A method for treating NTA-heavy metal complexes in electroplating wastewater using Fe-C / PMS catalytic coupling chelate adsorption
Through Fe-C/PMS catalytic coupling chelation adsorption method, carbon-based single-atom iron catalyst is used to degrade NTA-heavy metal complexes, and adsorption is carried out through chelating resin, which solves the problem of NTA-heavy metal treatment in electroplating wastewater and achieves Efficient removal and recovery of heavy metal resources avoids waste of energy and oxidants.
Patent Information
- Application Number
- CN202410367677.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing technology is difficult to efficiently treat NTA-heavy metal complexes in electroplating wastewater. The traditional catalytic complex-breaking process consumes oxidants and energy, and the generated precipitated products are difficult to recycle. It is difficult to remove NTA-heavy metals using a separate chelation adsorption method.
The Fe-C/PMS catalytic coupling chelation adsorption method is used to generate non-radical singlet oxygen through a carbon-based single-atom iron catalyst and potassium persulfate, which degrades NTA to form an organic acid with low complexing capacity, and uses a chelating resin. Static adsorption achieves efficient removal of heavy metals.
It significantly improves the removal rate and degradation rate of NTA, saves oxidants and energy, achieves efficient recovery of heavy metals, and the catalyst and resin can be recycled, avoiding the generation of hazardous sludge waste.
Smart Images

Figure CN118388015B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electroplating wastewater treatment technology, and specifically relates to a method for treating NTA-heavy metal complexes in electroplating wastewater by utilizing Fe-C / PMS catalytic coupling chelating adsorption. Background Art
[0002] In recent years, with the continuous development of the electroplating industry, especially the rapid rise of township electroplating enterprises, the scope of electroplating wastewater pollution has continued to expand. Electroplating wastewater is considered one of the most difficult industrial wastewaters to treat. The most challenging component is heavy metals, especially complexed heavy metal ions. During the electroplating process, to improve the quality of the coating and enhance the stability of the plating solution, a large amount of chelating agents is added to form highly stable complexes with the heavy metals to prevent heavy metal precipitation at high pH values. Common chelating agents include ethylenediaminetetraacetic acid (EDTA), hydroxyethylidene diphosphonic acid (HEDP), citric acid (CA), tartaric acid (TA), and nitrilotriacetic acid (NTA). These additives can form extremely stable complexes with heavy metal ions, causing the heavy metals in the wastewater to also exist in a complexed state, making the wastewater difficult to treat using traditional methods such as chemical precipitation, biological methods, membrane separation, ion exchange, and adsorption. These traditional electroplating wastewater treatment technologies also suffer from long treatment cycles, low treatment efficiency, secondary pollution, and poor pollution resistance.
[0003] Currently, the combined catalytic decomposition and precipitation process is a new method for treating strongly complexed heavy metal systems in electroplating wastewater. Catalytic decomposition refers to the use of catalytic technology to destroy the structure of organic ligands, weaken their complexing ability for heavy metals, and then remove heavy metals through conventional technology. Common catalytic technologies include Fenton, electrochemical and photochemical catalysis. However, this process requires a large amount of oxidant or energy in the early decomposition process to completely mineralize the organic acid. Only when only free heavy metals remain in the solution can the precipitation method be effective in removing heavy metals, but the resulting precipitated products are difficult to recycle.
[0004] As we all know, EDTA is a widely used chelating agent, and the complexes it forms with typical heavy metals have high stability constants. A large number of studies have shown that EDTA can be degraded, but its degradation intermediates are complex and difficult to completely mineralize, resulting in the inability of subsequent precipitation methods to effectively remove heavy metals. When a catalytic coupled chelating adsorption process is used to treat strong EDTA-heavy metal complexes in electroplating wastewater, the catalytic degradation of EDTA can not only generate organic acids with low chelating ability, but also produce high chelating ability organic acids NTA that are difficult to remove. The degradation of EDTA will produce the product NTA, which is difficult to degrade by conventional catalytic means. For example, conventional free radicals such as hydroxyl radicals (·OH) and sulfate radicals (SO4·-) show very limited effectiveness in the degradation process of NTA. More importantly, NTA has extremely strong chelating ability. A large number of studies have shown that chelating adsorption alone is also difficult to remove heavy metals in NTA-heavy metal complexes, and the adsorption capacity is almost zero.
[0005] Therefore, in order to solve the above problems, it is urgent to provide an efficient and environmentally friendly method for treating NTA-heavy metal complexes. Summary of the Invention
[0006] In response to the above-mentioned problems existing in the prior art, the technical problem to be solved by the present invention is to provide a method for treating NTA-heavy metal complexes in electroplating wastewater using Fe-C / PMS catalytic coupled chelating adsorption. This method efficiently treats NTA-heavy metal complexes, which not only greatly saves oxidants and energy, but also can efficiently remove heavy metals, which is conducive to the efficient recycling of heavy metal resources.
[0007] In order to solve the above problems, the technical solutions adopted by the present invention are as follows:
[0008] A method for treating NTA-heavy metal complexes in electroplating wastewater by utilizing Fe-C / PMS catalytic coupled chelate adsorption comprises the following steps: firstly preparing a carbon-based single-atom iron catalyst, adding the carbon-based single-atom iron catalyst and PMS to the NTA-heavy metal complex, stirring, and after catalysis is completed, filtering, adjusting the pH, adding resin, and performing static adsorption. After adsorption is completed, the NTA-heavy metal complex is treated; wherein, the carbon-based single-atom iron catalyst is separated, washed, dried, and then recycled; and the resin is separated, desorbed, washed, dried, and then recycled.
[0009] Furthermore, the concentration of the carbon-based single-atom iron catalyst in the electroplating wastewater is 0.01 to 0.2 g / L.
[0010] Furthermore, the concentration of the PMS in the electroplating wastewater is 1 to 10 mM.
[0011] Furthermore, the pH is 2-9.
[0012] Furthermore, the dosage of the resin is 0.1-1 g / L.
[0013] Furthermore, the carbon-based single-atom iron catalyst and the resin are both circulated 1 to 4 times.
[0014] Furthermore, the heavy metals in the NTA-heavy metal complex are Ni, Cu, Zn and Cd.
[0015] Furthermore, the PMS is potassium persulfate.
[0016] Furthermore, the preparation method of the carbon-based single-atom iron catalyst is as follows: ammonia water, deionized water and ethanol are mixed, ethyl silicate is added dropwise, and the mixture is stirred to form a nano-silica ball dispersion; a pure dopamine solution and a dopamine solution containing FeCl3·6H2O are prepared, and the two solutions are alternately injected into the nano-silica ball dispersion, stirred and centrifuged, and the solid is collected, calcined, cooled to room temperature, taken out, and then poured into an ammonium bifluoride solution, stirred and centrifuged, the solid powder is collected, and washed and dried to obtain the carbon-based single-atom iron catalyst.
[0017] Further, the specific steps are as follows:
[0018] 1) Ammonia water, deionized water, and ethanol are mixed, and then ethyl silicate is added dropwise to the mixed solution, and the mixture is stirred at 30° C. for 25 minutes to form a nano-silica sphere dispersion; a pure dopamine solution and a dopamine solution containing FeCl3·6H2O are prepared, and the two solutions are alternately injected into the nano-silica sphere dispersion, stirred for 12 hours, and then centrifuged to collect solid powder; the solid powder is then placed in a tube furnace, and the temperature is raised to 800° C. at 2° C. / min under nitrogen protection, and retained for 5 hours. After calcination, the solid powder is taken out after cooling to room temperature, poured into an ammonium bifluoride solution, stirred for 12 hours, and then centrifuged to collect the solid powder, washed continuously with deionized water, and then dried at 70° C. to obtain a carbon-based single-atom iron catalyst;
[0019] 2) Mix deionized water and NTA evenly to prepare an NTA stock solution; mix deionized water with NiCl2, CuCl2, ZnCl2, and CdCl2 respectively to prepare a heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare an NTA-heavy metal solution;
[0020] 3) adding the carbon-based single-atom iron catalyst and PMS prepared in step 1) to the NTA-heavy metal solution prepared in step 2), performing magnetic stirring, and after the catalysis is completed, filtering to obtain a clear liquid;
[0021] 4) Sodium hydroxide solution and hydrochloric acid solution were added to the clear solution obtained after the catalysis in step 3) to adjust the pH, and then resin was added. After static adsorption on a shaker for 24 hours, the adsorption was completed and the NTA-heavy metal complex treatment was completed.
[0022] Beneficial effects: Compared with the prior art, the advantages of the present invention are:
[0023] (1) The present invention uses a carbon-based single-atom Fe as a catalyst, and the non-radical singlet oxygen ( 1 O2), greatly improving the removal rate and degradation rate of NTA, and more than 95% of NTA can be degraded within 30 minutes, which is significantly better than other common Fenton and Fenton-like catalytic technologies, laying an excellent foundation for the subsequent removal of heavy metals.
[0024] (2) The present invention takes "mild complex breaking" as its core, and catalytically degrades NTA with high complexing ability, converting it into organic acid with low complexing ability, forming a low complexing system with heavy metals, and then using chelating adsorption resin based on chelation to efficiently capture heavy metal ions in water, thereby achieving the purification of heavy metal ions in water. Its total organic carbon removal rate is only about 23%, and the subsequent heavy metal ion removal rate is as high as more than 90%. Therefore, compared with the traditional "deep complex breaking" strategy, this method does not require a large amount of energy and reagents to completely mineralize NTA (i.e., organic carbon removal rate>80% or more) and heavy metals can be removed only after all heavy metals are in a free state, which can greatly save oxidants and energy.
[0025] (3) After heavy metals are adsorbed and enriched on the resin, they can be desorbed by acid washing to obtain high-concentration heavy metal resources. Compared with traditional catalytic-precipitation treatment, this method integrates catalysis and chelating adsorption, does not produce sludge hazardous waste, and has high heavy metal recovery purity, high concentration ratio, and significant recovery value.
[0026] (4) The carbon-based single-atom iron catalyst / persulfate catalytic system of the present invention has low usage, and the catalyst and resin can be recycled, with high efficiency, low consumption, no secondary pollution, and resource recovery to improve economic benefits.
[0027] (5) The method of treating NTA-heavy metal complexes of the present invention has a wide range of applications and has a good removal effect on different types of NTA-heavy metals, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The effect of different Fe-C dosages on the degradation of NTA by the Fe-C / PMS system of the present invention;
[0029] Figure 2The effect of different PMS dosages on the degradation of NTA by the Fe-C / PMS system of the present invention is shown;
[0030] Figure 3 The effect of different pH values on the adsorption method (Ni removal) after catalysis by the Fe-C / PMS system of the present invention;
[0031] Figure 4 The effect of different dosages of resin catalyzed by the Fe-C / PMS system on the adsorption method (Ni removal) of the present invention is shown;
[0032] Figure 5 The effect of the recycling of Fe-C on the NTA removal rate of the present invention;
[0033] Figure 6 The effect of recycling of the resin of the present invention on Ni removal rate;
[0034] Figure 7 The removal effect of the Fe-C / PMS system of the present invention on different NTA-heavy metals;
[0035] Figure 8 The results of NTA degradation using different catalytic systems are shown;
[0036] Figure 9 The results of EDTA degradation using different catalytic systems are shown in the figure;
[0037] Figure 10 The figure shows the TOC removal efficiency results of EDTA-Ni and NTA-Ni systems using different catalytic systems;
[0038] Figure 11 This is a diagram showing the treatment results of Ni in the catalytic solution using precipitation and adsorption methods. DETAILED DESCRIPTION
[0039] The present invention will be further described below with reference to specific embodiments.
[0040] The resin used in the following examples is aminoacetic acid type chelating resin D463.
[0041] The specific test method of the high performance liquid chromatography used in the following examples to determine the concentration of NTA and EDTA is as follows: FeCl3 solution is added to the liquid to be tested so that Fe 3+ :NTA (or EDTA) = 1.5:1, and the determination was performed using a high performance liquid chromatography. The conditions for high performance liquid chromatography were: the mobile phase was a mixed solution of 10% acetonitrile and 90% buffered saline solution (1 mM tetrabutylammonium bromide, 5 mM sodium formate and 15 mM formic acid), and the detection wavelength was 258 nm.
[0042] The specific test method of the flame atomic absorption spectrophotometer used in the following examples for determining the concentration of heavy metals is as follows: the liquid to be tested is diluted 50 times, and a 10% dilute nitric acid solution is added to the diluted solution (the volume ratio of the solution to the 10% dilute nitric acid is 50:1), and the heavy metals are determined using a flame atomic absorption spectrometer.
[0043] The specific testing method of the total organic carbon analyzer used in the following examples for determining TOC concentration is as follows: the liquid to be tested is diluted 10 times, 0.1 mL of 2M hydrochloric acid solution is added, and the TOC of the solution is measured using a total organic carbon analyzer (Shimadzu, Japan).
[0044] Example 1
[0045] 1. Preparation of carbon-based single-atom iron catalyst (Fe-C)
[0046] (1) 5 mL of ammonia water, 20 mL of deionized water, and 100 mL of ethanol were mixed, and then 5 mL of ethyl silicate was added dropwise to the mixed solution. The mixture was stirred at 30°C for 25 min to form a nanosilica sphere dispersion.
[0047] (2) Prepare pure dopamine solution (5 mg / L, 160 mL) and dopamine solution containing FeCl3·6H2O (5 mg / L, 160 mL, FeCl3·6H2O dosage is 0.046 g) respectively. Alternately inject 40 mL of pure dopamine solution and dopamine solution containing FeCl3·6H2O into the nano-silica dispersion prepared in step 1) at an injection interval of 5 minutes. Stir continuously for 12 hours and then centrifuge at 10,000 rpm for 8 minutes to collect the solid powder, which is the nano-silica sphere with a polymerized dopamine shell with an Fe source.
[0048] (3) The nano-silica spheres obtained in step 2) were placed in a tube furnace, heated to 800°C at 2°C / min under N2 protection, and then retained for 5 hours. The mixture was cooled to room temperature and then taken out. The obtained black powder was poured into 250 mL of 1 mol / L ammonium bifluoride solution, stirred for 12 hours, and then centrifuged at 10,000 r / min for 8 minutes. The powder was collected and continuously washed with deionized water until the pH was close to neutral, and then dried at 70°C overnight to obtain a carbon-based single-atom iron catalyst.
[0049] 2. Treatment of NTA-Ni by Fe-C / PMS catalytic coupled chelate adsorption (the mass concentrations of Fe-C were 0.01 g / L, 0.03 g / L, 0.06 g / L, 0.08 g / L and 0.1 g / L, the molar concentration of PMS was 4 mM, the pH was 6, and the resin input was 0.6 g / L)
[0050] (1) Mix deionized water and NTA evenly to prepare a 5 mM NTA stock solution; mix deionized water with NiCl2 to prepare a 5 mM heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare a 1 mM NTA-Ni solution.
[0051] (2) The carbon-based single-atom iron catalyst (mass concentration of 0.01 g / L, 0.03 g / L, 0.06 g / L, 0.08 g / L and 0.1 g / L) and PMS (molar concentration of 4 mM) prepared above were added to the NTA-Ni solution prepared in step (1), and then magnetically stirred for 30 minutes. 1 mL of sample was taken at set reaction times of 0, 1, 5, 10, 20 and 30 minutes, and 0.5 mL of methanol was immediately added to terminate the reaction. The sample was filtered using a filter head with a pore size of 0.22 μm to obtain the filtrate as the sample to be tested. The concentration of NTA in the sample was determined by high performance liquid chromatography. The results are as follows: Figure 1 The NTA-heavy metal solution after the reaction is terminated is filtered to obtain a clear solution (the solution used for subsequent adsorption).
[0052] (3) Sodium hydroxide solution and hydrochloric acid solution were added to the clear solution obtained after the catalysis in step (2) to adjust the pH to 6, and then resin (input amount was 0.6 g / L) was added. After the solution was placed on a shaker for static adsorption for 24 hours, the adsorption was completed and the NTA-Ni solution was treated. 1 mL of the treated NTA-Ni solution was taken and filtered using a filter head with a pore size of 0.22 μm. The filtrate was the sample to be tested, and the Ni concentration in the sample was determined by flame atomic absorption spectrophotometry.
[0053] Figure 1 The figure shows the effect of different Fe-C dosages on NTA degradation in the Fe-C / PMS system of the present invention. As shown in the figure, in the Fe-C / PMS catalytic system, the NTA removal rate continues to improve with increasing Fe-C dosage. When the Fe-C dosage is greater than or equal to 0.06 g / L, the NTA removal rate after 30 minutes of reaction is comparable. Increasing the Fe-C dosage only increases wastewater treatment costs.
[0054] Example 2
[0055] Treatment of NTA-Ni by Fe-C / PMS catalytic coupled chelate adsorption (Fe-C concentration of 0.06 g / L, PMS molar concentrations of 0 mM, 1 mM, 2 mM, 4 mM, and 5 mM, pH 6, resin input of 0.6 g / L)
[0056] (1) Mix deionized water and NTA evenly to prepare a 5 mM NTA stock solution; mix deionized water and NiCl2 to prepare a 5 mM heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare a 1 mM NTA-Ni solution.
[0057] (2) The carbon-based single-atom iron catalyst (mass concentration of 0.06 g / L) and PMS (molar concentrations of 0 mM, 1 mM, 2 mM, 4 mM and 5 mM, respectively) prepared in Example 1 were added to the NTA-Ni solution prepared in step (1), and then magnetically stirred for 30 min. 1 mL of sample was taken at set reaction times of 0, 1, 5, 10, 20 and 30 min, and 0.5 mL of methanol was immediately added to terminate the reaction. The sample was filtered using a filter head with a pore size of 0.22 μm to obtain the filtrate as the sample to be tested. The concentration of NTA in the sample was determined by high performance liquid chromatography. The results are shown in FIG. Figure 2 The NTA-Ni solution after the reaction was terminated was filtered to obtain a clear solution (the solution used for subsequent adsorption).
[0058] (3) Sodium hydroxide solution and hydrochloric acid solution were added to the clear solution obtained after the catalysis in step (2) to adjust the pH to 6, and then resin (input amount was 0.6 g / L) was added. After the solution was placed on a shaker for static adsorption for 24 hours, the adsorption was completed and the NTA-Ni solution was treated. 1 mL of the treated NTA-Ni solution was taken and filtered using a filter head with a pore size of 0.22 μm. The filtrate was the sample to be tested, and the Ni concentration in the sample was determined by flame atomic absorption spectrophotometry.
[0059] Figure 2 The figure shows the effect of different PMS dosages on NTA degradation in the Fe-C / PMS system of the present invention. As can be seen from the figure, in the Fe-C / PMS catalytic system, the higher the PMS dosage, the more significant the improvement in NTA removal efficiency. Increasing the PMS dosage from 0 mM to 4 mM increases the NTA removal efficiency from 6% to 90%. However, further increasing the PMS dosage to 5 mM limits the improvement in reaction efficiency, and further increasing the PMS dosage will only increase wastewater treatment costs.
[0060] Example 3
[0061] Treatment of NTA-Ni by Fe-C / PMS catalytic coupled chelate adsorption (Fe-C mass concentration of 0.06 g / L, PMS molar concentration of 4 mM, pH of 3, 4, 5, 6, 7 and 8, resin input of 0.6 g / L)
[0062] (1) Mix deionized water and NTA evenly to prepare a 5 mM NTA stock solution; mix deionized water with NiCl2 to prepare a 5 mM heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare a 1 mM NTA-Ni solution.
[0063] (2) The carbon-based single-atom iron catalyst and PMS (molar concentration of 4 mM) prepared in Example 1 were added to the NTA-Ni solution prepared in step (1), and then magnetically stirred for 30 minutes. The NTA-Ni solution after the reaction was terminated was then filtered to obtain a clear solution.
[0064] (3) Sodium hydroxide solution and hydrochloric acid solution were added to the clear solution obtained after the catalysis in step (2) to adjust the pH to 3, 4, 5, 6, 7 and 8 respectively, and then resin was added and placed on a shaker for static adsorption for 24 hours. After the adsorption was completed, the NTA-Ni solution was treated. 1 mL of the treated NTA-Ni solution was taken and filtered using a filter head with a pore size of 0.22 μm. The filtrate was the sample to be tested, and the Ni concentration in the sample was determined by flame atomic absorption spectrophotometry. The results are as follows: Figure 3 shown.
[0065] Figure 3 The figure shows the effect of different pH values on the adsorption method (Ni removal) after catalysis by the Fe-C / PMS system. As shown in the figure, after catalysis by the Fe-C / PMS system, when the solution pH is 3 to 6 before adsorption, the Ni removal rate continues to increase with the increase of pH. When the pH is 6, the Ni removal rate of the chelating resin D463 reaches the highest, and can remove 90% by adsorption. As the pH continues to rise, the Ni removal rate will decrease. Therefore, the optimal solution pH before adsorption is 6.
[0066] Example 4
[0067] Treatment of NTA-Ni by Fe-C / PMS catalytic coupled chelate adsorption (Fe-C mass concentration of 0.06 g / L, PMS molar concentration of 4 mM, pH 6, resin input amounts of 0.4 g / L, 0.5 g / L, 0.6 g / L, 0.7 g / L, and 0.8 g / L, respectively)
[0068] (1) Mix deionized water and NTA evenly to prepare a 5 mM NTA stock solution; mix deionized water with NiCl2 to prepare a 5 mM heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare a 1 mM NTA-Ni solution.
[0069] (2) The carbon-based single-atom iron catalyst (mass concentration of 0.06 g / L) and PMS (molar concentration of 4 mM) prepared in Example 1 were added to the NTA-Ni solution prepared in step (1), followed by magnetic stirring for 30 minutes. The terminated NTA-Ni solution was filtered to obtain a clear solution.
[0070] (3) After the catalysis in step (2) is completed, sodium hydroxide solution and hydrochloric acid solution are added to the clear solution to adjust the pH to 6, and then resin is added (the input amount is 0.4g / L, 0.5g / L, 0.6g / L, 0.7g / L and 0.8g / L respectively). After being placed in a shaker for static adsorption for 24 hours, the adsorption is completed and the NTA-Ni solution is treated. Take 1mL of the treated NTA-Ni solution and filter it with a filter head with a pore size of 0.22μm. The filtrate is the sample to be tested, and the concentration of heavy metals in the sample is determined by flame atomic absorption spectrophotometry. The results are as follows Figure 4 shown.
[0071] Figure 4 The figure shows the effect of different resin dosages on the adsorption method (Ni removal) after Fe-C / PMS catalysis. As can be seen from the figure, after Fe-C / PMS catalysis, the higher the resin dosage before adsorption, the higher the Ni removal rate. When the resin D463 dosage is increased from 0.4g / L to 0.6g / L, the Ni removal rate can be increased from 70% to 90%. However, further increasing the resin dosage to 0.7g / L and 0.8g / L shows limited improvement in removal efficiency. Further increasing the resin dosage will only increase wastewater treatment costs.
[0072] Example 5
[0073] Fe-C cycle life test
[0074] The Fe-C prepared in Example 1, when treating NTA-heavy metal complexes, when Fe-C is added to NTA-Ni solution and reacted for 30 minutes, it is immediately separated using a suction filtration device and washed and dried with water to obtain Fe-C after one cycle; the Fe-C after one cycle is reacted for 30 minutes in a new round of pollutant removal experiments, and then immediately separated and washed and dried to obtain Fe-C after two cycles; this cycle can obtain Fe-C after three cycles; the Fe-C after the third cycle is re-calcined (placed in a tubular furnace, raised to 800°C at 2°C / min under N2 protection and retained for 5 hours), and then repeated for the fourth cycle to obtain Fe-C after four cycles. The results are as follows Figure 5 shown.
[0075] Figure 5The figure shows the effect of the recycling of Fe-C on the NTA removal rate of the present invention. As can be seen from the figure, the Fe-C / PMS system of the present invention has good recycling performance. Even after three cycles, the NTA removal rate can still reach 72% or above within 30 minutes. Before the fourth cycle, the Fe-C is re-calcined, and the performance of the Fe-C is greatly restored.
[0076] Example 6
[0077] Cyclic service life test of chelating resin D463
[0078] According to the method in the embodiment of the present invention, after the resin has been adsorbed for 24 hours, it is immediately separated and desorbed in a 0.1 mol / L HCl solution for 12 hours, and then washed with water and dried to obtain a resin for one cycle; after the resin has been adsorbed for 24 hours in a new round of Fe-C / PMS catalyzed solution, it is immediately separated and desorbed for 12 hours, and then washed with water and dried to obtain a resin for two cycles; and this cycle is repeated to obtain a resin that has been used three or four times. The results are shown in FIG. Figure 6 shown.
[0079] Figure 6 The figure shows the effect of recycling of the resin of the present invention on the Ni removal rate. As can be seen from the figure, the resin D463 of the present invention has good recycling performance. Even after four cycles, the Ni removal rate can still reach 89% or more, and the Ni recovery rate reaches 95% or more, realizing efficient recovery of Ni resources.
[0080] Example 7
[0081] Treatment of NTA-Cu / Zn / Cd using Fe-C / PMS catalytic coupled chelate adsorption (Fe-C mass concentration of 0.06 g / L, PMS molar concentration of 4 mM, pH 6, resin input amount of 0.6 g / L)
[0082] (1) Mix deionized water and NTA evenly to prepare a 5 mM NTA stock solution; take deionized water and mix it with CuCl2, ZnCl2 and CdCl2 respectively to prepare a 5 mM heavy metal stock solution; mix the NTA stock solution with the heavy metal stock solution to prepare a 1 mM NTA-heavy metal solution.
[0083] (2) The carbon-based single-atom iron catalyst (mass concentration of 0.06 g / L) and PMS (molar concentration of 4 mM) prepared above were added to the NTA-heavy metal solution prepared in step (1), and then magnetically stirred for 30 minutes. 1 mL of sample was taken at set reaction times of 0, 1, 5, 10, 20, and 30 minutes, and 0.5 mL of methanol was immediately added to terminate the reaction. The sample was filtered using a filter head with a pore size of 0.22 μm to obtain the filtrate as the test sample. The concentration of NTA in the sample was determined by high performance liquid chromatography. The results are as follows: Figure 7 The NTA-heavy metal solution after the reaction is terminated is filtered to obtain a clear solution (the solution used for subsequent adsorption).
[0084] (3) Sodium hydroxide solution and hydrochloric acid solution were added to the clear solution obtained after the catalysis in step (2) to adjust the pH to 6, and then resin (input amount was 0.6 g / L) was added. After static adsorption on a shaker for 24 hours, the adsorption was completed and the NTA-heavy metal solution was treated. 1 mL of the treated NTA-heavy metal solution was taken and filtered using a filter with a pore size of 0.22 μm. The filtrate was the sample to be tested, and the concentration of heavy metals in the sample was determined by flame atomic absorption spectrophotometry.
[0085] Figure 7 The figure shows the removal effect of the Fe-C / PMS system of the present invention on different NTA-heavy metals. As can be seen from the figure, the Fe-C / PMS system shows high removal effectiveness in various NTA-heavy metal cases, indicating that the process has good broad-spectrum properties for treating NTA-heavy metal complexes.
[0086] Comparative Example 1
[0087] Treatment of EDTA-Ni by Fe-C / PMS catalytic coupled chelate adsorption (Fe-C mass concentration 0.06 g / L, PMS molar concentration 4 mM, pH 6, resin input 0.6 g / L)
[0088] (1) Mix deionized water and EDTA evenly to prepare a 5 mM EDTA stock solution; mix deionized water with NiCl2 to prepare a 5 mM heavy metal stock solution; mix the EDTA stock solution with the heavy metal stock solution to prepare a 1 mM EDTA-Ni solution.
[0089] (2) The carbon-based single-atom iron catalyst (mass concentration of 0.06 g / L) and PMS (molar concentration of 4 mM) prepared in Example 1 were added to the EDTA-Ni solution prepared in step (1), and then magnetically stirred for 30 min. 1 mL of the solution was sampled at set reaction times of 0, 1, 5, 10, 20, and 30 min, respectively. 0.5 mL of methanol was immediately added after sampling to terminate the reaction. The solution was filtered through a filter head with a pore size of 0.22 μm to obtain the filtrate as the sample to be tested. The concentration of EDTA in the sample was determined by high performance liquid chromatography. The results are as follows: Figure 9 The EDTA-Ni solution after the reaction was terminated was filtered to obtain a clear solution.
[0090] (3) In step (2), 1 mL of sample was taken at 0 and 30 min after the catalytic reaction, filtered using a filter with a pore size of 0.22 μm, diluted 10 times, and 0.1 mL of 2 M hydrochloric acid solution was added. The TOC of the solution was measured using a TOC analyzer (Shimadzu, Japan). The results are as follows: Figure 10 shown.
[0091] (4) After the catalysis in step (2) is completed, sodium hydroxide solution and hydrochloric acid solution are added to the clear solution to adjust the pH to 6, and then resin (input amount is 0.6 g / L) is added. After the solution is placed on a shaker for static adsorption for 24 hours, the adsorption is completed and the EDTA-Ni solution is treated. Take 1 mL of the treated EDTA-Ni solution and filter it with a filter head with a pore size of 0.22 μm. The filtrate is the sample to be tested. The concentration of Ni in the sample is determined by flame atomic absorption spectrophotometry. The results are as follows: Figure 11 shown.
[0092] Comparative Example 2
[0093] Adding different catalytic systems (B / Fe 2+ / H2O2、B / Fe 2+ / PMS and B / Fe 2+ / PAA) degrades NTA
[0094] (1) Boron (B), ferrous sulfate (FeSO4), hydrogen peroxide (H2O2), potassium persulfate (PMS) and peracetic acid (PAA) were added to the NTA-Ni solution prepared in Examples 1 to 4, respectively, and the mass concentration of B in the catalytic process was controlled to be 0.1 g / L, and the mass concentration of FeSO4 was controlled to be 0.1 g / L. 2+The molar concentration of 0.5mM, the molar concentration of H2O2 was 20mM, and the molar concentrations of PMS and PAA were 5mM. Magnetic stirring was then performed for 30 minutes. 1 mL of samples were taken at set reaction times of 0, 1, 5, 10, 20, and 30 minutes. 0.5 mL of methanol was immediately added to terminate the reaction. The sample was filtered through a filter head with a pore size of 0.22 μm. The filtrate was used as the test sample. The concentration of NTA in the sample was determined by high performance liquid chromatography. The results are shown in Figure 2. Figure 8 The NTA-Ni solution after the reaction was terminated was filtered to obtain a clear solution.
[0095] (2) In step (1), 1 mL of sample was taken at 0 and 30 min after the catalytic reaction, filtered using a filter with a pore size of 0.22 μm, diluted 10 times, and 0.1 mL of 2 M hydrochloric acid solution was added. The TOC of the solution was measured using a TOC analyzer (Shimadzu, Japan). The results are as follows: Figure 10 shown.
[0096] (3) After the catalysis in step (1) is completed, sodium hydroxide solution and hydrochloric acid solution are added to the clear solution to adjust the pH to 6, and then resin (input amount is 0.6 g / L) is added. After the solution is placed on a shaker for static adsorption for 24 hours, the adsorption is completed and the NTA-Ni solution is treated. Take 1 mL of the treated NTA-Ni solution and filter it with a filter head with a pore size of 0.22 μm. The filtrate is the sample to be tested. The concentration of heavy metal Ni in the sample is determined by flame atomic absorption spectrophotometry. The results are as follows: Figure 11 shown.
[0097] Figure 8 The results of NTA degradation using different catalytic systems are shown in the figure. It can be seen that Fe-C / PMS, B / Fe 2+ / H2O2、B / Fe 2 + / PMS and B / Fe 2+ The NTA removal rates of the Fe-C / PMS system in the present invention after 30 min of reaction were 96.5%, 41.2%, 10.8% and 10.6%. The removal effect of the other three processes on NTA was not ideal.
[0098] Comparative Example 3
[0099] Adding different catalytic systems (B / Fe 2+ / H2O2、B / Fe 2+ / PMS and B / Fe 2+ / PAA) degrades EDTA
[0100] (1) Boron (B), ferrous sulfate (FeSO4), hydrogen peroxide (H2O2), potassium persulfate (PMS) and peracetic acid (PAA) were added to the EDTA-Ni solution prepared in the comparative example 1, respectively, and the mass concentration of B in the catalytic process was controlled to be 0.1 g / L, and the mass concentration of FeSO4 was controlled to be 0.1 g / L. 2+ The molar concentration of 0.5mM, the molar concentration of H2O2 was 20mM, and the molar concentrations of PMS and PAA were 5mM. Magnetic stirring was then performed for 30 minutes. 1 mL of samples were taken at set reaction times of 0, 1, 5, 10, 20, and 30 minutes. Immediately after sampling, 0.5 mL of methanol was added to terminate the reaction. The sample was filtered through a filter head with a pore size of 0.22 μm. The filtrate was used as the test sample. The concentration of EDTA in the sample was determined by high performance liquid chromatography. The results are shown in Figure 2. Figure 9 The EDTA-Ni solution after the reaction was terminated was filtered to obtain a clear solution.
[0101] (2) In step (1), 1 mL of sample was taken at 0 and 30 min after the catalytic reaction, filtered using a filter with a pore size of 0.22 μm, diluted 10 times with deionized water, and 0.1 mL of 2 M hydrochloric acid solution was added. The TOC of the solution was measured using a TOC analyzer (Shimadzu, Japan). The results are as follows: Figure 10 shown.
[0102] (3) After the catalysis in step (1) is completed, sodium hydroxide solution and hydrochloric acid solution are added to the clear solution to adjust the pH to 6, and then resin (input amount is 0.6 g / L) is added. After the solution is placed on a shaker for static adsorption for 24 hours, the adsorption is completed and the EDTA-Ni solution is treated. Take 1 mL of the treated EDTA-Ni solution and filter it with a filter head with a pore size of 0.22 μm. The filtrate is the sample to be tested. The concentration of heavy metal Ni in the sample is determined by flame atomic absorption spectrophotometry. The results are as follows: Figure 11 shown.
[0103] Comparative Example 4
[0104] Precipitation method for removing heavy metals
[0105] After the Fe-C / PMS catalysis in Examples 1 to 4 of the present invention, sodium hydroxide solution was added to the NTA-Ni solution or EDTA-Ni solution to adjust the pH to 9.5-10. After standing for 3 hours, the solution was filtered using a filter with a pore size of 0.22 μm to obtain the sample to be tested. Figure 11 shown.
[0106] Figure 9 The results of EDTA degradation using different catalytic systems are shown in the figure. It can be seen that Fe-C / PMS, B / Fe 2+ / H2O2、B / Fe 2 + / PMS and B / Fe 2+ / PAA process has a significant removal effect on EDTA, and the EDTA removal rate can reach more than 95.5% within 30 minutes of reaction.
[0107] Figure 10 The results of the TOC removal efficiency in EDTA-Ni and NTA-Ni systems using different catalytic systems are shown in the figure. It can be seen that Fe-C / PMS, B / Fe 2+ / H2O2、B / Fe 2+ / PMS and B / Fe 2+ The Fe-C / PMS process achieved TOC removal efficiencies of 22.4%, 11.4%, 2.8%, and 2.5% for the NTA-Ni system, respectively, and 14.3%, 13.6%, 15.1%, and 16.6% for the EDTA-Ni system, respectively. While all four processes completely degraded EDTA, the TOC removal rates were very low, indicating only slight EDTA decomposition. Only the Fe-C / PMS process demonstrated significant NTA removal, achieving a TOC removal rate of only 22.4%, achieving only slight decomposition.
[0108] Figure 11 The figure shows the results of nickel removal in the catalytic solution using precipitation and adsorption methods. The figure shows that after NTA degradation, the chelating adsorption resin D463 achieved nickel removal efficiencies of 92.3%, 54.7%, 16.6%, and 17.5% using the Fe-C / PMS, B / Fe2+ / H2O2, B / Fe2+ / PMS, and B / Fe2+ / PAA processes, while the precipitation method achieved nickel removal efficiencies of 52.7%, 21.3%, 8.5%, and 9.1%. After EDTA degradation, the chelating adsorption resin D463 achieved nickel removal efficiencies of 17.9%, 73.6%, 69.2%, and 70.8%, while the precipitation method achieved nickel removal efficiencies of 10.5%, 22.3%, 33.7%, and 36.1%. Observing the treatment results of the four processes for the two systems, it was found that the chelating adsorption method consistently outperformed the precipitation method in nickel removal.
[0109] Combine Figure 8 、 9 , 10 and 11, we can see that C / PMS, B / Fe 2+ / H2O2、B / Fe 2+ / PMS and B / Fe 2+The four processes, C / PMS, PAA, and C / PMS, all showed significant EDTA removal effects when treating EDTA-Ni. However, the C / PMS process was significantly less effective than the other three processes in the subsequent application of chelating resin to remove Ni. However, in the NTA-Ni system, the C / PMS process showed significant NTA removal, and the subsequent application of chelating resin also showed significant Ni removal effects, demonstrating the unique and significant performance of the C / PMS process in treating NTA-heavy metal complexes.
Claims
1. A method for treating NTA-heavy metal complexes in electroplating wastewater using Fe-C / PMS catalytic coupled chelating adsorption, characterized in that: First, a carbon-based single-atom iron catalyst is prepared, and the carbon-based single-atom iron catalyst and PMS are added to an NTA-heavy metal complex, stirred, and after the catalysis is completed, suction filtration is performed, the pH value is adjusted, and a resin is added for static adsorption. After the adsorption is completed, the NTA-heavy metal complex is treated; wherein, the carbon-based single-atom iron catalyst is separated, washed, dried, and then recycled; the resin is separated, desorbed, washed, dried, and then recycled; the preparation method of the carbon-based single-atom iron catalyst is as follows: ammonia water, deionized water, and ethanol are mixed, and then ethyl silicate is added dropwise, stirred, and a nano-silica ball dispersion is formed; a pure dopamine solution and a dopamine solution containing FeCl3·6H2O are prepared, and they are alternately injected into the nano-silica ball dispersion, stirred, centrifuged, and then the solid is collected, calcined, cooled to room temperature, and then taken out, and then poured into an ammonium bifluoride solution, stirred, centrifuged, and solid powder is collected, washed, and dried to obtain the carbon-based single-atom iron catalyst; the NTA is aminotriacetic acid.
2. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The concentration of the carbon-based single-atom iron catalyst in electroplating wastewater is 0.01-0.2 g / L.
3. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The concentration of the PMS in the electroplating wastewater is 1-10 mM.
4. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The pH is 2-9.
5. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The dosage of the resin is 0.1-1 g / L.
6. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The carbon-based single-atom iron catalyst and the resin are circulated for 1 to 4 times.
7. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The heavy metals in the NTA-heavy metal complex are Ni, Cu, Zn and Cd.
8. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The PMS is potassium persulfate.
9. The method for treating NTA-heavy metal complexes in electroplating wastewater by using Fe-C / PMS catalytic coupling chelating adsorption according to claim 1, characterized in that: The specific steps are as follows: 1) Ammonia water, deionized water and ethanol are mixed, and then ethyl silicate is added dropwise to the mixed solution, and the mixture is stirred continuously for 25 minutes at 30°C to form a nano-silica ball dispersion; a pure dopamine solution and a dopamine solution containing FeCl3·6H2O are prepared, and they are alternately injected into the nano-silica ball dispersion, respectively, and the solid powder is collected by centrifugation after continuous stirring for 12 hours; the solid powder is then placed in a tubular furnace, and the temperature is raised to 800°C at 2°C / min under N2 protection, and retained for 5 hours. After calcination, the solid powder is taken out after cooling to room temperature, and the solid powder is poured into an ammonium bifluoride solution, stirred for 12 hours, and then centrifuged, and the solid powder is collected, and continuously washed with deionized water, and then dried at 70°C to obtain a carbon-based single-atom iron catalyst; 2) Mix deionized water and NTA evenly to prepare NTA stock solution; mix deionized water with NiCl2, CuCl2, ZnCl2 and CdCl2 respectively to prepare heavy metal stock solution; mix NTA stock solution with heavy metal stock solution to prepare NTA-heavy metal solution; 3) adding the carbon-based single-atom iron catalyst and PMS prepared in step 1) into the NTA-heavy metal solution prepared in step 2), performing magnetic stirring, and after the catalysis is completed, filtering to obtain a clear solution; 4) After the catalysis in step 3), sodium hydroxide solution and hydrochloric acid solution are added to the clear solution to adjust the pH, and then resin is added and placed on a shaker for static adsorption for 24 hours. After that, the adsorption is completed and the NTA-heavy metal complex treatment is completed.
Citation Information
Patent Citations
Method for synchronous complex breaking and heavy metal removal based on self-strengthening ozone
CN105502739A
Treatment method of copper complex wastewater
CN110342628A
Biomagnetic microsphere, and preparation method and use method thereof
CN112111042A
Preparation and application of low-temperature-resistant nitrogen self-doped hollow carbon sphere supported iron catalyst
CN115337948A
Single-atom catalyst for activation of persulfate to generate pure singlet oxygen as well as preparation method and application thereof
US20220315425A1
Cited By
Method for removing heavy metal complex in wastewater
CN119841432A
A method for removing heavy metal complexes from wastewater
CN119841432B