antioxidants and antistatic agents, stirring and mixing, and obtaining a coating composition for use; S2 Surface coating: 1) Pretreatment: Clean, degrease and dry the screen surface to ensure good bonding between the coating and the screen; 2) Coating: uniformly coating the composition obtained in step S1 on the surface of the screen; 3) Curing treatment: After the coating is applied, it is cured by ultraviolet light to obtain the surface coating.
[0022] Beneficial effects: Nano silicon dioxide particles have low surface energy and can effectively reduce the wettability of the coating surface, making the coating show excellent hydrophobic properties. In addition, nano silicon dioxide can also improve the hardness, wear resistance and anti-aging properties of the coating. In addition to photocatalysis, nano titanium dioxide can also obtain hydrophobic properties through a specific surface treatment process. This nano material can form a dense hydrophobic layer on the surface of the coating, effectively blocking the penetration of moisture and oil. The coating prepared by compounding nano silicon dioxide or nano titanium dioxide with fluorocarbon resin in the present invention has both excellent hydrophobic and oleophobic properties and good weather resistance and wear resistance.
[0023] The microcapsule self-repairing material of the present invention, when the coating is damaged, the capsules rupture to release the repairing agent, and the repairing agent undergoes a polymerization reaction under the action of a catalyst or external conditions (such as temperature and humidity) to fill the damaged area and achieve self-repair.
[0024] Rare earth oxides have good optical properties and chemical stability, and can be used to improve the light transmittance, anti-reflection and weather resistance of coatings. They can be combined with fluorocarbon resins to form composites, thereby having higher light absorption efficiency and better thermal stability.
[0025] The invention adds multi-walled carbon nanotubes to improve the mechanical properties and thermal stability of the screen. DETAILED DESCRIPTION
[0026] The surface coating of the D-type screen and the preparation method thereof in the present invention are further described below in conjunction with specific embodiments.
[0027] The raw materials in the present invention are all commonly available on the market.
[0028] Example 1 A screen surface coating, the composition by weight is as follows: 20 parts of polymethyl methacrylate, 3 parts of fluorocarbon resin, 1.2 parts of silicon nitride, 0.2 parts of aluminum oxide, 0.01 parts of rare earth oxide, 0.01 parts of nanoparticles, 0.001 parts of carbon nanotubes, 0.01 parts of self-repairing microcapsules, 0.02 parts of ultraviolet absorbers, 0.03 parts of antioxidants, and 0.003 parts of antistatic agents.
[0029] Among them, the rare earth oxide is cerium oxide.
[0030] Among them, the nanoparticles are nano titanium dioxide.
[0031] The shell layer of the self-repairing microcapsule is urea-formaldehyde resin, and the core material is epoxy resin or polyurethane.
[0032] The ultraviolet absorber is 2-(2'-hydroxy-5'-methylphenyl)benzotriazole.
[0033] Wherein, butylated hydroxytoluene is selected as the antioxidant.
[0034] Among them, the antistatic agent is amide phosphate.
[0035] The carbon nanotubes are multi-walled carbon nanotubes with 10 layers and an average interlayer spacing of 0.15 nm.
[0036] The method for preparing the screen surface coating comprises the following steps: S1 Coating composition preparation: 1) dissolving polymethyl methacrylate and fluorocarbon resin in xylene solvent, pre-dispersing silicon nitride and aluminum oxide nanoparticles in toluene solvent, and then mixing and stirring the two; 2) Add rare earth oxides and carbon nanotubes and continue stirring to mix; 3) adding self-repairing microcapsules, ultraviolet absorbers, antioxidants and antistatic agents, stirring and mixing, and obtaining a coating composition for use; S2 Surface coating: 1) Pretreatment: Clean, degrease and dry the screen surface to ensure a good bond between the coating and the screen; 2) Coating: uniformly coating the composition obtained in step S1 on the surface of the screen; 3) Curing treatment: After the coating is applied, the surface coating is cured by ultraviolet light. The wavelength of the ultraviolet light source is 365nm, the light intensity is 60mW / cm², the curing time is 30min, and the thickness of the cured coating is 12μm.
[0037] Example 2 A screen surface coating, the composition by weight is as follows: 30 parts of polymethyl methacrylate, 6 parts of fluorocarbon resin, 2.4 parts of silicon nitride, 0.3 parts of aluminum oxide, 0.015 parts of rare earth oxide, 0.02 parts of nanoparticles, 0.002 parts of carbon nanotubes, 0.02 parts of self-repairing microcapsules, 0.025 parts of ultraviolet absorbers, 0.04 parts of antioxidants, and 0.005 parts of antistatic agents.
[0038] Among them, the rare earth oxide is lanthanum oxide.
[0039] Among them, the nanoparticles are nano silicon dioxide.
[0040] The shell layer of the self-repairing microcapsule is urea-formaldehyde resin, and the core material is epoxy resin or polyurethane.
[0041] Among them, the ultraviolet absorber is 2,4-dihydroxybenzophenone.
[0042] Wherein, butylated hydroxytoluene is selected as the antioxidant.
[0043] Among them, the antistatic agent is amide phosphate.
[0044] The carbon nanotubes are multi-walled carbon nanotubes with 30 layers and an average interlayer spacing of 0.2 nm.
[0045] A method for preparing a screen surface coating, the preparation method comprising the following steps: S1 Coating composition preparation: 1) dissolving polymethyl methacrylate and fluorocarbon resin in xylene solvent, pre-dispersing silicon nitride and aluminum oxide nanoparticles in toluene solvent, and then mixing and stirring the two; 2) Add rare earth oxides and carbon nanotubes and continue stirring to mix; 3) adding self-repairing microcapsules, ultraviolet absorbers, antioxidants and antistatic agents, stirring and mixing, and obtaining a coating composition for use; S2 Surface coating: 1) Pretreatment: Clean, degrease and dry the screen surface to ensure good bonding between the coating and the screen; 2) Coating: uniformly coating the composition obtained in step S1 on the surface of the screen; 3) Curing treatment: After the coating is applied, the surface coating is cured by ultraviolet light. The wavelength of the ultraviolet light source is 365nm, the light intensity is 60mW / cm², the curing time is 30min, and the thickness of the cured coating is 12μm.
[0046] Example 3 A screen surface coating, the composition by weight is as follows: 40 parts of polymethyl methacrylate, 8 parts of fluorocarbon resin, 3.6 parts of silicon nitride, 0.5 parts of aluminum oxide, 0.02 parts of rare earth oxide, 0.03 parts of nanoparticles, 0.003 parts of carbon nanotubes, 0.03 parts of self-repairing microcapsules, 0.03 parts of ultraviolet absorbers, 0.06 parts of antioxidants, and 0.006 parts of antistatic agents.
[0047] Among them, the rare earth oxide is lanthanum oxide.
[0048] Among them, the nanoparticles are nano titanium dioxide.
[0049] The shell layer of the self-repairing microcapsule is urea-formaldehyde resin, and the core material is epoxy resin or polyurethane.
[0050] Among them, the ultraviolet absorber is 2-hydroxy-4-methoxybenzophenone.
[0051] Among them, butylated hydroxyanisole is selected as the antioxidant.
[0052] Among them, the antistatic agent is amide phosphate.
[0053] The carbon nanotubes are multi-walled carbon nanotubes with 50 layers and an average interlayer spacing of 0.34 nm.
[0054] The method for preparing the screen surface coating comprises the following steps: S1 Coating composition preparation: 1) dissolving polymethyl methacrylate and fluorocarbon resin in xylene solvent, pre-dispersing silicon nitride and aluminum oxide nanoparticles in toluene solvent, and then mixing and stirring the two; 2) Add rare earth oxides and carbon nanotubes and continue stirring to mix; 3) adding self-repairing microcapsules, ultraviolet absorbers, antioxidants and antistatic agents, stirring and mixing, and obtaining a coating composition for use; S2 Surface coating: 1) Pretreatment: Clean, degrease and dry the screen surface to ensure good bonding between the coating and the screen; 2) Coating: uniformly coating the composition obtained in step S1 on the surface of the screen; 3) Curing treatment: After the coating is applied, the surface coating is cured by ultraviolet light. The wavelength of the ultraviolet light source is 365nm, the light intensity is 60mW / cm², the curing time is 30min, and the thickness of the cured coating is 12μm.
[0055] Comparative Example 1 This embodiment does not contain nanoparticles and fluorocarbon resin, and the rest is the same as that in Embodiment 2.
[0056] Comparative Example 2 This embodiment does not contain rare earth oxide fluorocarbon resin, and the rest is the same as that in Embodiment 2.
[0057] Comparative Example 3 This embodiment does not contain nanoparticles, rare earth oxides and fluorocarbon resin, and the rest is the same as that in Embodiment 2.
[0058] Comparative Example 4 This embodiment does not contain microcapsule self-healing material, and the rest is the same as that in Embodiment 2.
[0059] Comparative Example 5 This embodiment does not contain multi-walled carbon nanotubes, and the rest is the same as that in Embodiment 2.
[0060] Comparative Example 6 This embodiment does not contain rare earth oxides, and the rest is the same as that in Embodiment 2.
[0061] The screens prepared in Examples 1-3 and Comparative Examples 1-4 were placed in a UV aging test box (model: QUV / SPRAY, manufacturer: Q-LAB) for UV aging test. The test conditions were: radiation intensity 0.98 W / m 2 , wavelength 340nm, blackboard temperature 58℃, test duration of each cycle 240h, and glossiness and color difference were rated. The specific test results are shown in Table 1 and Table 2 respectively.
[0062] Table 1 Gloss loss rate (%) Table 2 Color difference The screens prepared in Examples 1-3 and Comparative Examples 5-6 were placed in a temperature shock resistance test box (model: EW0470W, manufacturer: Guangwu Institute) for a temperature shock resistance test. The test conditions were: high temperature stage temperature 65°C, low temperature stage temperature -30°C, temperature change rate 1°C / m / n, exposure duration 1h, and the temperature change test was carried out 5 times in each cycle; steps (1) and (2) were repeated 3 times, a grid was scratched on the coating with a knife, and the peeling condition was observed to evaluate the powdering grade and adhesion grade. The specific results are shown in Tables 3 and 4, respectively.
[0063] Table 3 Powdering grade, grade Powdering is usually divided into the following levels: 1. No powdering: There is no obvious powdering on the coating surface, indicating that the coating is of good quality and strong durability.
[0064] 2. Slight powdering: Some particles or powder appear on the surface, but it is not obvious and does not affect the basic performance of the coating.
[0065] 3. Moderate powdering: Particles or powder appear on the surface and are relatively obvious, but the coating still has certain adhesion and corrosion resistance.
[0066] 4. Severe powdering: A large amount of particles or powdery substances appear on the surface, which obviously affects the basic properties of the coating, such as corrosion resistance and decreased adhesion.
[0067] 5. Failure: The surface particles or powder fall off seriously, causing the coating to lose its proper function. At this time, the coating needs to be re-coated or replaced.
[0068] Table 4 Adhesion, Grade Adhesion Grade Description: Grade 0: The cutting edge is completely smooth without any peeling. This means that the adhesion between the coating and the substrate is excellent, and the coating can be firmly attached to the substrate and is not easy to fall off.
[0069] Level 1: There is a small amount of paint film falling off at the intersection of the cuts, but the cross-cut area affected cannot be greater than 5%. This means that the adhesion between the coating and the substrate is very good, with only a small amount of film falling off at the intersection, which is suitable for occasions with extremely high requirements for coating adhesion.
[0070] Grade 2: There is paint film detachment at the cut edges and / or intersections, and the affected cut area is greater than 5% but less than 15%. This means that the adhesion between the coating and the substrate is still good, but there is detachment in some areas, which needs to be considered in specific applications.
[0071] Grade 3: The paint film has partially or completely fallen off in large pieces along the cut edges and / or partially or completely fallen off in different parts of the grid. The affected cut area is greater than 15% and less than 35%. This indicates that the adhesion between the coating and the substrate is moderate and further quality inspection and evaluation may be required.
[0072] Level 4: The paint film falls off in large pieces along the cut edges and / or partially or completely falls off in some grids. The affected cut area is greater than 35% and less than 65%. This indicates that the adhesion between the coating and the substrate is poor, and in-depth analysis and improvement of the coating process is required.
[0073] Level 5 (may not exist in some systems, but similar concept): Any degree of peeling exceeding Level 4. This indicates that the adhesion between the coating and the substrate is extremely poor, the coating can hardly adhere to the substrate, and the coating process and material selection need to be reconsidered.
[0074] In addition, it should be understood that although the present specification is described according to the implementation methods, not every implementation method contains only one independent claim scheme. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment can also be appropriately combined to form a technical solution that can be understood by those skilled in the art.
Claims
1. A screen surface coating, Features: The coating is composed of the following components by weight: 20-40 parts of polymethyl methacrylate, 3-8 parts of fluorocarbon resin, 1.2-3.6 parts of silicon nitride, 0.2-0.5 parts of aluminum oxide, 0.01-0.02 parts of rare earth oxide, 0.01-0.03 parts of nanoparticles, 0.001-0.003 parts of carbon nanotubes, 0.01-0.03 parts of self-repairing microcapsules, 0.02-0.03 parts of ultraviolet absorbers, 0.03-0.06 parts of antioxidants, and 0.003-0.006 parts of antistatic agents.
2. The screen surface coating according to claim 1, Features: The rare earth oxide is selected from one of cerium oxide and lanthanum oxide.
3. The screen surface coating according to claim 1, Features: The nanoparticles are selected from one of nano titanium dioxide and nano silicon dioxide.
4. The screen surface coating according to claim 1, Features: The shell layer of the self-repairing microcapsule is urea-formaldehyde resin, and the core material is epoxy resin or polyurethane.
5. The screen surface coating according to claim 1, Features: The ultraviolet absorber is selected from one of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2,4-dihydroxybenzophenone and 2-hydroxy-4-methoxybenzophenone.
6. The screen surface coating according to claim 1, Features: The antioxidant is selected from one of butylated hydroxytoluene and butylated hydroxyanisole.
7. The screen surface coating according to claim 1, Features: The antistatic agent is amide phosphate.
8. The screen surface coating according to claim 1, Features: The carbon nanotubes are multi-walled carbon nanotubes with 2-50 layers and an average interlayer spacing of 0.34±0.02nm.
9. A method for preparing a screen surface coating according to any one of claims 1 to 8, Features: The preparation method comprises the following steps: S1 Coating composition preparation: 1) dissolving polymethyl methacrylate and fluorocarbon resin in xylene solvent, pre-dispersing silicon nitride and aluminum oxide nanoparticles in toluene solvent, and then mixing and stirring the two; 2) Add rare earth oxides and carbon nanotubes and continue stirring to mix; 3) adding self-repairing microcapsules, ultraviolet absorbers, antioxidants and antistatic agents, stirring and mixing, and obtaining a coating composition for use; S2 Surface coating: 1) Pretreatment: Clean, degrease and dry the screen surface to ensure a good bond between the coating and the screen; 2) Coating: uniformly coating the composition obtained in step S1 on the surface of the screen; 3) Curing treatment: After the coating is applied, it is cured by ultraviolet light to obtain the surface coating.
Citation Information
Cited By
High-water-resistance coating for light-weight photovoltaic module and water-resistance light-weight module
CN120623892A
Coating structure for water conservancy project
CN120700835A