Ion conduction layer for electrochromic device and preparation method thereof, electrochromic device and application thereof

By adding water molecules to the ion conductive layer of the electrochromic device and using ultraviolet light to plasticize the polymer network structure and reduce the conductivity gradient, the problem of uneven discoloration of the electrochromic device is solved, and uniform discoloration and high temperature of the device are achieved. stability.

CN118393788BActive Publication Date: 2024-10-11BYD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410844924.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-11
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

When electrochromic devices are driven by voltage, the edges of the device change color preferentially, resulting in uneven overall color change. Especially when the size of the device is large, the response in the central area lags behind and the color difference is large.

Method used

Design an ion conductive layer. By adding water molecules as additives to the gel electrolyte, water molecules are used to plasticize the polymer network structure under ultraviolet light irradiation, and the conductivity decreases along the direction from the center to the edge of the ion conductive layer to control the conductivity gradient. , thereby optimizing the electrochromic effect, making the color change response in different areas consistent and the color difference small.

Benefits of technology

The color change response of different areas of the electrochromic device is almost consistent, the color difference is less than 2, the color change is uniform, and the response time change is less than 20% in a high temperature environment, and the color difference uniformity is less than 2.5, which is suitable for large-size electrochromic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118393788B_ABST
    Figure CN118393788B_ABST
Patent Text Reader

Abstract

The present invention discloses an ion conduction layer for an electrochromic device and a preparation method thereof, an electrochromic device and an application thereof. The ion conduction layer for the electrochromic device comprises, by mass percentage, 96% to 99.5% of a gel electrolyte and 0.5% to 4% of water, wherein the gel electrolyte comprises polyurethane acrylate, organic small molecules, lithium salts and initiators, and the conductivity gradient of the gel electrolyte decreases from the center to the edge of the ion conduction layer. According to the ion conduction layer for an electrochromic device of the present invention, by controlling the conductivity of the edge of the ion conduction layer to be lower than the conductivity of the center, the center part preferably reacts to electrochromism, thereby compensating for the response lag caused by the center area being far away from the electrode, so that the color change response of different regions of the electrochromic device is almost the same, the color difference is small, and the color change is uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to an ion conduction layer for an electrochromic device and a preparation method thereof, an electrochromic device and applications thereof. Background Art

[0002] In the related art, when electrochromic materials are operated in an external electric field, their optical properties such as transmittance, reflectivity, and absorptivity undergo stable and reversible changes, which manifest as reversible color changes such as coloring and fading. When the size of the electrochromic material device is large, the entire device surface will not change color at the same time under the drive of voltage. This is mainly because the voltage is input at the edge of the device, causing the edge of the device to change color first, and then expand to the middle area, making the overall color change of the device uneven. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, one object of the present invention is to provide an ion conduction layer for an electrochromic device, so that the color change response of different regions of the electrochromic device is almost the same, the color difference is small, and the color change is uniform.

[0004] Another object of the present invention is to provide a method for preparing an ion conducting layer for an electrochromic device.

[0005] Another object of the present invention is to provide an electrochromic device.

[0006] Another object of the present invention is to provide an application of an electrochromic device.

[0007] According to an embodiment of the first aspect of the present invention, the present invention provides an ion conduction layer for an electrochromic device, comprising, by mass percentage: 96% to 99.5% of a gel electrolyte and 0.5% to 4% of water, wherein the gel electrolyte comprises: polyurethane acrylate, organic small molecules, lithium salts and initiators, and the conductivity gradient of the gel electrolyte decreases along the direction from the center of the ion conduction layer to the edge of the ion conduction layer.

[0008] According to the ion conduction layer for the electrochromic device of the present invention, water molecules are used as additives of the system. Due to the large polarity of water molecules, water molecules can plasticize the polymer network structure of the gel electrolyte during the curing process of the gel electrolyte under the irradiation of ultraviolet (UV) light, thereby improving the transmission performance of lithium ions. The conductivity gradient of the gel electrolyte decreases along the direction from the center of the ion conduction layer to the edge of the ion conduction layer. In this way, when the size of the electrochromic device is large, since the electrodes are distributed around the electrochromic device, the electrochromic effect is preferentially generated around the electrochromic device. We control the conductivity of the edge of the ion conduction layer to be lower than the conductivity of the center, so that the central part preferably responds to electrochromism, thereby compensating for the response lag caused by the central area being far away from the electrode, so that the color change response of different areas of the electrochromic device is almost the same, the color difference is small, and the color change is uniform. For example, within 100ms of the color change of the edge of the electrochromic device, the color difference of the overall device uniformity is less than 2.

[0009] According to some embodiments of the present invention, the conductivity of the gel electrolyte decreases uniformly along a direction from the center of the ion conducting layer to the edge of the ion conducting layer.

[0010] According to some embodiments of the present invention, the conductivity of the central region of the ion conducting layer is σ1, and the conductivity of the edge region of the ion conducting layer is σ2, and σ1 and σ2 satisfy: σ1:σ2=5~12.

[0011] According to some embodiments of the present invention, the water has an electrical conductivity of 0.055 µS / cm to 0.061 µS / cm and a resistivity of 16.5 MΩ.cm to 18.2 MΩ.cm.

[0012] According to some embodiments of the present invention, the polyurethane acrylate, the organic small molecules, the lithium salt and the initiator satisfy: the polyurethane acrylate content is 50wt%-70wt%, the organic small molecules content is 20wt%-40wt%, the lithium salt content is 5wt%-20wt%, and the initiator content is 0.5wt%-3wt%.

[0013] According to some embodiments of the present invention, the gel electrolyte further includes: at least one of PEO, PVDF and PAN.

[0014] According to some embodiments of the present invention, in the gel electrolyte, the ratio of the total weight of the PEO, PVDF and PAN to the total weight of the polyurethane acrylate, PEO, PVDF and PAN is w, and the w satisfies: w<40%.

[0015] According to some embodiments of the present invention, the organic small molecule is an organic molecule comprising an active group and / or an unsaturated bond and having a molecular weight less than 800; preferably, the active group comprises at least one of a carbonate group, an amide group, a hydroxyl group and an ester group.

[0016] According to some embodiments of the present invention, the organic small molecules include: at least one of propylene carbonate, ethylene carbonate, acetonitrile, vinyl ethylene carbonate, vinylene carbonate, N,N-dimethylformamide, dimethyl carbonate, ethyl methyl carbonate, butanediol, propylene glycol, dimethylpropylene glycol, hexadiyne and diols.

[0017] According to some embodiments of the present invention, the lithium salt includes: at least one of 1-butyl-3-methylimidazolium lithium hexafluorophosphate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide lithium, 1-butyl-3-methylimidazolium lithium toluenesulfonate, 1-ethyl-2,3-dimethylimidazolium lithium hexafluorophosphate, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, bis(trifluoromethylsulfonyl)imide lithium salt, lithium tetrafluoroborate and lithium perchlorate.

[0018] According to some embodiments of the present invention, the initiator includes at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and ethyl 2,4,6-trimethylbenzoylphenylphosphonate.

[0019] According to some embodiments of the present invention, the thickness of the ion conducting layer is d, wherein d satisfies: 40 μm≤d≤100 μm; and / or,

[0020] The integrated transmittance of visible light is greater than 90%; and / or,

[0021] The L, a, and b values ​​of the ion conducting layer satisfy the following conditions: 90≤L≤95, -0.5≤a≤0.5, and -0.5≤b≤0.5, respectively.

[0022] According to an embodiment of the second aspect of the present invention, the present invention provides a method for preparing an ion conducting layer for an electrochromic device according to an embodiment of the first aspect of the present invention, comprising the following steps:

[0023] Prepare the polymer prepolymer, add organic small molecules and lithium salt, add initiator after mixing, then add water, cure and crosslink,

[0024] The amount of light is controlled so that the amount of light decreases gradually along the direction from the center of the ion conductive layer to the edge of the ion conductive layer, so that the curing cross-linking rate of the ion conductive layer decreases accordingly along the direction from the center of the ion conductive layer to the edge of the ion conductive layer.

[0025] According to some embodiments of the present invention, the method of gradually decreasing the amount of light includes: using white glass as a mask, and processing it through exposure and development technology, so that the transmittance of the light gradually decreases from the central area to the edge area of ​​the mask; preferably, the transmittance of the light gradually decreases from 92% to 70%.

[0026] According to some embodiments of the present invention, the illumination is ultraviolet illumination; and / or the energy of the ultraviolet light is 800 mJ / cm 2 ~3500mJ / cm 2 ; and / or the curing time is 300s to 1800s.

[0027] According to an embodiment of the third aspect of the present invention, the present invention provides an electrochromic device, comprising: a transparent conductive layer, an ion storage layer, an ion conduction layer, an electrochromic layer and a transparent conductive layer in sequence along the thickness direction, wherein the ion conduction layer is the ion conduction layer for the electrochromic device according to the above-mentioned first aspect of the present invention, or the ion conduction layer prepared by the preparation method according to the above-mentioned second aspect of the present invention.

[0028] According to some embodiments of the present invention, the transparent conductive layer includes: at least one of a metal mesh transparent conductive electrode, silver nanowires, indium tin oxide, fluorine-doped tin oxide, aluminum zinc oxide, carbon nanotubes and graphene.

[0029] According to some embodiments of the present invention, the electrochromic layer includes: at least one of poly 2,5-dibromo-3,4-ethylenedioxythiophene, poly 3,4-ethylenedioxythiophene, poly 3,4-bis(4-ethylhexyloxy)thiophene, polypyrrole, polyaniline, polystyrene sulfonate, di-(2-phosphonoethyl)-4,4'-bipyridine, 1,1'-dimethyl-4,4'-bipyridine, molybdenum oxide, tungsten oxide and titanium oxide.

[0030] According to some embodiments of the present invention, the ion storage layer includes at least one of vanadium pentoxide, nickel oxide, niobium pentoxide, Prussian blue and cerium oxide.

[0031] According to some embodiments of the present invention, within 100 ms after the edge of the electrochromic device changes color, the color difference uniformity of the device is less than 2.

[0032] According to some embodiments of the present invention, after being placed at 90° C. for 1000 hours, the response time of the electrochromic device changes by less than 20%, and the color difference uniformity of the device is less than 2.5.

[0033] According to an embodiment of the fourth aspect of the present invention, the present invention provides applications of an electrochromic device, wherein the electrochromic device is used in electronic and electrical components, automobile windows, rearview mirrors, and architectural glass windows.

[0034] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 is a schematic diagram of an electrochromic device according to a specific embodiment of the present invention;

[0036] Figure 2 is a schematic diagram of the position arrangement of E1, E2, E3, E4 and C on an electrochromic device according to a specific embodiment of the present invention;

[0037] Figure 3 It is a schematic diagram of a method for achieving a gradient decrease in light intensity by adjusting the mask transmittance according to a specific embodiment of the present invention (the light energy decreases gradually in the direction of the arrow).

[0038] Reference numerals:

[0039] 100: Electrochromic devices;

[0040] 1: ion conduction layer; 2: ion storage layer; 3: electrochromic layer; 4: transparent conductive layer. DETAILED DESCRIPTION

[0041] The ion conducting layer 1 for the electrochromic device 100 according to the first aspect of the present invention is described in detail below.

[0042] The ion conduction layer 1 for the electrochromic device 100 according to the first embodiment of the present invention includes a gel electrolyte and water. Here, water molecules are used as additives of the system. Due to the large polarity of water molecules, under the irradiation of ultraviolet (UV) light, during the curing process of the gel electrolyte, the water molecules can plasticize the gel electrolyte polymer network structure and improve the transmission performance of lithium ions. Among them, the strength of the interaction between water molecules and the gel electrolyte polymer network can seriously affect the conductivity of the ion conduction layer 1, and the conductivity of the ion conduction layer 1 is expressed as conductivity.

[0043] Among them, the water content is 0.5% to 4% by mass, and the remainder is gel electrolyte. In this way, if the water content is lower than 0.5%, the water content in the ion conductive layer 1 is less, the conductivity of the ion conductive layer 1 is poor, and the color difference of the electrochromic device 100 may be large; if the water content is higher than 4%, the water content in the ion conductive layer 1 is more, the gel electrolyte system of the ion conductive layer 1 is uneven, and flocculent substances are generated, and the color difference of the electrochromic device 100 may be large. By setting so that the water content is 0.5% to 4% by mass, the conductivity of the ion conductive layer 1 is good, the color difference of the electrochromic device 100 is small, and the electrochromic is uniform.

[0044] Among them, the gel electrolyte includes: polyurethane acrylate, organic small molecules, lithium salt and initiator. In this way, the gel electrolyte is generated by mixing and reacting the polymer, organic small molecules, lithium salt and initiator under certain conditions, and the conductivity of the gel electrolyte can be adjusted as needed. In addition, polyurethane acrylate has good adhesion, excellent optical properties and weather resistance. At the same time, due to the presence of urethane bonds, polyurethane acrylate has high elongation at break and can still maintain good performance at low temperatures. Polyurethane acrylate can be quickly cured by ultraviolet (UV) curing technology. During the photocuring process, the acrylate functional group undergoes free radical polymerization under the action of ultraviolet light and initiator to form a cross-linked network structure. The above curing process does not require solvents and has a fast curing speed, which is environmentally friendly and efficient.

[0045] Furthermore, since polyurethane acrylate water molecules have characteristic functional groups such as cyano (CN) and methyl (CH3), the intensity of the infrared absorption peak of the above characteristic functional groups is related to the strength of the gel electrolyte polymer network. Therefore, the strength of the gel electrolyte polymer network can be measured by the 1380cm -1 The methyl group at 1240 cm -1 The strength of the absorption peak of CN can be used to judge. Specifically, a certain content of water molecules will affect the hydrogen bonds and van der Waals forces between the molecular chains of the gel electrolyte polymer compound. When the water molecule content is too low, the effect is not obvious. When the water molecule content is too high, a large number of water molecules will reduce the compatibility with the gel electrolyte polymer network, which will destroy the gel electrolyte polymer network and cause crystal-like substances to precipitate and cannot be used.

[0046] In addition, along the direction from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1, the conductivity gradient of the gel electrolyte decreases. Here, the gradient decrease is to iteratively update the model parameters so that the conductivity of the gel electrolyte is in a downward direction. The gradient decrease is a step-like level decrease. For example, from the center of the ion conductive layer 1 to the area 10 microns away from the center, the conductivity of the gel electrolyte is x, from the area 10 microns to 20 microns away from the center, the conductivity of the gel electrolyte is y, and from the area 20 microns to 30 microns away from the center, the conductivity of the gel electrolyte is z, where x>y>z. In this way, when the size of the electrochromic device 100 is large (for example, when the diameter of the electrochromic device 100 is greater than 300mm), since the electrodes are distributed around the electrochromic device 100, the electrochromic effect is preferentially generated around the electrochromic device 100. By controlling the conductivity of the edge of the ion conducting layer 1 to be lower than that of the center, the center part preferentially responds to the electrochromic change, thereby compensating for the response lag caused by the center area being far away from the electrode, so that the color change response of different areas of the electrochromic device 100 is almost the same, the color difference is small, and the color change is uniform. For example, within 100ms of the color change of the edge of the electrochromic device 100, the color difference of the uniformity of the entire device is less than 2.

[0047] According to the ion conduction layer 1 for the electrochromic device 100 of the specific embodiment of the present invention, water molecules are used as additives of the system. Due to the large polarity of water molecules, water molecules can plasticize the polymer network structure of the gel electrolyte during the curing process of the gel electrolyte under the irradiation of ultraviolet (UV) light, thereby improving the transmission performance of lithium ions. The conductivity gradient of the gel electrolyte decreases along the direction from the center of the ion conduction layer 1 to the edge of the ion conduction layer 1. In this way, when the size of the electrochromic device 100 is large, since the electrodes are distributed around the electrochromic device 100, the electrochromic effect is preferentially generated around the electrochromic device 100. We control the conductivity of the edge of the ion conduction layer 1 to be lower than the conductivity of the center, so that the center part preferentially responds to electrochromism, thereby compensating for the response lag caused by the central area being far away from the electrode, so that the color change response of different areas of the electrochromic device 100 is almost the same, the color difference is small, and the color change is uniform. For example, within 100ms of the color change of the edge of the electrochromic device 100, the color difference of the uniformity of the overall device is less than 2.

[0048] According to some embodiments of the present invention, the conductivity of the gel electrolyte decreases uniformly along the direction from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1 (i.e., the conductivity decreases at a fixed value along the direction from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1). In this way, the speed of the gel electrolyte's electrochromic reaction decreases along the direction from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1, thereby effectively adjusting the color change effect of the electrochromic device 100, so that along the direction from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1, the color change of the electrochromic device 100 is uniform and the color difference is small.

[0049] According to some embodiments of the present invention, the conductivity of the central region of the ion conducting layer 1 is σ1, and the conductivity of the edge region of the ion conducting layer 1 is σ2, and σ1 and σ2 satisfy: σ1:σ2=5 to 12. Therefore, the setting of the ratio of the conductivity of the central region of the ion conducting layer 1 to the conductivity of the edge region of the ion conducting layer 1 is relatively reasonable, which is conducive to achieving the color change of the central region of the ion conducting layer 1 within 100ms after the color change of the edge region of the ion conducting layer 1, and the uniformity of the ion conducting layer 1 is less than 2, the color change is relatively uniform, and there is no obvious electrochromic delay phenomenon.

[0050] According to some embodiments of the present invention, the conductivity in water is 0.055µS / cm to 0.061µS / cm, and the resistivity is 16.5MΩ.cm to 18.2MΩ.cm. As a result, the ion concentration of water is low and the purity is high. For example, it can be ultrapure water, which is water produced by distillation, deionization, reverse osmosis technology or other appropriate supercritical fine technology, and its resistivity is greater than 16.5MΩ.cm, or close to the limit value of 18.2MΩ.cm (25°C). Simply put, it is water with almost all atoms except oxygen and hydrogen removed. In this way, during the solidification process of the gel electrolyte, the interference of ions in the water molecules can be avoided, and the water molecules can fully plasticize the polymer network structure of the gel electrolyte to improve the transmission performance of lithium ions. The conductivity and resistivity of water molecules can effectively improve the conductivity of the ion conduction layer 1.

[0051] In addition, polyurethane acrylate, organic small molecules, lithium salt and initiator meet the following conditions: polyurethane acrylate content is 50wt%-70wt%, organic small molecules content is 20wt%-40wt%, lithium salt content is 5wt%-20wt%, and initiator content is 0.5wt%-3wt%. Thus, the gel electrolyte generated by the mixed reaction of polyurethane acrylate, organic small molecules, lithium salt and initiator meets the requirements of ion conduction layer 1, improves the conductivity of ion conduction layer 1, and thus improves the electrochromic effect of electrochromic device 100.

[0052] Furthermore, the gel electrolyte may also include at least one of PEO (polyethylene oxide), PVDF (polyvinylidene fluoride) and PAN (polyacrylonitrile). Among them, PEO has good water solubility and thermoplasticity, is easy to shape, and has good elasticity. PVDF is a high-performance thermoplastic fluoropolymer, which has excellent chemical stability, weather resistance and thermal stability. The repeating unit of PAN is -CH2-CH(CN)-, and the cyano group (-CN) gives the polymer special properties, such as chemical corrosion resistance, heat resistance and certain hydrophilicity. Therefore, using at least one of PEO, PVDF and PAN as a copolymer is conducive to enhancing the chemical stability of the ion conductive layer 1 and reducing the difficulty of processing.

[0053] According to some specific embodiments of the present invention, in the gel electrolyte, the total weight of PEO, PVDF and PAN accounts for the total weight of polyurethane acrylate, PEO, PVDF and PAN by mass percentage, and w satisfies: w<40%. As a result, the content of polyurethane acrylate in the polymer is relatively large, while the total content of PEO, PVDF and PAN is relatively small, so as to facilitate the copolymerization of polyurethane acrylate, PEO, PVDF and PAN in the polymer.

[0054] According to some specific embodiments of the present invention, the organic small molecule is an organic molecule comprising an active group and / or an unsaturated bond and having a molecular weight less than 800; preferably, the active group comprises at least one of a carbonate group, an amide group, a hydroxyl group and an ester group.

[0055] Among them, active groups refer to atomic groups that can participate in chemical reactions, determine molecular properties or provide specific functions. Carbonate groups, amide groups, hydroxyl groups and ester groups can all generate dipole moments due to their electronic distribution states, charge characteristics or spatial configurations, resulting in the separation of positive and negative charges inside organic small molecules. As a result, the above-mentioned organic small molecules can exhibit different degrees of polarity, so that the organic small molecules can play a plasticizing role in the gel electrolyte.

[0056] Unsaturated bonds make organic small molecules have higher reactivity, which is beneficial to improve the preparation efficiency of gel electrolytes.

[0057] In addition, when the molecular weight of the organic small molecule is greater than 800, the molecular weight is large, which makes the solubility of the organic small molecule poor, and due to the large volume and rigid structure of the organic small molecule, it is easy to affect the effective contact between multiple reactants in the gel electrolyte, thereby affecting the reaction rate. Therefore, by making the molecular weight of the organic small molecule less than 800, it is beneficial to improve the solubility of the organic small molecule, so that multiple reactants in the gel electrolyte are fully contacted, the reaction rate is improved, and the uniformity of the gel electrolyte is improved.

[0058] According to some embodiments of the present invention, the organic small molecules include at least one of propylene carbonate, ethylene carbonate, acetonitrile, ethylene carbonate, vinylene carbonate, N,N-dimethylformamide, dimethyl carbonate, ethyl methyl carbonate, butanediol, propylene glycol, dimethyl propanediol, hexadiyne and diols. The functional groups (ester group, cyano group, amide group, hydroxyl group, etc.) of the above-mentioned organic small molecules can all generate dipole moments, resulting in the separation of positive and negative charges inside the organic small molecules, so that the above-mentioned organic small molecules can show different degrees of polarity, so that the organic small molecules can play a plasticizing role in the gel electrolyte. In addition, the above-mentioned organic small molecules have a wide range of sources and low costs, which is conducive to reducing the cost of the gel electrolyte.

[0059] According to some specific embodiments of the present invention, the lithium salt includes: 1-butyl-3-methylimidazolium lithium hexafluorophosphate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide lithium, 1-butyl-3-methylimidazolium toluenesulfonate lithium, 1-ethyl-2,3-dimethylimidazolium lithium hexafluorophosphate, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, bistrifluoromethanesulfonyl imide lithium, bisfluorosulfonyl imide lithium salt, lithium tetrafluoroborate and lithium perchlorate. The lithium salt adopts one of the above-mentioned organic lithium salts, and the anions in the organic lithium salt have a large radius and a relatively dispersed charge distribution, which is conducive to reducing the lattice energy of the lithium salt and weakening the interaction between positive and negative ions, thereby enhancing the stability of the gel electrolyte, and is conducive to improving the solubility of the organic lithium salt in the electrolyte, thereby helping to improve the ion conductivity of the gel electrolyte. In addition, the organic lithium salt also has the advantages of safety, greenness and low cost, which is conducive to improving the environmental protection performance of the gel electrolyte and reducing the cost of the gel electrolyte.

[0060] According to some specific embodiments of the present invention, the initiator includes at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester. The initiator is a substance that can absorb radiation energy of a specific wavelength (usually ultraviolet light or visible light). The above organic matter is used as an initiator. After absorbing light energy, the organic matter generates an active intermediate with the ability to initiate polymerization, such as a free radical or a cation. The active intermediate then initiates a chain polymerization reaction between monomer molecules to form a cross-linked polymer network to complete the curing process.

[0061] According to some embodiments of the present invention, the thickness of the ion conduction layer 1 is d, wherein d satisfies: 40 μm ≤ d ≤ 100 μm; and / or the integrated transmittance of visible light is greater than 90%; and / or the L, a, and b values ​​of the ion conduction layer 1 respectively satisfy: 90 ≤ L ≤ 95, -0.5 ≤ a ≤ 0.5, and -0.5 ≤ b ≤ 0.5.

[0062] Among them, the thickness of the ion conducting layer 1 is relatively reasonable, which meets the electrochromic requirements of the ion conducting layer 1 and avoids reducing the efficiency of the electrochromic due to the thick ion conducting layer 1.

[0063] The light integrated transmittance refers to the ratio of the energy attenuation of light after passing through a transparent or translucent material, and is usually used to quantify the light transmittance of a material. A higher visible light integrated transmittance is beneficial for lower energy loss after light passes through the ion conduction layer 1, thereby improving energy efficiency.

[0064] The Lab color model is a color calibration model specified by the International Commission on Illumination (CE—International Commission on Illumination - abbreviated as CIE from its French title CommissionInternationale de l'Eclairage), in which:

[0065] L represents brightness, ranging from 0 to 100, with 0 being the darkest and 100 being the brightest;

[0066] a is the color change from green to red, ranging from -128 to +128, pure green is negative 128, pure red is positive 128, and there are 256 levels in between;

[0067] b is the color change from blue to yellow, ranging from -128 to +128, pure blue is negative 128, pure yellow is positive 128, and there are 256 levels in between.

[0068] Therefore, the L, a, and b values ​​of the ion conductive layer 1 respectively satisfy: 90≤L≤95, -0.5≤a≤0.5, and -0.5≤b≤0.5. The color of the ion conductive layer 1 is relatively advanced, and the brightness and color saturation can meet the requirements of the electrochromic device 100.

[0069] According to an embodiment of the second aspect of the present invention, the present invention provides a method for preparing an ion conduction layer 1 for an electrochromic device 100 according to an embodiment of the first aspect of the present invention, comprising the following steps: preparing a prepolymer of a polymer, adding an organic small molecule and a lithium salt, adding an initiator after mixing, and then adding water to cure and crosslink. As a result, the molecular weight of the polymer prepolymer is low, and more functional groups that can be used for the next reaction are retained at both ends of the prepolymer. Small organic molecules and lithium salts are added to the prepolymer for mixing to facilitate the reaction of the groups of the prepolymer with the small organic molecules and the lithium salt. Initiators and water are added to initiate further polymerization reactions to form a cross-linked polymer network to complete the curing process.

[0070] The light irradiation is controlled so that the light irradiation decreases gradually from the center of the ion-conducting layer 1 to the edge of the ion-conducting layer 1, so that the curing cross-linking rate of the ion-conducting layer 1 decreases gradually from the center of the ion-conducting layer 1 to the edge of the ion-conducting layer 1. Thus, by controlling the light irradiation, the conductivity of the gel electrolyte decreases uniformly from the center of the ion-conducting layer 1 to the edge of the ion-conducting layer 1, thereby improving the color change uniformity and consistency of the electrochromic device 100, and making the color change of the electrochromic device 100 have no obvious color change delay phenomenon.

[0071] The method for preparing the ion conducting layer 1 for the electrochromic device 100 according to the embodiment of the present invention simplifies the method for preparing the ion conducting layer 1, improves the preparation efficiency of the ion conducting layer 1, helps to reduce the production cost of the ion conducting layer 1, and improves the market competitiveness of the ion conducting layer 1. In addition, the electrochromic device 100 prepared by the method greatly reduces the confluence procedure, saving the process of gradient treatment of the electrochromic device 100.

[0072] Further, refer to Figure 3 The method of decreasing the light intensity gradient includes: using white glass as a mask, and processing through exposure and development technology, and decreasing the light intensity transmittance gradient from the center area to the edge area of ​​the mask. In this way, the white glass is used as a mask after exposure and development to simplify the control process of decreasing the light intensity gradient from the center of the ion conductive layer 1 to the edge of the ion conductive layer 1, so that the light intensity gradient can be controlled under the condition of consistent gel electrolyte concentration, avoiding multiple adjustments of gel electrolyte concentration and glue filling steps, and facilitating the preparation of the ion conductive layer 1 that meets the needs. At the same time, the operability is strong, which is conducive to large-scale continuous production.

[0073] Preferably, the transmittance of the light intensity decreases gradually from 92% to 70%. Thus, the corresponding curing crosslinking rate of the ion conductive layer 1 is suitable for satisfying the requirement of uniform color change and small color difference of the ion conductive layer 1. Even within 100ms after the edge changes color, the uniform color difference of the entire device is less than 2. The light is ultraviolet light; and / or the energy of the ultraviolet light is 800mJ / cm 2 ~3500mJ / cm 2 ; and / or the curing time is 300s to 1800s. The energy of the ultraviolet light and the exposure time will affect the curing time and efficiency. Therefore, by controlling the energy of the ultraviolet light and the exposure curing time, it is beneficial to improve the curing efficiency, improve the curing and cross-linking effect, and further improve the color change effect of the ion conductive layer 1.

[0074] According to an embodiment of the third aspect of the present invention, referring to Figure 1The present invention provides an electrochromic device 100, comprising: a transparent conductive layer 4, an ion storage layer 2, an ion conduction layer 1, an electrochromic layer 3 and a transparent conductive layer 4 in order along the thickness direction, wherein the ion conduction layer 1 is the ion conduction layer 1 for the electrochromic device 100 according to the first aspect of the present invention, or the ion conduction layer 1 prepared by the preparation method according to the second aspect of the present invention.

[0075] Among them, light can freely pass through the transparent conductive layer 4 to act on the ion storage layer 2, the ion conduction layer 1 and the electrochromic layer 3. At the same time, the transparent conductive layer 4 can also be used for conduction, which is conducive to the realization of the electrochromic function of the electrochromic device 100. The ion storage layer 2 is used to store and provide the ions required in the electrochromic process. When an external electric field acts on the ion storage layer 2, the ion storage layer 2 and the electrochromic layer 3 work together to achieve a reversible change in color.

[0076] The electrochromic device 100 according to the embodiment of the present invention is conducive to increasing the structural stability of the electrochromic device 100 and realizing the reversible change of the color of the electrochromic device 100.

[0077] Further, the transparent conductive layer 4 includes: at least one of a metal mesh transparent conductive electrode, silver nanowires, indium tin oxide (ITO), fluorine-doped tin oxide (FTO), aluminum zinc oxide (AZO), carbon nanotubes and graphene. The above materials all have excellent light transmittance and conductivity, that is, using at least one of a metal mesh transparent conductive electrode, silver nanowires, indium tin oxide, fluorine-doped tin oxide, aluminum zinc oxide, carbon nanotubes and graphene as the transparent conductive layer 4 is conducive to realizing the conductive function of the transparent conductive layer 4 without affecting the penetration of light.

[0078] In addition, the electrochromic layer 3 includes: at least one of poly-2,5-dibromo-3,4-ethylenedioxythiophene, poly-3,4-ethylenedioxythiophene (PEDOT), poly-3,4-bis(4-ethylhexyloxy)thiophene, polypyrrole, polyaniline, polystyrene sulfonate (PSS), di-(2-phosphonoethyl)-4,4'-bipyridine, 1,1'-dimethyl-4,4'-bipyridine, molybdenum oxide, tungsten oxide and titanium oxide. The above materials have good thermal stability and chemical stability, strong adjustability and easy processing. Therefore, using at least one of the above materials as the electrochromic layer 3 is conducive to achieving a reversible change in the color or transparency of the electrochromic layer 3, while ensuring the stability of the electrochromic layer 3 and extending the service life of the electrochromic device 100.

[0079] According to some embodiments of the present invention, the ion storage layer 2 includes: at least one of vanadium pentoxide, nickel oxide, niobium pentoxide, Prussian blue and cerium oxide. During the electrochromic process, when an external electric field acts on the electrochromic layer 3, the ion storage layer 2 releases ions into the electrochromic layer 3, causing the color of the electrochromic layer 3 to change. When the direction of the electric field is reversed, the ions return from the electrochromic layer 3 to the ion storage layer 2, so that the electrochromic device 100 returns to the original color state.

[0080] Vanadium pentoxide, nickel oxide, niobium pentoxide, Prussian blue and cerium oxide all have good ionic conductivity and chemical stability, and are also suitable for capturing and releasing ions. Using at least one of vanadium pentoxide, nickel oxide, niobium pentoxide, Prussian blue and cerium oxide as the ion storage layer 2 improves the electrochromic effect of the electrochromic device 100, while ensuring that the electrochromic device 100 can be recycled for a long time, further extending the service life of the electrochromic device 100.

[0081] Among them, within 100ms after the edge of the electrochromic device 100 changes color, the color difference uniformity of the device is less than 2. Therefore, the electrochromic device 100 has a fast color change speed and good color change uniformity.

[0082] According to some embodiments of the present invention, after being placed at 90°C for 1000 hours, the response time of the electrochromic device 100 changes by less than 20%, and the color difference uniformity of the device is less than 2.5. Therefore, the electrochromic device 100 is suitable for use in a high temperature environment, thereby improving the applicability of the electrochromic device 100 and improving the market competitiveness of the electrochromic device 100.

[0083] According to an embodiment of the fourth aspect of the present invention, the present invention provides an application of an electrochromic device 100, wherein the electrochromic device 100 is used in electronic and electrical components, automobile windows, rearview mirrors, and architectural glass windows, wherein the automobile windows include automobile sunroofs.

[0084] The application of the electrochromic device 100 according to the embodiment of the present invention has a wide range of applications, which is beneficial to improving the applicability of the electrochromic device 100 and enhancing the market competitiveness of the electrochromic device 100.

[0085] Example 1

[0086] 1. Coating a PEDOT electrochromic layer 3:PSS (poly 3,4-ethylenedioxythiophene:polystyrene sulfonate) on a flexible conductive ITO (i.e. indium tin oxide) substrate using a slit coating technique to obtain a component with an electrochromic layer 3;

[0087] 2. Sputtering nickel oxide as the ion storage layer 2 on the flexible conductive ITO substrate using physical vapor deposition technology, thereby obtaining a component with the ion storage layer 2;

[0088] 3. Heat and mix polyoxypropylene glycol and polyethylene glycol at 110°C, and keep under vacuum for 2 hours to remove moisture from the polyether polyol. Cool down to 75°C, add a measured amount of isophorone diisocyanate, heat to about 90°C and react for 3 hours. Cool down to 80°C, add hydroxyethyl acrylate, chain extender 1,4-butanediol and catalyst, heat to about 70°C and react for 5 hours. You can get polyurethane acrylate prepolymer;

[0089] Take 70g of the prepolymer, then add 27g of propylene carbonate solution dissolved with lithium perchlorate (25%) to the prepolymer and mix well, then add 2% of 1-hydroxycyclohexyl phenyl ketone initiator, then add 1% of water using a microliter syringe, mix well and store in the dark, wherein the conductivity of water is 0.055µS / cm and the resistivity is 18.2MΩ.cm;

[0090] 4. Use a cutting device to cut the electrochromic layer 3 and the ion conducting layer 1 into a circle with a diameter of 300 mm, and use gel electrolyte glue to bond the electrochromic layer 3 and the ion storage layer 2 together in a composite device;

[0091] 5. Then put the mask on the color-changing device. The mask shape is circular with a diameter of 350mm. The transmittance from the center to the edge changes from 92% to 85%. Set the UV light energy to 1000mJ / cm 2 , then exposed and cured for 360 seconds to obtain the electrochromic device 100;

[0092] 6. Finally, the uniformity of the electrochromic device 100 is tested;

[0093] 7. The ratio of the conductivity of the central area of ​​the ion conduction layer to the conductivity of the edge area is 5.2.

[0094] Example 2

[0095] The difference from Example 1 is that the water content of the ion conducting layer 1 is 2%, and the optical transmittance from the center to the edge of the mask is from 92% to 80%. The other steps remain unchanged.

[0096] Example 3

[0097] The difference from Example 1 is that the water content of the ion conducting layer 1 is 3%, and the optical transmittance from the center to the edge of the mask is from 92% to 75%. The other steps remain unchanged.

[0098] Example 4

[0099] The difference from Example 1 is that the water content of the ion conducting layer 1 is 4%, and the optical transmittance from the center to the edge of the mask is from 92% to 70%. The other steps remain unchanged.

[0100] Example 5

[0101] 1. Coating a PEDOT:PSS electrochromic layer 3 on a flexible conductive ITO substrate using a slit coating technique to obtain a component with an electrochromic layer 3;

[0102] 2. Sputtering nickel oxide as the ion storage layer 2 on the flexible conductive ITO substrate using physical vapor deposition technology, thereby obtaining a component with the ion storage layer 2;

[0103] 3. Heat and mix the polyester polyol at 120℃ and keep it under vacuum for 2 hours to remove the moisture in the polyester polyol. Cool down to 75℃, add the measured amount of toluene diisocyanate and heat it to about 85℃ and react for 3 hours. Cool down to 80℃, add hydroxyethyl acrylate, chain extender 1,4-butanediol and catalyst, heat it to about 70℃ and react for 6 hours. The polyurethane acrylate prepolymer can be obtained;

[0104] Take 70g of the prepolymer, then add 26g of propylene carbonate solution containing 25% lithium perchlorate to the prepolymer and mix well, then add 2% of 1-hydroxycyclohexyl phenyl ketone initiator, then add 2% of water using a microliter syringe, mix well and store in a dark place;

[0105] 4. Use a cutting device to cut the electrochromic layer 3 and the ion conducting layer 1 into a circle with a diameter of 300 mm, and use gel electrolyte glue to bond the electrochromic layer 3 and the ion storage layer 2 together in a composite device;

[0106] 5. Then place the mask on the color-changing device. The mask is circular in shape with a diameter of 350mm. The transmittance from the center to the edge changes from 92% to 80%. Set the UV light energy to 1000mJ / cm 2 , then exposed and cured for 360 seconds to obtain the electrochromic device 100;

[0107] 6. Finally, the uniformity and high temperature stability of the electrochromic device 100 are tested.

[0108] Example 6

[0109] 1. Coating a PEDOT:PSS electrochromic layer 3 on a flexible conductive ITO substrate using a slit coating technique to obtain a component with an electrochromic layer 3;

[0110] 2. Sputtering nickel oxide as the ion storage layer 2 on the flexible conductive ITO substrate using physical vapor deposition technology, thereby obtaining a component with the ion storage layer 2;

[0111] 3. Heat and mix the polyester polyol at 120°C, and keep it under vacuum for 2 hours to remove moisture from the polyester polyol. Cool down to 75°C, add the measured amount of isophorone diisocyanate and raise the temperature to about 85°C to react for 4 hours. Cool down to 75°C, add hydroxyethyl acrylate, chain extender 1,4-butanediol and catalyst, raise the temperature to about 85°C to react for 8 hours. The polyurethane acrylate prepolymer can be obtained. Take 70g of the prepolymer, then add 26g of propylene carbonate solution dissolved with lithium perchlorate (25%) to the prepolymer and mix well, then add 2% of 1-hydroxycyclohexyl phenyl ketone initiator, and then use a microliter syringe to add 2% of water, mix well and store in the dark;

[0112] 4. Use a cutting device to cut the electrochromic layer 3 and the ion conducting layer 1 into a circle with a diameter of 300 mm, and use gel electrolyte glue to bond the electrochromic layer 3 and the ion storage layer 2 together in a composite device;

[0113] 5. Then put the mask on the color-changing device. The mask shape is circular with a diameter of 350mm. The transmittance from the center to the edge changes from 92% to 80%. Set the UV light energy to 1000mJ / cm 2 , then exposed and cured for 360 seconds to obtain the electrochromic device 100;

[0114] 6. Finally, the uniformity of the electrochromic device 100 is tested.

[0115] Example 7

[0116] The difference from Example 2 is that the prepolymer is a mixture of the prepolymer synthesized in Example 1 and polyethylene oxide (ie, PEO), 70 g of the prepolymer includes 55 g of the prepolymer synthesized in Example 1 and 15 g of PEO, and the other steps remain unchanged.

[0117] Example 8

[0118] The difference from Example 1 is that in step 4, the size of the functional membrane is 600 mm, in step 5, the light intensity is increased to 2000 mJ / cm2, the curing time is 600 s, and finally the conductivity ratio of the central area to the edge area is 7.5.

[0119] Example 9

[0120] The difference from Example 1 is that the size of the functional membrane in step 4 is 900 mm, the light intensity in step 5 is increased to 2500 mJ / cm2, the curing time is 1080 s, and finally the ratio of the conductivity of the central area to the conductivity of the edge area is 9.8.

[0121] Example 10

[0122] The difference from Example 1 is that the size of the functional membrane in step 4 is 1200 mm, the light intensity in step 5 is increased to 3500 mJ / cm2, the curing time is 1800 s, and finally the ratio of the conductivity of the central area to the conductivity of the edge area is 12.

[0123] Embodiment 11

[0124] The difference from Example 1 is that the ionic conductivity of water is 10 uS / cm, and the other steps remain unchanged. Finally, the ratio of the conductivity of the central area to the conductivity of the edge area is 2.7.

[0125] Example 12

[0126] The difference from Example 1 is that the curing time in step 5 is 60 seconds, and the final ratio of the conductivity of the central area to the conductivity of the edge area is 3.2.

[0127] Comparative Example 1

[0128] The difference from Example 1 is that the water content in the ion conducting layer 1 is 0%, and the other steps remain unchanged. Finally, the ratio of the conductivity of the central area to the conductivity of the edge area is 1.5.

[0129] Comparative Example 2

[0130] The difference from Example 1 is that the water content in the ion conducting layer 1 is 5%, and the other steps remain unchanged.

[0131] Comparative Example 3

[0132] The difference from Example 1 is that the ion conducting layer 1 is a PMMA (polymethyl methacrylate) based gel electrolyte, and the specific preparation method is as follows:

[0133] 1. Take 10g of dried LiClO4 powder and add it to 90g of propylene carbonate (PC) solvent. Stir it magnetically for more than 5 hours in a dark environment to obtain a lithium salt solution, which is stored in a brown reagent bottle for later use. Weigh 20g of the standby lithium salt solution and an appropriate amount of PMMA particles (high flow type), mix them evenly, and heat them in a blast drying oven at 180℃ for 4 hours to obtain a PMMA gel electrolyte with a lithium salt content of 7.5%;

[0134] 2. Use a cutting device to cut the electrochromic layer 3 and the ion conducting layer 1 into a circle with a diameter of 300 mm, and use electrolyte glue to bond the electrochromic layer 3 and the ion storage layer 2 together in a composite device. PMMA gel electrolyte does not require gradient light curing.

[0135] Uniformity test of electrochromic device 100

[0136] Test method: Reference Figure 2 , the electrochromic devices 100 cured and packaged in Examples 1-12 and Comparative Examples 1-3 were connected to a 1.5V external power supply, and when the edge positions E1, E2, E3, and E4 of the device changed from a faded state to a colored state, the power input was canceled within 100ms, and the color difference ΔE between the edge positions E1, E2, E3, and E4 of the device and the center position C was tested using a colorimeter, where E1, E2, E3, and E4 were 4 cm away from the edge, and C was located at the center of the electrochromic device 100. The test results are shown in Table 1.

[0137] Table 1 Color difference between different positions and the central area within 100ms

[0138]

[0139] After the above-mentioned Examples 1 to 12 and Comparative Examples 1 to 3 were placed at 90° C. for 1000 hours, experimental tests were performed. The results are shown in Table 2:

[0140] Table 2 Color difference between different positions and the central area after 1000 hours (100ms)

[0141]

[0142] Combining the test results of Examples 1 to 12, Comparative Examples 1 to 3 and Tables 1 and 2, it can be seen that the gel electrolyte containing water and a polyurethane acrylate system can obtain a color difference between the edge and the middle area of ​​less than 2 within 100ms of edge discoloration under the condition of gradient curing, and after high temperature for 1000h, the color difference between the edge and the middle area of ​​less than 2.5 within 100ms of edge discoloration.

[0143] Combining Examples 1 to 4 and their test results, it can be seen that with the increase of water content, the required light gradient will also change. This is mainly due to the difference in water content, and the gel electrolyte polymer network structure of the ion conductive layer 1 has different responses to UV generation, but an electrochromic device 100 with a color difference of less than 2 can be obtained. Even if different types of polyurethane acrylate systems are replaced, such as Examples 5 and 6, an electrochromic device 100 with a uniform color change response can be obtained.

[0144] Combining Example 7 and its test results, it can be seen that the polyurethane acrylate system doped with the PEO network can still obtain an electrochromic device 100 with a color difference of less than 2 within 100 ms.

[0145] Combining Examples 8 to 10 and their test results, it can be seen that as the size of the functional membrane increases, the required illumination energy and time also change accordingly. This is because when the size of the functional membrane increases, the ion conductivity ratio of the middle area and the edge area needs to increase, that is, the degree of curing and crosslinking of the edge area and the middle area should be more different. Therefore, by adjusting the appropriate conductivity ratio, a device with a color difference of less than 2 is finally obtained, indicating that the technical solution can solve the problem of uneven color change of large sizes.

[0146] Combining Example 1 and Example 11 and their test results, it can be seen that if there is no water in the ion conduction layer 1, the color difference of the electrochromic device 100 is greater than 14, and even reaches 17.47. This is mainly because without the addition of water, the conductivity of the ion conduction layer 1 is poor.

[0147] Combining Example 1 and Example 11 and their test results, it can be seen that the conductivity of water molecules is 10uS / cm, the color difference obtained under the same curing conditions is greater than 2, and the conductivity ratio is 2.7. This is mainly due to the influence of other ions in water on the curing of the electrolyte glue network.

[0148] Combining Example 1 and Example 12 and their test results, it can be seen that if the curing time is short, the degree of glue curing is insufficient, resulting in a smaller conductivity ratio between the middle area and the edge area, ultimately resulting in a larger color difference.

[0149] Combining Example 1 and Comparative Example 2 and their test results, it can be seen that the amount of water molecules cannot be excessive. When the water content is 5%, the gel electrolyte system is uneven and flocculent substances are generated.

[0150] Combining Example 1, Comparative Example 1 and Comparative Example 3 and their test results, it can be seen that when PMMA is used instead of polyurethane acrylate, the color difference of Comparative Example 3 is smaller than that of Comparative Example 1. This may be mainly because the color changing ability of PMMA itself is higher than that of anhydrous polyurethane acrylate, but PMMA cannot adjust the gradient conductivity of the ion conductive layer 1 by photocuring, which ultimately leads to slow color change in the middle of the electrochromic device 100 and fast color change around it, and the color difference is also more than 10, and uniform electrochromism cannot be achieved.

[0151] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.

[0152] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.

Claims

1. An ion conducting layer for an electrochromic device, characterized in that: The invention comprises, by mass percentage, 96% to 99.5% of a gel electrolyte and 0.5% to 4% of water, wherein the water has an electrical conductivity of 0.055 µS / cm to 0.061 µS / cm and a resistivity of 16.5 MΩ.cm to 18.2 MΩ.cm. The gel electrolyte comprises polyurethane acrylate, organic small molecules, lithium salt and initiator. The conductivity gradient of the gel electrolyte decreases gradually along a direction from the center of the ion conducting layer to the edge of the ion conducting layer.

2. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The conductivity of the gel electrolyte decreases uniformly along a direction from the center of the ion conducting layer to the edge of the ion conducting layer.

3. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The electrical conductivity of the central region of the ion conducting layer is σ1, and the electrical conductivity of the edge region of the ion conducting layer is σ2, and the σ1 and σ2 satisfy: σ1:σ2=5~12.

4. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The polyurethane acrylate, the organic small molecules, the lithium salt and the initiator satisfy the following conditions: the polyurethane acrylate content is 50wt% to 70wt%, the organic small molecules content is 20wt% to 40wt%, the lithium salt content is 5wt% to 20wt%, and the initiator content is 0.5wt% to 3wt%.

5. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The gel electrolyte further comprises at least one of PEO, PVDF and PAN.

6. The ion conducting layer for an electrochromic device according to claim 5, characterized in that: In the gel electrolyte, the ratio of the total weight of the PEO, PVDF and PAN to the total weight of the polyurethane acrylate, PEO, PVDF and PAN is w, and the w satisfies: w<40%.

7. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The organic small molecule is an organic molecule including an active group and / or an unsaturated bond and having a molecular weight less than 800.

8. The ion conducting layer for an electrochromic device according to claim 7, characterized in that: The active group includes at least one of a carbonate group, an amide group, a hydroxyl group and an ester group.

9. The ion conducting layer for an electrochromic device according to claim 7, characterized in that: The organic small molecules include at least one of propylene carbonate, ethylene carbonate, acetonitrile, vinyl ethylene carbonate, vinylene carbonate, N,N-dimethylformamide, dimethyl carbonate, ethyl methyl carbonate, butanediol, propylene glycol, dimethylpropylene glycol, hexadiyne and diols.

10. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The lithium salt includes: at least one of 1-butyl-3-methylimidazolium lithium hexafluorophosphate, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)imide lithium, 1-butyl-3-methylimidazolium lithium toluenesulfonate, 1-ethyl-2,3-dimethylimidazolium lithium hexafluorophosphate, lithium hexafluorophosphate, lithium trifluoromethanesulfonate, lithium bistrifluoromethanesulfonyl imide, bisfluorosulfonyl imide lithium salt, lithium tetrafluoroborate and lithium perchlorate.

11. The ion conducting layer for an electrochromic device according to claim 1, characterized in that: The initiator comprises at least one of 2-hydroxy-2-methyl-1-phenylpropanone, 1-hydroxycyclohexylphenyl ketone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylphosphonic acid ethyl ester.

12. The ion conducting layer for an electrochromic device according to any one of claims 1 to 11, characterized in that: The thickness of the ion conducting layer is d, wherein d satisfies: 40 μm≤d≤100 μm; and / or, The visible light integrated transmittance of the ion conducting layer is greater than 90%; and / or, The L, a, and b values ​​of the ion conducting layer satisfy the following conditions: 90≤L≤95, -0.5≤a≤0.5, and -0.5≤b≤0.5, respectively.

13. A method for preparing an ion conducting layer for an electrochromic device according to any one of claims 1 to 12, characterized in that: The steps include: Prepare the polymer prepolymer, add organic small molecules and lithium salt, add initiator after mixing, then add water, cure and crosslink, The amount of light is controlled so that the amount of light decreases gradually along the direction from the center of the ion conductive layer to the edge of the ion conductive layer, so that the curing cross-linking rate of the ion conductive layer decreases accordingly along the direction from the center of the ion conductive layer to the edge of the ion conductive layer.

14. The preparation method according to claim 13, characterized in that: The method for decreasing the light intensity gradually includes: using white glass as a mask, and processing it through exposure and development technology, so that the transmittance of the light intensity gradually decreases from the central area to the edge area of ​​the mask.

15. The preparation method according to claim 14, characterized in that: The transmittance of the light intensity decreases gradually from 92% to 70%.

16. The preparation method according to claim 13, characterized in that: The light is ultraviolet light, and the energy of the ultraviolet light is 800mJ / cm 2 ~3500mJ / cm 2 ; The curing time is 300s to 1800s.

17. An electrochromic device, characterized in that: include: Along the thickness direction, there are a transparent conductive layer, an ion storage layer, an ion conduction layer, an electrochromic layer and a transparent conductive layer. The ion conducting layer is an ion conducting layer for an electrochromic device according to any one of claims 1 to 12, or an ion conducting layer prepared by the preparation method according to any one of claims 13 to 16.

18. The electrochromic device according to claim 17, characterized in that: The transparent conductive layer comprises: at least one of a metal mesh transparent conductive electrode, silver nanowires, indium tin oxide, fluorine-doped tin oxide, aluminum zinc oxide, carbon nanotubes and graphene.

19. The electrochromic device according to claim 17, characterized in that: The electrochromic layer includes at least one of poly 2,5-dibromo-3,4-ethylenedioxythiophene, poly 3,4-ethylenedioxythiophene, poly 3,4-bis(4-ethylhexyloxy)thiophene, polypyrrole, polyaniline, polystyrene sulfonate, di-(2-phosphonoethyl)-4,4'-bipyridine, 1,1'-dimethyl-4,4'-bipyridine, molybdenum oxide, tungsten oxide and titanium oxide.

20. The electrochromic device according to claim 17, characterized in that: The ion storage layer includes at least one of vanadium pentoxide, nickel oxide, niobium pentoxide, Prussian blue and cerium oxide.

21. The electrochromic device according to any one of claims 17 to 20, wherein within 100 ms after the edge of the electrochromic device changes color, the color difference uniformity of the device is less than 2.

22. The electrochromic device according to any one of claims 17 to 20, characterized in that: After being placed at 90° C. for 1000 hours, the response time of the electrochromic device changes by less than 20%, and the color difference uniformity of the device is less than 2.

5.

23. Use of an electrochromic device according to any one of claims 17 to 22, characterized in that: The electrochromic device is used for electronic and electrical components, automobile windows, rearview mirrors and architectural glass windows.