A pressure-resistant balloon, preparation method and balloon dilatation catheter
Through the design of the tightly hooked fiber layer and the thin dense glue layer, the problem of the balloon being prone to bursting and poor passability under high pressure is solved, and the pressure resistance performance and intravascular stability of the balloon are improved.
Patent Information
- Application Number
- CN202410868124.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-07-01
AI Technical Summary
Existing balloons are prone to bursting under high pressure, causing damage to blood vessels, and fiber braiding increases the thickness of the balloon, affecting passability, making it difficult to move stably within blood vessels.
It adopts a tightly hooked fiber layer and a dense glue layer. The fiber layer is crocheted and cross-threaded by a hook knitting machine. The glue layer is thin and evenly sprayed to enhance the pressure resistance and passability of the balloon.
It improves the pressure resistance and intravascular passability of the balloon, reduces the risk of deformation and collapse, and ensures the stability and precise shape control of the balloon under high pressure.
Smart Images

Figure CN118403272B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of medical equipment, and in particular to a pressure-resistant balloon, a preparation method and a balloon dilatation catheter. Background Art
[0002] Balloon dilatation catheter is the most widely used type of vascular interventional treatment, and has a good therapeutic effect on improving the symptoms of vascular stenosis or occlusion. It uses a guidewire to push the balloon catheter to the lesion site, and uses the balloon to expand the blood vessel in a pressurized manner, so that calcification or plaque moves from the center of the blood vessel lumen to the wall of the vascular system, thereby improving blood flow. Therefore, pressure resistance is one of the main properties of the balloon. However, in the process of treating some lesions with severe calcification, heavy plaque load or long-term chronic occlusion, very high working pressure (>24atm) is often required. However, expanding the balloon under higher pressure will make the balloon explode at risk. Once the balloon cannot withstand the pressure and ruptures, it will cause extremely serious damage to the patient's blood vessels, causing vascular dissection or tearing at the mildest, and vascular perforation or rupture at the worst, endangering the patient's life.
[0003] In order to improve the pressure resistance of the balloon, the current common method is to use a weaving machine to weave fibers onto the balloon and coat them with glue to connect them to form a high-pressure resistant balloon. However, during the weaving process, the fiber layer is mostly plain or twill. When the fiber is woven to the cone of the balloon, the presence of the inclined surface will cause the fiber to slide. Therefore, a thicker glue layer is required to stably connect the fiber layer to the outer surface of the balloon. However, the weaving part on the balloon has increased the thickness of the balloon. After the glue layer is applied, it will be harder and occupy a larger volume during the folding and winding process, affecting the passability of the balloon in the blood vessel and increasing the difficulty of the surgical procedure.
[0004] Therefore, how to improve the pressure resistance of the balloon while ensuring its intravascular permeability is an urgent problem to be solved by those skilled in the art. Summary of the invention
[0005] In view of this, an object of the present invention is to provide a pressure-resistant balloon to improve the pressure resistance of the balloon on the basis of ensuring the intravascular passability of the balloon.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned pressure-resistant balloon.
[0007] Another object of the present invention is to provide a balloon dilatation catheter comprising the pressure-resistant balloon.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] A pressure-resistant balloon, comprising:
[0010] A balloon body, wherein both ends of the balloon body are of a conical configuration;
[0011] A fiber layer and a glue layer, wherein the fiber layer is crocheted from a fiber bundle formed by twisting multiple fibers, the fiber layer is tightly crocheted and attached to the outer wall of the balloon body, and both ends of the fiber layer are located at the tube legs of the balloon body and cross-threaded and crocheted, the glue layer is used to bond the balloon body and the fiber layer, the glue layer is a dense glue layer and its thickness is no greater than that of the fiber layer.
[0012] Preferably, in the above-mentioned pressure-resistant balloon, the fiber layer is tightly crocheted in a specific manner, with a pore size of the crocheted mesh being 200 μm-800 μm, and the crocheting manner being front crocheting, back crocheting, front and back single-sided crocheting, or front and back double-sided crocheting.
[0013] Preferably, in the above-mentioned pressure-resistant balloon, the front side crochet is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in the first direction, any of the peak configurations passes through the bottoms of two of the peak configurations of the adjacent fiber bundles;
[0014] The reverse side crochet is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in a second direction, any of the peak configurations passes through the tops of two of the peak configurations of the adjacent fiber bundles, and the second direction is opposite to the first direction;
[0015] The one-front-one-back single-sided crochet weaving is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, the peak configuration on one side sequentially passes through the top and bottom of the peak configuration in the adjacent fiber bundle, and the top of the peak configuration on the opposite side passes through the middle of the raised edges of the two peak configurations in the adjacent fiber bundle;
[0016] The front and back double-sided crochet weaving is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in the first direction and the second direction, any peak configuration passes through the top and bottom of two peak configurations of the adjacent fiber bundles in sequence.
[0017] Preferably, in the above-mentioned pressure-resistant balloon, the hooking position of the fiber layer starts from the tube leg 1mm-20mm away from the balloon body or the cone portion of the mold, and ends at the tube leg 1mm-20mm away from the cone portion of the balloon body or the other end of the mold, or, the hooking position of the fiber layer starts from the cone portion of the balloon body or the mold and ends at the cone portion at the other end.
[0018] Preferably, the above-mentioned pressure-resistant balloon further comprises a lubricating layer, wherein the lubricating layer is an elastic film wrapped around the balloon body or a lubricating coating applied when the balloon body is in an inflated state.
[0019] A preparation method for preparing the pressure-resistant balloon provided in any one of the above embodiments, the preparation method comprising at least the following steps:
[0020] Crocheting the fiber layer: the fiber layer is crocheted by a crochet loom in the middle cylindrical area of the balloon body, the fiber layer is closely crocheted to avoid sliding, and the fiber layer is cross-threaded at the conical positions at both ends of the balloon body to tighten the fiber layer and avoid curling;
[0021] Spraying the glue layer: spraying the atomized glue evenly toward the fiber layer through an atomizing device, and curing it in an oxygen-isolated environment to form the glue layer.
[0022] Preferably, in the above preparation method, in the step of spraying the glue layer, the balloon body is sprayed with atomized glue after plasma treatment, and is cured for 2 minutes to 5 minutes under nitrogen protection or vacuum environment to form the glue layer.
[0023] Preferably, in the above preparation method, the processing gas for the plasma treatment process of the balloon body is air, oxygen, argon or argon-hydrogen mixed gas, and the gas volume is 50-180sccm.
[0024] A balloon dilatation catheter comprises a terminal tube, a catheter and a pressure-resistant balloon provided by any one of the above embodiments, wherein the pressure-resistant balloon is arranged between the terminal tube and the catheter.
[0025] Preferably, in the above-mentioned balloon dilatation catheter, the balloon dilatation catheter is an integral exchange balloon dilatation catheter or a rapid exchange balloon dilatation catheter.
[0026] It can be seen from the above technical scheme that the pressure-resistant balloon provided by the present invention includes a balloon body, a fiber layer and a glue layer, wherein the balloon body is a single-lumen tube extruded by an extruder and is hot-blow molded on a balloon molding machine containing a convex mold, and the two ends of the balloon body are conical configurations to facilitate guidance and movement in the blood vessel, and the fiber layer is sleeved on the periphery of the balloon body to utilize the higher strength of the fiber to restrain the balloon, thereby improving the pressure resistance of the balloon body and reducing deformation of the balloon as much as possible during use to obtain more precise shape control. Specifically, the fiber layer is a fiber bundle formed by twisting multiple fibers, which is made by tightly crocheting. In order to improve the fit between the fiber layer and the balloon body, reduce the risk of collapse of the fiber layer in the conical area on the balloon body, and thereby shorten the length of the conical area on the balloon body to improve the bending performance of the pressure-resistant balloon, the two ends of the fiber layer, that is, the fiber layer located at the tube leg position of the balloon, adopt a cross-threading crocheting method. The finishing treatment of the fiber layer hooking is completed so that the two ends of the fiber layer can fully contact the balloon body to prevent the fiber layer from curling up. The glue layer is used to bond and fix the balloon body and the fiber layer. Preferably, the glue layer is a dense glue layer, and its thickness is not greater than the thickness of the fiber layer, so that the pressure-resistant balloon has better foldability. Preferably, after the fiber layer is sleeved on the balloon body, the atomized glue is evenly sprayed toward the fiber layer through an atomizing device, and cured in an oxygen-isolated environment to form a glue layer. During the setting of the glue layer, the atomized glue can evenly enter the gap, thereby achieving fixation of the balloon body and the fiber layer through a thinner glue layer. The glue layer is isolated from oxygen during the curing process to prevent oxygen in the air from inhibiting the free radical polymerization reaction of the contacted glue during the curing process, so that the glue monomer can be completely polymerized and cross-linked to form a completely cured product, thereby ensuring the connection effect between the balloon body and the fiber layer. The pressure-resistant balloon provided by the present invention has a tightly crocheted fiber layer on the outer surface of the balloon body, and the fiber layer is cross-threaded at both ends, so that the fiber layer has strong integrity and is not prone to sliding. Preferably, the fiber layer is evenly sprayed with atomized glue through an atomizing device, and the glue is cured in an oxygen-isolated environment to ensure the polymerization and bonding effect of the glue, and then the balloon body and the fiber layer are bonded and fixed by a thinner glue layer, avoiding the glue layer being too thick and affecting the folding performance of the balloon, ensuring the passability of the balloon in the blood vessel, and at the same time, the fiber layer is tightly crocheted to reduce the mesh size and enhance its binding force on the balloon body, combined with the fiber layer being cross-threaded and crocheted at both ends of the balloon body to make the fiber layer fit tightly with the tapered area of the balloon body, and under the action of the dense glue layer, the risk of sliding of the fiber layer is avoided, thereby ensuring the pressure resistance of the pressure-resistant balloon. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A schematic diagram of the structure of a pressure-resistant balloon provided in an embodiment of the present invention;
[0029] Figure 2 for Figure 1 A schematic cross-sectional view of the bureau;
[0030] Figure 3 for Figure 1 Lateral magnified view of area A;
[0031] Figure 4 This is a schematic diagram of the crocheted structure on the front side of the fiber layer;
[0032] Figure 5 This is a schematic diagram of the crochet structure on the reverse side of the fiber layer;
[0033] Figure 6 It is a schematic diagram of a single-sided crochet structure of a fiber layer with one front and one back;
[0034] Figure 7 It is a schematic diagram of the double-sided crochet structure of the fiber layer;
[0035] Figure 8 This is a performance test table of the embodiments of the present invention and the comparative examples;
[0036] Fig. 9 Schematic diagram of spraying glue on the balloon body and the fiber layer in the air pressure atomization device;
[0037] Fig.10 It is a schematic diagram of the curing action of the balloon body in the curing device after the glue is sprayed;
[0038] Fig.11 A schematic diagram of the structure of a balloon dilatation catheter provided in an embodiment of the present invention;
[0039] Among them, 10-balloon body; 20-fiber layer; 30-glue layer;
[0040] 400-terminal tube; 500-catheter; 600-pressure-resistant balloon; 700-Y-shaped connector; 800-developing device; 910-air pressure atomizing device; 920-curing device; 930-ultraviolet lamp. DETAILED DESCRIPTION
[0041] The core of the present invention is to disclose a pressure-resistant balloon to improve the pressure-resistant performance of the balloon on the basis of ensuring the balloon's intravascular passability.
[0042] Another core of the present invention is to provide a method for preparing the above-mentioned pressure-resistant balloon.
[0043] Another core of the present invention is to provide a balloon dilatation catheter including the above-mentioned pressure-resistant balloon.
[0044] In order to make the technical personnel in this field better understand the scheme of the present invention, the embodiments of the present invention are described below with reference to the accompanying drawings. In addition, the embodiments shown below do not limit the content of the invention recorded in the claims. In addition, the entire contents of the structures represented by the following embodiments are not limited to those necessary for the solutions of the invention recorded in the claims.
[0045] like Figure 1 , Figure 2 and Figure 3 As shown, the pressure-resistant balloon provided by the embodiment of the present invention includes a balloon body 10, a fiber layer 20 and a glue layer 30, wherein the balloon body 10 is a single-lumen tube extruded by an extruder and is hot-blow molded on a balloon molding machine containing a convex mold, and the two ends of the balloon body 10 are conical configurations to facilitate guidance and movement in the blood vessel, and the fiber layer 20 is sleeved on the outer periphery of the balloon body 10 to utilize the higher strength of the fiber to restrain the balloon, thereby improving the pressure resistance of the balloon body 10 and reducing the deformation of the balloon as much as possible during use to obtain more precise shape control. Specifically, the fiber layer 20 is a fiber bundle formed by twisting multiple fibers, and is made by tightly crocheting to improve the fit between the fiber layer 20 and the balloon body 10 and reduce the risk of collapse of the fiber layer 20 in the conical area on the balloon body 10. At the same time, it is preferred that the fiber layer 20 is tapered at both ends of the balloon body 10 as shown in the figure. Figure 3The cross-threading method shown is used for hooking and fixing to avoid the fiber layer 20 extending too long at both ends to reduce the folding and passing performance of the pressure-resistant balloon; the glue layer 30 is used to bond and fix the balloon body 10 and the fiber layer 20. Preferably, the glue layer 30 is a dense glue layer, and its thickness is not greater than the thickness of the fiber layer, so that the pressure-resistant balloon has better foldability. In a preferred embodiment of the present invention, after the fiber layer 20 is sleeved on the balloon body 10, the atomized glue is evenly sprayed toward the fiber layer 20 through an atomizing device, and in an oxygen-isolated environment The lower curing is achieved by forming a glue layer 30. During the setting process of the glue layer 30, the atomized glue can evenly enter the gap, so that the balloon body 10 and the fiber layer 20 are fixed by the thinner glue layer 30. The glue layer 30 isolates oxygen during the curing process to prevent the oxygen in the air from inhibiting the free radical polymerization reaction of the contacting glue during the curing process, so that the glue monomer can be completely polymerized and cross-linked to form a completely cured product, thereby ensuring the connection effect between the balloon body 10 and the fiber layer 20.
[0046] It should be noted that the glue layer 30 in the embodiment of the present invention is made of materials such as polyurethane, polyurethane acrylate, epoxy acrylate, unsaturated polyester or their composites, and is a UV-curing glue (ultraviolet glue) with both bonding strength and toughness. The UV-curing glue has the advantages of good bonding strength and strong toughness. At the same time, the device for atomizing the glue is a pneumatic atomization device 910 or an ultrasonic atomization device, so that the glue layer 30 is thinner and the curing effect is better, thereby making the pressure-resistant balloon have a smaller folded outer diameter and obtain better permeability in the blood vessel.
[0047] It should be further explained that the balloon body 10 is a polymer material, which includes one or more materials selected from the group consisting of polyvinyl chloride (PVC), polyethylene (PE), polyurethane (TPU), polyamide material (Nylon), polyether block polyamide (Pebax) and polyethylene terephthalate (PET).
[0048] In addition, the fiber layer 20 can be formed by twisting a plurality of fibers to form a fiber bundle and then weaving it by a weaving machine, or it can be formed by twisting and weaving a plurality of limiting fibers.
[0049] The pressure-resistant balloon provided by the embodiment of the present invention has a tightly woven outer surface of the balloon body 10, and the fiber layer 20 is cross-threaded at both ends to make the fiber layer 20 have strong integrity and not prone to collapse. Preferably, the fiber layer 20 is evenly sprayed with atomized glue through an atomizing device, and the glue is cured in an oxygen-isolated environment to ensure the polymerization and bonding effect of the glue, and then the balloon body 10 and the fiber layer 20 are bonded and fixed through a thinner glue layer 30, thereby avoiding the glue from leaking. The layer 30 is too thick and affects the folding performance of the balloon, which ensures the passability of the balloon in the blood vessel. At the same time, the tightly crocheted fiber layer 20 can reduce the mesh size and enhance its binding force on the balloon body 10. The fiber layer 20 is cross-threaded and crocheted at both ends of the balloon body 10 to make the fiber layer 20 fit tightly with the tapered area of the balloon body 10. The dense glue layer 30 avoids the risk of sliding of the fiber layer 20, thereby ensuring the pressure resistance of the pressure-resistant balloon.
[0050] Furthermore, in order to improve the pressure resistance of the fiber layer 20, in a specific embodiment of the present invention, the fiber bundle used for crocheting the fiber layer 20 is made of extremely fine high-strength fibers, and the diameter of a single fiber is 0.010mm-0.030mm, and the tensile strength is 3.0GPa-4.0GPa. At the same time, the number of fibers in a single strand of the fiber bundle is 3-20, and the twist degree is 10-50, so that the prepared fiber layer 20 meets the required pressure resistance effect. It should be noted that the extremely fine high-strength fiber material used in the embodiment of the present invention is a high-strength fiber composite of one or more materials selected from polyparaphenylene terephthalamide fiber, aromatic polyamide copolymer fiber, heterocyclic polyamide fiber, carbon fiber, graphite fiber, and silicon carbide fiber.
[0051] In order to further optimize the above technical solution, in the pressure-resistant balloon provided by the present invention, the fiber layer 20 is tightly woven in a specific manner as follows: the woven mesh of the fiber layer 20 is 200 μm-800 μm to ensure the structural strength of the fiber layer 20. At the same time, the fiber layer 20 is woven by a woven loom, and each bundle of fibers is woven and interwoven with each other to form a woven net. The woven method is the same to prevent the fiber layer 20 from sliding and loosening when woven on the cone of the balloon. The woven method can be as follows: Figure 4 The front crocheted as shown, Figure 5 Crochet on the reverse side as shown. Figure 6 One side crochet or as shown Figure 7 One of the two crocheted front and back patterns shown.
[0052] It should be noted that if Figure 4-7 As shown in the figure, the shaded area is intended to indicate the direction of a single fiber, see Figure 4 ,by Figure 4Taking the fibers in the shaded part as an example, in the front crocheting form, a single fiber extends out peak-shaped protrusions on both sides in its extension direction. When observed from the side of the fiber layer 20 away from the balloon body 10 toward the balloon body 10, a single protrusion structure passes through the fiber and goes back to the bottom of the two protrusion structures at adjacent positions with the same structure. The protrusion structures on both sides of the shaded fiber are like this, and several protrusion structures in adjacent fibers also pass through the bottom of the peak protrusions of fibers at other positions, so that when various areas in the fiber layer 20 are subjected to the expansion of the balloon body 10, the tension will be transmitted sequentially in a single direction without stress concentration at some positions to damage the fiber layer 20, thereby improving the pressure resistance of the fiber layer 20; and refer to Figure 5 , the reverse side crochet method is the same as Figure 4 The structure of the front crochet method is opposite to that of the reverse crochet method. Each time the fiber passes through, a peak-shaped protrusion structure formed by bending will pass through the fiber at an adjacent position. The tops of two adjacent protrusion structures have the same effect as the front crochet method. When the various areas in the fiber layer 20 are subjected to the expansion of the balloon body 10, the tensioning force is transmitted unidirectionally and quickly, thereby reducing the risk of collapse of the fiber layer 20 in the conical area of the balloon body 10.
[0053] Further, see Figure 6 In the hook weaving method of one front and one back single-sided hook weaving, as shown in the shaded fiber layer, the peak-shaped structure on one side will alternately pass through the top and bottom of the raised structure in the adjacent fiber, while the raised structure on the opposite side will pass through the middle of the two raised edges of the adjacent fiber. Figure 4 The front side of the crocheted Figure 5 The reverse crochet is more complicated, but the alternating positive and negative patterns make it more integrated and have a higher structural strength. When the balloon body 10 is expanded, the pressure resistance is higher and it is not easy to cause damaging deformation. Figure 7 The double-sided crochet method is to connect the raised structures on the opposite sides of a single fiber by passing them through the top and bottom of the adjacent fibers. Figure 6 The hook method of the middle-front-back single-sided hook is similar. Figure 6 The threading method of the raised structure on one side is changed. Figure 6 The single-sided crochet method of middle-front-back has better deformation ability and strong pressure resistance. The fiber layer 20 is not easily damaged when expanding, thereby improving the pressure resistance of the fiber layer 20.
[0054] Furthermore, in the pressure-resistant balloon provided in an embodiment of the present invention, the fiber layer 20 is crocheted directly on the outer wall of the balloon body 10 in an inflated state by a crochet machine, or it can be crocheted separately on a mold and then installed on the outer wall of the balloon after the crocheting is completed. The size and tightness of the mesh of the fiber layer 20 can be controlled by adjusting the number of needles and speed of the crocheting density.
[0055] Based on the above embodiments, the hooking position of the fiber layer 20 can be starting from the tube leg 1mm-20mm away from the balloon body 10 or the mold cone, and ending at the tube leg 1mm-20mm away from the cone at the other end of the balloon body 10 or the mold, or it can be crocheted from the balloon body 10 or the mold cone to the other end cone. After the hooking is completed, the two ends of the tail of the fiber layer 20 are trimmed, and cross-threading is performed to complete the finishing treatment of the hooking of the fiber layer 20, so that the two ends of the fiber layer 20 are in full contact with the balloon body 10 to prevent curling.
[0056] Furthermore, in order to improve the permeability and flexibility of the pressure-resistant balloon provided by an embodiment of the present invention in a blood vessel, the pressure-resistant balloon also includes a lubricating layer. The lubricating layer is an elastic film or a lubricating coating coated on the balloon body 10 when it is in an inflated state. The thickness of the elastic film or the lubricating coating is preferably 0.01mm-0.03mm to avoid the balloon body 10 being too large after folding after the lubricating layer is set, thereby affecting its permeability. It should be noted that the elastic film is preferably composed of a tough polymer material such as polyurethane and silicone film, and the lubricating coating can be a hydrophilic coating or a hydrophobic coating. The lubricating coating includes polyvinyl pyrrolidone (PVP), polyurethane, a copolymer of polyvinyl pyrrolidone and polyurethane, polytetrafluoroethylene (PTFE), silicone, silicone oil, etc.
[0057] Furthermore, in the pressure-resistant balloon provided in the embodiment of the present invention, the inner diameter of the balloon body 10 is 1.0 mm-40.0 mm, and the length is 10 mm-300 mm.
[0058] The present invention also provides a preparation method, which is used to prepare the pressure-resistant balloon provided in any of the above embodiments, and the preparation method at least comprises the following steps:
[0059] S01: Crocheting the fiber layer: The fiber layer 20 is crocheted by a crochet loom in the middle cylindrical area of the balloon body 10. The fiber layer 20 is closely crocheted to avoid collapse. The fiber layer 20 is cross-threaded at the tapered positions at both ends of the balloon body 10 to tighten the fiber layer 20 and avoid curling.
[0060] S02: Spraying a glue layer: spraying the atomized glue evenly toward the fiber layer 20 through an atomizing device, and curing it in an oxygen-isolated environment to form a glue layer 30 .
[0061] Furthermore, in the above-mentioned preparation method, in step S02, it is preferred that the balloon body 10 is sprayed with atomized glue after plasma treatment, and cured for 2min-5min under nitrogen protection or vacuum environment to form a glue layer 30. Specifically, in a specific embodiment of the present invention, in order to ensure the bonding and fixing effect of the glue layer 30 on the fiber layer 20 and the balloon body 10, it is preferred that the balloon body 10 is plasma treated and then sprayed with atomized glue, and after the glue spraying is completed, it is cured for 2min-5min under nitrogen protection or vacuum environment to form a glue layer 30. It should be noted that the purpose of plasma treatment is to make the balloon body 10 The surface of the body 10 is attached with polar groups, thereby increasing the adhesion performance between the balloon body 10 and the fiber layer 20. Specifically, the cleaning machine used for plasma treatment is not particularly limited. The gas selected by the plasma cleaning machine can be air, oxygen, argon, argon-hydrogen mixed gas, etc. The gas volume is preferably 50sccm-180sccm, the power of the plasma cleaning machine is preferably 250W-550W, and the processing time is preferably 100s-500s. The balloon body 10 after plasma treatment is subjected to oxygen-isolating treatment such as passing inert gas or vacuuming in the curing device 920, and then cured for 2min-5min to form a glue layer 30.
[0062] On the basis of the above embodiments, a specific embodiment of the present invention is described in combination with a comparative example, and the specific embodiment is as follows:
[0063] The pressure-resistant balloon provided in this embodiment includes a balloon body 10, a fiber layer 20 and a glue layer 30, wherein the balloon body 10 is made of a single-lumen tube extruded from nylon (PA) as a raw material and is hot-blow molded on a balloon molding machine with a convex mold, and the fiber layer 20 has a structure as shown in FIG. Figure 1 As shown, after the balloon body 10 is filled, both ends of the tube legs are sealed to reduce the deformation of the pressure-resistant balloon when subjected to external force. The filled balloon body 10 is placed horizontally on a crochet machine, and three poly(p-phenylene terephthalamide) fibers with a wire diameter of 0.013 mm are selected. The balloon body 10 is crocheted while being twisted. The twist of the fiber bundle is 30. The crocheting work starts from the tube leg 5-10 mm away from the cone of the balloon body 10, and ends at the tube leg 5-10 mm away from the cone at the other end of the balloon body 10. The size and tightness of the mesh of the fiber layer 20 are controlled by adjusting the number of needles and speed of the crocheting density, so that the mesh size of the fiber layer 20 is 300±50μm to ensure that the fibers are tightly wrapped on the outer surface of the balloon. Figure 4 After the weaving is completed, the two ends of the fiber layer 20 are trimmed and the following steps are performed: Figure 3 The cross-threading process shown in the figure is then further performed to finish the weaving of the fiber layer 20, so that both ends of the fiber layer 20 are closely attached to the balloon body 10 to prevent the curling edge from warping; Figure 2The glue layer 30 shown is a method of first plasma treating the surface of the crocheted balloon body 10 with argon gas of 100 sccm, power of 300 W, and treatment time of 100 s to make the balloon surface have polar groups to increase the adhesion performance of the balloon body 10 and the fiber, and then placing the plasma treated balloon on a surface such as Fig. 9 The air pressure atomization device 910 shown in the figure adjusts the movement parameters according to the shape of the balloon body 10, and the glue is evenly coated on the balloon through air pressure atomization, and then the balloon sprayed with glue is placed on the Fig.10 In the curing device 920 shown, nitrogen is introduced for nitrogen protection and thus oxygen is isolated, and then it is irradiated by an ultraviolet lamp 930 for 3 minutes to solidify it to form a glue layer 30. On this basis, the surface of the pressure-resistant balloon in the filled state is coated with a silicone oil coating to further increase the flexibility and permeability of the pressure-resistant balloon. The coating thickness is about 0.01 mm.
[0064] The pressure-resistant balloon prepared in the above embodiment is used as an embodiment sample, and three burst pressure performance tests are carried out. At the same time, comparative examples 1-4 under different process treatments are set for performance test comparison. Three samples are provided for each comparative example for testing. The performance test results are shown in the attached Figure 8 , wherein the preparation process of each comparative example is as follows:
[0065] Comparative Example 1:
[0066] The fiber layer 20 with a mesh size of 2000±50 μm is woven in the same manner as in the above embodiment and coated on the outer wall of the balloon body 10 , and the other process steps are the same;
[0067] Comparative Example 2:
[0068] Nylon fibers with a diameter of 0.056 mm are selected to be woven and bonded in the manner of the above embodiment and made into pressure-resistant balloons of the same specifications, and the other process steps are the same;
[0069] Comparative Example 3:
[0070] Without plasma treatment, the fiber layer 20 and the balloon body 10 are bonded with ethyl cyanoacrylate instant glue, and the other process steps are the same;
[0071] Comparative Example 4:
[0072] A balloon of the same specification is made by using the balloon body 10 without being covered with the fiber layer 20 , and the process steps of the balloon body 10 are the same as those in the embodiment.
[0073] By attaching Figure 8It can be seen from the comparison results in that the fiber material selected in this embodiment, the mesh density of the fiber layer 20 and the processing method of the balloon body 10 can enable the pressure-resistant balloon to have the strongest pressure resistance performance while having a smaller size and permeability.
[0074] like Fig.11 As shown, the present invention also provides a balloon dilatation catheter, which includes a terminal tube 400, a catheter 500 and a pressure-resistant balloon 600 provided in any of the above embodiments. Specifically, the pressure-resistant balloon 600 is arranged between the terminal tube 400 and the catheter 500, the terminal tube 400 is not connected to the pressure-resistant balloon 600, the pressure-resistant balloon 600 is connected to the catheter 500, and an inner tube with one end connected to the terminal tube 400 is arranged in the pressure-resistant balloon 600.
[0075] At the same time, a guide wire is passed through the terminal tube 400, the inner tube and the catheter 500. The guide wire is inserted from the terminal tube 400, passes through the inner tube of the pressure-resistant balloon 600, reaches the proximal end of the pressure-resistant balloon 600, and then enters the catheter 500. It should be noted that in the embodiment of the present invention, the inner diameter of the inner tube is not less than 0.3 mm, which can allow three specifications of guide wires of 0.014 inches, 0.018 inches and 0.035 inches to pass through. The end of the inner tube connected to the terminal tube 400 is connected to the pressure-resistant balloon 600 to form a sealing point of the balloon cavity. Furthermore, developing devices 800 are provided at both ends of the inner tube. Preferably, the developing device 800 is a developing ring. At the same time, the developing device 800 is preferably arranged at the inner tube position relative to the highest point of the slope when the pressure-resistant balloon 600 is in the expanded state. The developing device 800 is preferably a thin-walled annular structure made of platinum-iridium alloy or other metals and plastics that are opaque to X-rays. The developing device 800 is visible under X-rays and can mark the position of the working area of the pressure-resistant balloon 600 during surgery, so that the surgical staff can smoothly deliver the pressure-resistant balloon 600 to the diseased blood vessel area. The catheter 500 can be a multi-lumen tube, a single-lumen tube, or a multi-lumen tube connected to a single-lumen tube. When the catheter 500 is a single-lumen tube, the catheter 500 is simultaneously connected to the pressure-resistant balloon 600, and the inner tube is preferably located in the cavity of the catheter 500, and the inner tube and the catheter 500 form a coaxial arrangement or a multi-lumen configuration, and the guide wire is in the inner tube; when it is a multi-lumen tube, preferably one of the channels is connected to the inner tube, and the other channels are connected to the pressure-resistant balloon 600.
[0076] Furthermore, the balloon dilatation catheter provided in the embodiment of the present invention is an integral exchange type balloon dilatation catheter or a rapid exchange type balloon dilatation catheter. Specifically, when the balloon dilatation catheter is an integral exchange type, the end of the catheter 500 away from the high-pressure resistant balloon is connected to a Y-shaped connector 700, and the Y-shaped connector 700 includes a guide guide wire outlet and a balloon filling port. The Y-shaped connector 700 cooperates with the catheter 500 to form two channels, namely, a balloon channel for inflating and depressurizing the balloon and a multifunctional channel penetrated by the guide guide wire. When the catheter 500 is a single-lumen tube, the balloon filling port of the Y-shaped connector 700 is connected to the high-pressure resistant balloon through the catheter 500 to form a balloon channel, and the inner tube with a guide guide wire is connected to the guide guide wire outlet to form a multifunctional channel; when the catheter 500 is a multi-lumen tube, the channel with the guide guide wire is connected to the guide guide wire outlet to form a multifunctional channel, and the balloon filling port is connected to the high-pressure resistant balloon through other channels to form a balloon channel.
[0077] It should be noted that the multifunctional channel can be used not only for guiding the passage of the catheter, but also for injecting heparin, contrast agents, etc.
[0078] Furthermore, when the balloon dilatation catheter is a rapid exchange type balloon dilatation catheter, a rapid exchange guidewire port is provided on the catheter 500 at the proximal end of the balloon dilatation catheter, and the catheter 500 is connected to the balloon filling port, the balloon filling port is not connected to the rapid exchange guidewire port, and the distance between the rapid exchange guidewire port and the proximal end of the balloon catheter 500, i.e., the balloon filling port, is preferably 10mm-1000mm. When the catheter 500 is a single-lumen tube, the inner tube with a guide guidewire forms a coaxial arrangement or a multi-lumen configuration in the catheter 500, and the inner tube is connected to the rapid exchange guidewire port provided on the catheter 500; when the catheter 500 is a multi-lumen tube, the channel with the guide guidewire is connected to the rapid exchange guidewire port.
[0079] The terms "left side" and "right side" in the specification and claims of the present invention and the above drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but may include steps or units that are not listed.
[0080] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A pressure-resistant balloon, characterized in that: include: A balloon body (10), wherein both ends of the balloon body (10) are of a conical configuration; A fiber layer (20) and a glue layer (30), wherein the fiber layer (20) is crocheted from a fiber bundle formed by twisting a plurality of fibers, the fiber layer (20) is tightly crocheted and arranged on the outer wall of the balloon body (10), and both ends of the fiber layer (20) are located at the tube legs of the balloon body (10) and cross-threaded and crocheted, and the glue layer (30) is used to bond and connect the balloon body (10) and the fiber layer (20), and the glue layer (30) is a dense glue layer and its thickness is not greater than that of the fiber layer (20); The fiber layer (20) is tightly woven in a specific manner, wherein the aperture of the woven mesh is 200 μm-800 μm, and the woven manner is front woven, back woven, front and back single woven, or front and back double woven.
2. The pressure-resistant balloon according to claim 1, characterized in that: The front hook weaving is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in the first direction, any of the peak configurations passes through the bottoms of two of the peak configurations of the adjacent fiber bundles; The reverse side crochet is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in a second direction, any of the peak configurations passes through the tops of two of the peak configurations of the adjacent fiber bundles, and the second direction is opposite to the first direction; The one-front-one-back single-sided crochet weaving is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, the peak configuration on one side sequentially passes through the top and bottom of the peak configuration in the adjacent fiber bundle, and the top of the peak configuration on the opposite side passes through the middle of the raised edges of the two peak configurations in the adjacent fiber bundle; The front and back double-sided crochet weaving is as follows: the fiber bundle is reciprocatingly bent to form a plurality of adjacent peak configurations, and in the first direction and the second direction, any peak configuration passes through the top and bottom of two peak configurations of the adjacent fiber bundles in sequence.
3. The pressure-resistant balloon according to claim 2, characterized in that: The hooking position of the fiber layer (20) starts from the tube leg 1mm-20mm away from the balloon body (10) or the mold cone and ends at the tube leg 1mm-20mm away from the cone at the other end of the balloon body (10) or the mold, or the hooking position of the fiber layer (20) starts from the balloon body (10) or the mold cone and ends at the cone at the other end.
4. The pressure-resistant balloon according to claim 1, characterized in that: It also includes a lubricating layer, which is an elastic film or a lubricating coating coated on the balloon body (10) when it is in a pressurized state.
5. A preparation method for preparing the pressure-resistant balloon according to any one of claims 1 to 4, the preparation method comprising at least the following steps: Crocheting the fiber layer: the fiber layer (20) is crocheted in the middle cylindrical region of the balloon body (10) by a crochet loom, the fiber layer (20) is closely fitted and tightly crocheted to avoid collapse, and the fiber layer (20) is cross-threaded at the tapered positions at both ends of the balloon body (10) to tighten the fiber layer (20) and avoid curling; Spraying the glue layer: spraying the atomized glue evenly toward the fiber layer (20) through an atomizing device, and curing in an oxygen-isolated environment to form the glue layer (30).
6. The preparation method according to claim 5, characterized in that: In the step of spraying the glue layer, the balloon body (10) is sprayed with atomized glue after plasma treatment, and is cured for 2 minutes to 5 minutes under nitrogen protection or vacuum environment to form the glue layer (30).
7. The preparation method according to claim 5, characterized in that: The processing gas used in the plasma treatment process of the balloon body (10) is air, oxygen, argon or argon-hydrogen mixed gas, and the gas volume is 50-180 sccm.
8. A balloon dilatation catheter, characterized in that: It comprises a terminal tube (400), a catheter (500), and the pressure-resistant balloon (600) according to any one of claims 1 to 4, wherein the pressure-resistant balloon (600) is arranged between the terminal tube (400) and the catheter (500).