A method for reducing cover plate adhesion in DCB sintering fixture
By spraying a mixture of magnesium oxide and ethyl orthosilicate on the surface of the alumina ceramic plate and generating a magnesium silicate sintered layer at high temperature, the problem of adhesion between the cover plate and the product in the DCB sintering fixture is solved, and the scrap rate and production are reduced. cost effect.
Patent Information
- Application Number
- CN202410851754.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-28
AI Technical Summary
During the DCB sintering process, the alumina cover plate and the copper sheet of the DCB product are prone to adhesion at high temperatures, resulting in product scrap and increased production costs.
By uniformly mixing magnesium oxide and ethyl orthosilicate in the dispersant of absolute ethanol, spraying it on the surface of the alumina ceramic plate, and generating a magnesium silicate sintered layer under high temperature conditions to coat the alumina ceramic plate and insulate the cover plate. Contact with copper in DCB products.
Form a stable and dense magnesium silicate sintered layer to prevent the alumina cover plate from adhering to the copper in DCB products, reducing product scrap rate and production costs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of DCB sintering jigs, and in particular to a method for reducing adhesion of a cover plate in a DCB sintering jig. Background Art
[0002] DCB technology uses copper's oxygen-containing eutectic liquid to directly bond copper to ceramics. The basic principle is to introduce an appropriate amount of oxygen between copper and ceramic (aluminum oxide) before or during the bonding process. Within a certain temperature range, copper and oxygen form a Cu-O eutectic liquid, which infiltrates the copper foil to achieve the bonding of the ceramic substrate and the copper plate.
[0003] In the current industry, during the sintering production process of copper-clad ceramic substrates (DCB), since the products cannot be in direct contact with the production equipment, a cover plate must be added to the fixture when using a tunnel furnace to sinter the products. The cover plate is basically made of alumina. If the cover plate comes into contact with the DCB product due to slipping or cracking, it will bond with the copper sheet on the DCB product at high temperature, causing adhesion and causing the DCB product to be scrapped, increasing the production cost of the DCB product. Summary of the invention
[0004] The object of the present invention is to provide a method for reducing the adhesion of a cover plate in a DCB sintering jig, by mixing magnesium oxide and ethyl orthosilicate in anhydrous ethanol as a dispersant to obtain a reaction solution, and spraying the solution evenly onto the surface of an alumina ceramic plate, and generating a magnesium silicate calcined layer under high temperature conditions to coat the surface of the alumina ceramic plate, thereby preventing the magnesium silicate calcined layer from falling off during the sintering process, isolating the alumina cover plate from contacting the copper in the DCB product, and solving the above-mentioned problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention adopts the following solutions:
[0006] A method for reducing cover plate adhesion in a DCB sintering fixture comprises the following steps:
[0007] Step 1: The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is roughened;
[0008] Step 2: Mix magnesium oxide and tetraethyl orthosilicate in proportion to obtain a solution to be reacted;
[0009] Step 3: spraying the reaction solution in step 2 uniformly on the surface of the alumina ceramic plate roughened in step 1;
[0010] Step 4: After the alumina ceramic plate in step 3 is dried, it is sintered to form a magnesium silicate sintered layer on the surface of the alumina ceramic plate.
[0011] The present invention mainly adopts magnesium oxide and ethyl orthosilicate to react under high temperature conditions to produce a new phase of magnesium silicate. The new phase of magnesium silicate has good coating properties on alumina ceramics during the generation process and is easy to form a stable, dense and non-falling coating layer.
[0012] Both magnesium oxide and tetraethyl orthosilicate are used as reactants. Magnesium oxide provides a magnesium source, and tetraethyl orthosilicate provides a silicon source. The two generate magnesium silicate under high temperature conditions, thereby forming a coating on the surface of the cover plate.
[0013] The specific reaction principle is:
[0014] Ethyl orthosilicate (C2H5O)4Si reacts under high temperature conditions to generate nano-scale SiO2:
[0015] (C2H5O)4Si+O2→CO2+H2O+SiO2.
[0016] The newly generated silicon oxide reacts with magnesium oxide at above 1000°C to form magnesium silicate:
[0017] SiO2+MgO→MgSiO3.
[0018] Specifically, in this method, silicon oxide is not directly used as the coating raw material, but tetraethyl orthosilicate is used to newly generate silicon oxide to provide a reactant, because the silicon oxide newly produced by tetraethyl orthosilicate under high temperature conditions is nano-scale, and the reaction activity of nano-scale silicon oxide is higher, so as to produce a better coating effect. Directly applying magnesium silicate powder to the surface of the alumina ceramic plate will cause it to fall off easily, and the fallen powdery substance will fall into the fixture and come into contact with the DCB product in the fixture, eventually contaminating the DCB product, causing the DCB product to be scrapped, and increasing production costs.
[0019] It should be noted that the high temperature condition in this method refers to a temperature between 1000°C and 1400°C.
[0020] Further preferably, in the step 1, the surface roughness of the alumina ceramic plate after roughening treatment is 0.5 μm to 3 μm.
[0021] The surface of the alumina ceramic plate is roughened to increase the roughness of the surface, thereby improving the coating bonding strength between the magnesium silicate sintered layer and the alumina ceramic plate.
[0022] Further preferably, in the step 2, the components are calculated by mass percentage as follows: 40% to 50% magnesium oxide, 20% to 30% tetraethyl orthosilicate, and the rest is a dispersant.
[0023] The dispersant is used to ensure uniform distribution and stable suspension of magnesium oxide and tetraethyl orthosilicate, so that magnesium oxide and tetraethyl orthosilicate are uniformly sprayed on the surface of the alumina ceramic plate.
[0024] Further preferably, the magnesium oxide and tetraethyl orthosilicate are used as reactants respectively.
[0025] More preferably, the dispersant is anhydrous ethanol.
[0026] Further preferably, in the step 4, the sintering temperature is 1000° C. to 1400° C., and the sintering time is 3 h to 6 h.
[0027] Further preferably, in the step 4, the thickness of the magnesium silicate sintered layer is 0.5 μm to 1.5 μm.
[0028] Further preferably, the alumina ceramic plate has a length of 190 mm to 210 mm and a width of 150 mm to 170 mm.
[0029] Further preferably, the thickness of the alumina ceramic plate is 0.3 mm to 2.0 mm.
[0030] The beneficial effects of the present invention are as follows: the present invention is a method for reducing the adhesion of the cover plate in a DCB sintering jig, wherein a mixture of magnesium oxide and tetraethyl orthosilicate is firstly evenly sprayed on the surface of an alumina ceramic plate, and then subjected to high-temperature sintering, the tetraethyl orthosilicate generates nano-scale silicon oxide at high temperature, and the newly generated nano-scale silicon oxide then reacts with magnesium oxide to generate magnesium silicate under high-temperature conditions, and the magnesium silicate has good coating properties on the alumina ceramic plate during the generation process, and forms a stable, dense, and non-detachable coating layer on the surface of the alumina ceramic plate, so that the copper in the DCB product will not contact the alumina in the cover plate, and high-temperature bonding of copper and alumina is avoided, thereby not changing the performance of the DCB product and reducing the product scrap rate. DETAILED DESCRIPTION
[0031] In order to more clearly demonstrate the purpose, technical solutions and advantages of the present invention, the present application will be further described below in conjunction with embodiments.
[0032] Example 1
[0033] The present invention is a method for reducing cover plate adhesion in a DCB sintering jig, which mainly comprises the following steps:
[0034] Step 1: The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is roughened to make the surface roughness of 0.5μm~3μm;
[0035] Step 2: Calculated by mass percentage, 40% to 50% magnesium oxide, 20% to 30% ethyl orthosilicate, and the rest being a dispersant, are mixed uniformly to obtain a solution to be reacted;
[0036] Step 3: spraying the reaction solution in step 2 uniformly onto the surface of the alumina ceramic plate roughened in step 1;
[0037] Step 4: After the alumina ceramic plate in step 3 is dried, it is sintered to form a magnesium silicate sintered layer.
[0038] The sintering temperature is 1000°C to 1400°C, the sintering time is 3h to 6h, and a magnesium silicate sintering layer is formed on the surface of the alumina ceramic plate.
[0039] The thickness of the magnesium silicate sintered layer is 0.5 μm to 1.5 μm.
[0040] The length of the alumina ceramic plate is 190mm~210mm, the width is 150mm~170mm, and the thickness is 0.3mm~2.0mm.
[0041] Example 2
[0042] The present invention is a method for reducing cover plate adhesion in a DCB sintering jig, which mainly comprises the following steps:
[0043] Step 1: The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is roughened to make the surface roughness of 0.6μm~2μm;
[0044] Step 2: Calculated by mass percentage, 42% to 48% of magnesium oxide, 24% to 28% of ethyl orthosilicate, and the rest of the dispersant are mixed evenly to obtain a solution to be reacted;
[0045] Step 3: spraying the reaction solution in step 2 uniformly onto the surface of the alumina ceramic plate roughened in step 1;
[0046] Step 4: After the alumina ceramic plate in step 3 is dried, it is sintered to form a magnesium silicate sintered layer.
[0047] The sintering temperature is 1100°C~1300°C, the sintering time is 4 hours, and a magnesium silicate sintering layer is formed on the surface of the alumina ceramic plate.
[0048] The thickness of the magnesium silicate sintered layer is 0.8 μm~1.3 μm.
[0049] The length of the alumina ceramic plate is 190mm~210mm, the width is 150mm~170mm, and the thickness is 0.5mm~1.5mm.
[0050] Example 3
[0051] The present invention is a method for reducing cover plate adhesion in a DCB sintering jig, which mainly comprises the following steps:
[0052] Step 1: The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is roughened to make the surface roughness of 0.8μm~1.2μm;
[0053] Step 2: Calculated by mass percentage, 42% to 48% of magnesium oxide, 24% to 28% of ethyl orthosilicate, and the rest of the dispersant are mixed evenly to obtain a solution to be reacted;
[0054] Step 3: spraying the reaction solution in step 2 uniformly onto the surface of the alumina ceramic plate roughened in step 1;
[0055] Step 4: After the alumina ceramic plate in step 3 is dried, it is sintered to form a magnesium silicate sintered layer.
[0056] The sintering temperature is 1200°C~1250°C, the sintering time is 5 hours, and a magnesium silicate sintering layer is formed on the surface of the alumina ceramic plate.
[0057] The thickness of the magnesium silicate sintered layer is 0.9 μm~1.2 μm.
[0058] The length of the alumina ceramic plate is 190mm~210mm, the width is 150mm~170mm, and the thickness is 0.7mm~1.0mm.
[0059] Comparative Example 1
[0060] The cover plate is an alumina ceramic plate with an untreated surface.
[0061] Comparative Example 2
[0062] The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is coated with magnesium oxide powder or magnesium silicate powder.
[0063] Comparative Example 3
[0064] The cover plate is an alumina ceramic plate, the surface of which is coated with magnesium oxide powder or magnesium silicate powder and then sintered at a high temperature.
[0065] Table 1 Coating usage in this method and comparative example
[0066]
[0067] As shown in Table 1, the aluminum oxide material in Comparative Example 1 will come into contact with the product and bond with the copper sheet on the product under high temperature conditions, thereby adhering to the DCB product and causing it to be scrapped.
[0068] The cover plate in Comparative Example 2, i.e., the alumina ceramic plate, can be coated with magnesium oxide powder or magnesium silicate powder to prevent adhesion, but direct coating of magnesium oxide powder or magnesium silicate powder is prone to fall off, and the fallen powder will contaminate the DCB product, causing the product to be scrapped.
[0069] In Comparative Example 3, magnesium oxide powder or magnesium silicate powder is applied to the surface of the alumina ceramic plate, and then sintered at high temperature, which can also play an anti-adhesion role. However, since no new phase is generated and magnesium oxide and magnesium silicate have high melting points, it is difficult to fix them on the surface of the alumina ceramic plate only by high temperature. Although it is convenient to directly apply magnesium oxide powder or magnesium silicate powder, it is still easy to fall off, and the fallen powder will still contaminate the DCB product, resulting in product scrapping.
[0070] The method uses magnesium oxide and tetraethyl orthosilicate as reactants and anhydrous ethanol as a dispersant to ensure that the reactant components are evenly mixed and evenly sprayed onto the surface of the alumina ceramic substrate. During the uniform mixing process, magnesium oxide and tetraethyl orthosilicate do not react. Only under high temperature conditions, tetraethyl orthosilicate provides a nano-level silicon source and magnesium oxide provides a magnesium source, and then the two react to form magnesium silicate. During the generation process, magnesium silicate has a good coating property for alumina ceramics and is easy to form a stable, dense, and non-detachable coating layer, that is, a magnesium silicate sintered layer is finally formed on the surface of the alumina ceramic plate.
[0071] When the DCB copper-clad substrate is placed in a jig in a tunnel furnace to sinter the product, the top cover of the jig is coated with a magnesium silicate sintered layer produced after a high-temperature reaction. The magnesium silicate sintered layer will not react with alumina or the copper in the DCB product, thereby preventing the alumina ceramic plate coated with the magnesium silicate sintered layer from adhering to the copper in the product, reducing the scrap rate of the product and reducing production costs.
[0072] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. According to the technical essence of the present invention, within the spirit and principles of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for reducing cover plate adhesion in a DCB sintering jig, characterized in that: The following steps are involved: Step 1: The cover plate is an alumina ceramic plate, and the surface of the alumina ceramic plate is roughened; Step 2: Mix magnesium oxide and tetraethyl orthosilicate in proportion to obtain a solution to be reacted; Step 3: spraying the reaction solution in step 2 uniformly on the surface of the alumina ceramic plate roughened in step 1; Step 4: After the alumina ceramic plate in step 3 is dried, it is sintered to form a magnesium silicate sintered layer on the surface of the alumina ceramic plate; In the step 2, the components are calculated by mass percentage, 40% to 50% magnesium oxide, 20% to 30% tetraethyl orthosilicate, and the rest is a dispersant; In the step 4, the sintering temperature is 1000° C. to 1400° C., and the sintering time is 3 h to 6 h.
2. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 1, characterized in that: In the step 1, the roughness of the surface of the alumina ceramic plate after the roughening treatment is 0.5 μm to 3 μm.
3. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 2, characterized in that: The magnesium oxide and tetraethyl orthosilicate are used as reactants respectively.
4. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 3, characterized in that: The dispersant is anhydrous ethanol.
5. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 3, characterized in that: In the step 4, the thickness of the magnesium silicate sintered layer is 0.5 μm to 1.5 μm.
6. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 3, characterized in that: The alumina ceramic plate has a length of 190 mm to 210 mm and a width of 150 mm to 170 mm.
7. A method for reducing cover plate adhesion in a DCB sintering jig according to claim 3, characterized in that: The thickness of the alumina ceramic plate is 0.3 mm to 2.0 mm.
Citation Information
Patent Citations
High-strength low-dielectric-loss aluminum oxide ceramic substrate
CN113149619A
Ceramic material
GB8501260D0