Self-leveling colored sand and its production process

By modifying the epoxy resin with functional fillers and composite additives, the interpenetrating network structure and oxidation resistance are formed, and the performance problems of self-leveling color sand in high load and oxidation environments are solved, which significantly improves wear resistance and resistance Oxidation performance extends service life.

CN118405869BActive Publication Date: 2024-11-12GUANGZHOU DIMEI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410602078.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2024-11-12
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Self-leveling colored sand occurs indentation, wear and peeling when it is subjected to heavy loads, strong impact and frequent friction, and color changes and performance deteriorates due to oxidation.

Method used

20 to 40 parts of epoxy resin, 10 to 15 parts of talc powder, 4 to 8 parts of functional filler, 8 to 10 parts of colored sand, 0.4 to 0.8 parts of glyceryl tristearate, 1 to 3 parts of phthalic acid The formula of dioctyl ester, 0.3 to 0.7 parts of polybutyl acrylate, 0.4 to 0.6 parts of hydrogenated castor oil, 1 to 2 parts of polyoxyethylene polyoxypropylene pentaerythritol ether, and the basalt fiber and end vinyl fluoride are treated through specific processes. Silicone oil is surface modified to prepare functional fillers and composite additives to form an interpenetrating network structure and antioxidant properties.

Benefits of technology

It significantly improves the wear resistance, mechanical strength and oxidation resistance of self-leveling colored sand, extends its service life, avoids color changes and performance degradation caused by oxidation, and enhances market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118405869B_ABST
    Figure CN118405869B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building material preparation, and discloses a self-leveling colored sand and a production process thereof. The self-leveling colored sand comprises the following raw materials: epoxy resin, talcum powder, functional filler, composite additive, colored sand, glyceryl tristearate, dioctyl phthalate, polybutyl acrylate, hydrogenated castor oil, and polyoxyethylene polyoxypropylene pentaerythritol ether; wherein the functional filler is prepared by grafting terminal hydroxyl polyether sulfone onto the surface of basalt fiber, so that the prepared self-leveling colored sand has excellent mechanical properties and wear resistance; the composite additive is prepared by introducing amide groups into the structure of terminal vinyl fluorinated silicone oil, so that the composite additive can undergo curing reaction with an epoxy resin matrix, and can improve the leveling performance of the self-leveling colored sand, enhance its oxidation resistance, and prolong the service life of the self-leveling colored sand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material preparation, and in particular to self-leveling colored sand and a production process thereof. Background Art

[0002] Self-leveling colored sand is a high-performance building decoration material with rich colors, moisture-proof, anti-corrosion and other excellent properties. It is widely used in various places, such as industrial plants, hospitals, schools, shopping malls, squares, etc. Among them, epoxy self-leveling colored sand has more superior decorative and usage functions. It is composed of epoxy resin, colored sand filler, additives, etc. Through specific construction technology, it can form a smooth, seamless and beautiful effect.

[0003] In the current environment where infrastructure is becoming increasingly perfect, self-leveling colored sand is the main building decoration material, and the demand is increasing day by day. This puts higher requirements on the performance and quality of self-leveling colored sand to meet market demand. First of all, self-leveling colored sand must be able to withstand various pressures and frictions. In places with dense traffic, such as shopping malls and hospitals, the ground materials need to withstand the trampling of a large number of people and the movement of objects. Mechanical equipment and heavy objects in industrial sites may also cause impact and oppression on the ground. Therefore, self-leveling colored sand needs to have sufficient pressure resistance, impact resistance and wear resistance to ensure the stability, durability and safety of the ground. In addition, in high-temperature and high-pressure industrial environments, such as smelting, combustion and other industrial processes, they are often accompanied by extremely high temperatures and pressures. Such extreme conditions will significantly enhance the activity of oxygen and other oxidants, thereby forming a strong oxidizing environment. In such an environment, self-leveling colored sand faces the risk of color change or performance degradation due to oxidation. Therefore, it is very important to improve the antioxidant properties of self-leveling colored sand, which can effectively delay the oxidation process and ensure that self-leveling colored sand can maintain lasting color brightness and stable performance in a strong oxidizing environment.

[0004] The patent with publication number CN107586504B discloses a floating colored sand self-leveling floor coating and a preparation method thereof. The invention adopts two specific BPA-type epoxy resins (bimodal molecular weight distribution), BGE diluted epoxy resin and a specific modified alicyclic amine curing agent as the main film-forming substances of the system, and cooperates with specially designed sintered floating colored sand aggregates to significantly improve the compressive strength, flexural strength, wear resistance and other physical and mechanical properties of the floating colored sand self-leveling surface layer. Based on this, the present invention has developed a self-leveling colored sand with excellent mechanical properties and antioxidant properties, which is of great significance. Summary of the invention

[0005] The purpose of the present invention is to provide a self-leveling colored sand and a production process thereof, which solves the following technical problems:

[0006] (1) It solves the problem that self-leveling colored sand will be indented, worn, peeled off, etc. due to excessive load, strong impact and frequent friction;

[0007] (2) The problem of self-leveling colored sand changing color and deteriorating performance due to oxidation has been solved.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] A self-leveling colored sand comprises the following raw materials in parts by weight: 20-40 parts of epoxy resin, 10-15 parts of talc, 4-8 parts of functional fillers, 8-10 parts of composite additives, 10-30 parts of colored sand, 0.4-0.8 parts of tristearic acid glyceryl, 1-3 parts of dioctyl phthalate, 0.3-0.7 parts of polybutyl acrylate, 0.4-0.6 parts of hydrogenated castor oil, and 1-2 parts of polyoxyethylene polyoxypropylene pentaerythritol ether.

[0010] Furthermore, the preparation method of the functionalized filler comprises the following steps:

[0011] S1: placing the basalt fiber in an acetone solution, soaking for 30 to 50 minutes, taking it out and washing it with deionized water for 4 to 6 times to remove surface impurities, and then drying it in an oven at 70 to 90° C. for 2 to 4 hours to obtain pretreated basalt fiber;

[0012] S2: adding deionized water and anhydrous ethanol into the reactor, mixing evenly, adding 3-chloropropyltrimethoxysilane, stirring evenly, and then adding the pretreated basalt fiber, reacting at 50-60° C. for 1-2 hours, discharging, centrifuging and separating the solid material, washing, and drying to obtain halogenated basalt fiber;

[0013] S3: Disperse the halogenated basalt fiber in N,N-dimethylformamide to form a uniform suspension, add the terminal hydroxyl polyether sulfone and the accelerator to the suspension under stirring conditions, stir and mix evenly, and heat-treat at a temperature of 60 to 80°C for 4 to 6 hours. After the reaction is completed, filter and collect the product, wash and dry the product to obtain a functional filler.

[0014] Furthermore, in step S1, the diameter of the basalt fiber is 2-8 μm and the length is 1-4 mm.

[0015] Furthermore, in step S3, the accelerator is any one of sodium carbonate, potassium carbonate or sodium bicarbonate.

[0016] Through the above technical scheme, basalt fiber is placed in an acetone solution to remove surface impurities to obtain pretreated basalt fiber, and 3-chloropropyltrimethoxysilane is used to modify the surface of the pretreated basalt fiber, and halogen groups are modified on the surface of the basalt fiber to prepare halogenated basalt fiber. Under the action of a promoter, the halogen chlorine atoms on the surface of the basalt fiber can undergo a nucleophilic substitution reaction with the active hydroxyl groups in the terminal hydroxyl polyether sulfone structure to obtain a functional filler.

[0017] Furthermore, the preparation method of the composite additive comprises the following steps:

[0018] SS1: Add vinyl-terminated fluorinated silicone oil to toluene, stir evenly, then add 2-aminoethanethiol and a photoinitiator, place the system under a UV lamp for 20 to 40 minutes while stirring, and after the reaction is completed, remove the solvent by rotary evaporation to obtain a modified vinyl-terminated fluorinated silicone oil;

[0019] SS2: Mix the modified terminal vinyl fluorinated silicone oil with dimethyl sulfoxide, add ferulic acid, stir mechanically, add activator and condensation agent, and after the addition, stir at room temperature under nitrogen protection for 6 to 12 hours. After the reaction is completed, remove the nitrogen, discharge the material, and obtain a composite additive.

[0020] Furthermore, in step SS1, the photoinitiator is any one of benzoin ethyl ether, benzoin isopropyl ether or benzoin dimethyl ether.

[0021] Furthermore, in step SS1, the mass ratio of the vinyl-terminated fluorinated silicone oil to 2-aminoethanethiol is 1:0.1-0.4.

[0022] Furthermore, in step SS2, the activator is any one of 4-dimethylaminopyridine, N-hydroxysuccinimide or 1-hydroxybenzotriazole.

[0023] Furthermore, in step SS2, the condensing agent is any one of N,N-dicyclohexylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide or N,N'-diisopropylcarbodiimide.

[0024] Through the above technical scheme, benzoin isopropyl ether is used as a photoinitiator, under the condition of ultraviolet light irradiation, the unsaturated olefinic functional group in the structure of the terminal vinyl fluorinated silicone oil and the thiol group in the structure of 2-aminoethanethiol can be induced to undergo a click reaction, thereby introducing an amino group into the structure of the terminal vinyl fluorinated silicone oil to obtain a modified terminal vinyl fluorinated silicone oil. Under the joint action of an activator and a condensation agent, the active amino group in the structure of the modified terminal vinyl fluorinated silicone oil can react with the carboxyl group in the structure of ferulic acid to obtain a composite additive.

[0025] A process for producing self-leveling colored sand comprises the following steps:

[0026] (1) Add epoxy resin, talcum powder, functional filler and composite additives into a high-speed mixer and stir at high speed, control the stirring speed to 500-700 r / min, the stirring temperature to 40-60° C., stir for 20-40 min to obtain a premix;

[0027] (2) Add colored sand, tristearate, dioctyl phthalate, polybutyl acrylate, hydrogenated castor oil and polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 30 to 50 minutes to obtain self-leveling colored sand.

[0028] Beneficial effects of the present invention:

[0029] (1) The present invention prepares functionalized fillers as filler modifiers for colored sand. After organic modification, the interfacial compatibility between basalt fiber and epoxy resin matrix is ​​effectively improved, and the negative impact of basalt fiber agglomeration is avoided. Since the functionalized fillers contain active hydroxyl groups, the active hydroxyl groups can interact with the epoxy resin matrix, so that an interpenetrating network structure is formed between the functionalized fillers and the epoxy resin matrix, which can effectively limit the movement of the epoxy resin molecular chains, so that the prepared colored sand has high cohesion and density, and improves the wear resistance and mechanical strength of the colored sand. At the same time, the basalt fibers in the functionalized fillers can absorb stress and hinder the expansion of stress cracks, which can further improve the mechanical properties of the colored sand. In addition, the terminal hydroxyl polyether sulfone in the functionalized fillers can improve the toughness of the colored sand, so that the colored sand can better resist deformation or fracture when subjected to external forces, thereby extending its service life.

[0030] (2) The present invention participates in the preparation process of self-leveling colored sand by preparing a composite additive. Since the composite additive contains an amide group in its structure, it can be used as a curing agent to undergo a curing reaction with the epoxy resin matrix material, thereby improving the interface properties of the components in the matrix material and avoiding the problem of performance loss of the self-leveling colored sand due to phase separation. In addition, the composite additive contains siloxane segments and fluorine atoms, which can greatly reduce the surface tension of the polymer, making it easier to wet the substrate, improve the leveling performance of the colored sand, and provide an excellent smoothing effect. In addition, the introduction of ferulic acid can effectively improve the antioxidant properties of the colored sand, avoid fading, discoloration, performance degradation, etc. of the colored sand due to oxidation, reduce maintenance costs, extend the service life of the colored sand, and enhance its market competitiveness.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0033] Figure 1 This is a scanning electron microscope image of the basalt fiber and functionalized filler prepared in Example 1 of the present invention.

[0034] Figure 2 This is an infrared spectrum test chart of the modified vinyl-terminated fluorinated silicone oil and the composite additive prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] 1. Preparation of functionalized fillers

[0038] S1: 5 g of basalt fiber with a diameter of 4 μm and a length of 1 mm was placed in 150 ml of acetone solution and soaked for 40 min. After being taken out, it was washed with deionized water for 5 times to remove surface impurities, and then dried in an oven at 80 ° C for 3 h to obtain pretreated basalt fiber;

[0039] S2: Add 50 ml of deionized water and 65 ml of anhydrous ethanol into the reactor, mix well, add 0.3 g of 3-chloropropyltrimethoxysilane, stir well, add 10 g of basalt fiber, react at 55 ° C for 1.5 h, discharge, centrifuge and separate the solid material, wash and dry to obtain halogenated basalt fiber;

[0040] S3: Disperse 5 g of halogenated basalt fiber in 100 ml of N,N-dimethylformamide to form a uniform suspension, add 4.2 g of terminal hydroxyl polyethersulfone and 0.1 g of potassium carbonate to the suspension under stirring conditions, stir and mix evenly, and keep warm at 70°C for 5 hours. After the reaction is completed, filter and collect the product, wash and dry the product to obtain a functional filler.

[0041] The morphology of basalt fiber and functional filler was analyzed using a Hitachi SU8010 scanning electron microscope. The test results are shown in Figure 1, where A is basalt fiber and B is functional filler. As can be seen from the figure, the surface of basalt fiber is smooth, while the surface of functional filler is rough. This is because the end-hydroxyl polyether sulfone is grafted onto the surface of basalt fiber.

[0042] 2. Preparation of composite additives

[0043] SS1: Add 5 g of vinyl-terminated fluorinated silicone oil to toluene and stir evenly. Then add 0.78 g of 2-aminoethanethiol and 0.05 g of benzoin isopropyl ether. Under stirring, place the system under a 365 nm ultraviolet lamp for 30 min. After the reaction is completed, remove the solvent by rotary evaporation to obtain modified vinyl-terminated fluorinated silicone oil.

[0044] SS2: Mix 5g of modified terminal vinyl fluorinated silicone oil with dimethyl sulfoxide, add 1.2g of ferulic acid, stir mechanically, add 0.1g of N-hydroxysuccinimide and 0.08g of N,N-dicyclohexylcarbodiimide, and after the addition, stir at room temperature for 8h under nitrogen protection. After the reaction is completed, remove the nitrogen, discharge the material, and obtain a composite additive.

[0045] The modified vinyl-terminated fluorinated silicone oil and composite additives were tested by infrared spectrometer Nicolet Magna-Avatar 360. Figure 2 As shown in the figure, the analysis shows that in the infrared spectrum of the modified vinyl-terminated fluorinated silicone oil, 676 cm -1 The characteristic absorption peak of CS appears at 1023cm -1 The characteristic absorption peak of Si-O appears at 1216cm -1 The characteristic absorption peak of CF appears at 3345cm -1 The characteristic absorption peak of NH in the amino group appears at 655cm. This is because the unsaturated olefin group in the structure of the terminal vinyl fluorinated silicone oil can undergo a click reaction with the thiol group in the structure of 2-aminoethanethiol, thereby introducing an amino group into the structure of the terminal vinyl fluorinated silicone oil to obtain a modified terminal vinyl fluorinated silicone oil. In the infrared spectrum of the composite additive, 655cm -1 The characteristic absorption peak of CS appears at 3282cm -1 The characteristic absorption peak of the hydroxyl group appears at 1097 cm -1 The characteristic absorption peak of ether bond COC appears at 3135cm -1 The absorption peak of NH in the amide bond is 1656 cm -1 The absorption peak at the center is the C=O absorption peak in the amide bond. This is because the active amino group in the structure of the modified terminal vinyl fluorinated silicone oil can react with the carboxyl group in the ferulic acid structure to produce a composite additive.

[0046] 3. Preparation of self-leveling colored sand

[0047] (1) Add 20 g of E51 epoxy resin, 10 g of talcum powder, 4 g of functional filler, and 8 g of composite additives into a high-speed mixer and stir at high speed. Control the stirring speed to 500 r / min and the stirring temperature to 40°C for 20 min to obtain a premix.

[0048] (2) Add 10 g of colored sand, 0.4 g of tristearate, 1 g of dioctyl phthalate, 0.3 g of polybutyl acrylate, 0.4 g of hydrogenated castor oil and 1 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 30 min to obtain self-leveling colored sand.

[0049] Example 2

[0050] Preparation of self-leveling colored sand

[0051] (1) Add 30 g of E51 epoxy resin, 12 g of talcum powder, 6 g of functional filler, and 9 g of composite additives into a high-speed mixer and stir at high speed. Control the stirring speed to 600 r / min and the stirring temperature to 50°C for 30 min to obtain a premix.

[0052] (2) Add 20 g of colored sand, 0.6 g of tristearate, 2 g of dioctyl phthalate, 0.5 g of polybutyl acrylate, 0.5 g of hydrogenated castor oil and 1.5 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 40 min to obtain self-leveling colored sand.

[0053] The preparation method of the functional filler and the composite additive is the same as that in Example 1.

[0054] Example 3

[0055] Preparation of self-leveling colored sand

[0056] (1) Add 40 g of E51 epoxy resin, 15 g of talcum powder, 8 g of functional filler, and 10 g of composite additives into a high-speed mixer and stir at high speed. Control the stirring speed to 700 r / min and the stirring temperature to 60°C for 40 min to obtain a premix.

[0057] (2) Add 30 g of colored sand, 0.8 g of tristearate, 3 g of dioctyl phthalate, 0.7 g of polybutyl acrylate, 0.6 g of hydrogenated castor oil and 2 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 50 min to obtain self-leveling colored sand.

[0058] The preparation method of the functional filler and the composite additive is the same as that in Example 1.

[0059] Comparative Example 1

[0060] Preparation of self-leveling colored sand

[0061] (1) Add 30 g of E51 epoxy resin, 12 g of talcum powder, and 6 g of functionalized filler into a high-speed mixer and stir at high speed. Control the stirring speed to 600 r / min and the stirring temperature to 50°C for 30 min to obtain a premix.

[0062] (2) Add 20 g of colored sand, 0.6 g of tristearate, 2 g of dioctyl phthalate, 0.5 g of polybutyl acrylate, 0.5 g of hydrogenated castor oil and 1.5 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 40 min to obtain self-leveling colored sand.

[0063] The preparation method of the functionalized filler is the same as that in Example 1.

[0064] Comparative Example 2

[0065] Preparation of self-leveling colored sand

[0066] (1) Add 30 g of E51 epoxy resin, 12 g of talcum powder, and 9 g of composite additives into a high-speed mixer and stir at high speed. Control the stirring speed to 600 r / min and the stirring temperature to 50°C for 30 min to obtain a premix.

[0067] (2) Add 20 g of colored sand, 0.6 g of tristearate, 2 g of dioctyl phthalate, 0.5 g of polybutyl acrylate, 0.5 g of hydrogenated castor oil and 1.5 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 40 min to obtain self-leveling colored sand.

[0068] The preparation method of the composite additive is the same as that in Example 1.

[0069] Comparative Example 3

[0070] Preparation of self-leveling colored sand

[0071] (1) Add 30 g of E51 epoxy resin, 12 g of talc, 3 g of basalt fiber, 3 g of hydroxyl-terminated polyethersulfone, and 9 g of composite additives into a high-speed mixer and stir at high speed. Control the stirring speed to 600 r / min and the stirring temperature to 50°C for 30 min to obtain a premix.

[0072] (2) Add 20 g of colored sand, 0.6 g of tristearate, 2 g of dioctyl phthalate, 0.5 g of polybutyl acrylate, 0.5 g of hydrogenated castor oil and 1.5 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 40 min to obtain self-leveling colored sand.

[0073] The preparation method of the composite additive is the same as that in Example 1.

[0074] Comparative Example 4

[0075] Preparation of self-leveling colored sand

[0076] (1) Add 30 g of E51 epoxy resin and 12 g of talcum powder into a high-speed mixer and stir at high speed. Control the stirring speed to 600 r / min and the stirring temperature to 50°C for 30 min to obtain a premix.

[0077] (2) Add 20 g of colored sand, 0.6 g of tristearate, 2 g of dioctyl phthalate, 0.5 g of polybutyl acrylate, 0.5 g of hydrogenated castor oil and 1.5 g of polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 40 min to obtain self-leveling colored sand.

[0078] Performance Testing

[0079] ① The self-leveling colored sand prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was evenly coated on a tinplate that met the specifications to prepare a sample, and the flexibility of the sample was tested according to GB / T1731-2020 "Determination of Flexibility of Paint Film and Putty Film"; the compressive strength performance of the sample was tested according to GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)"; the impact resistance of the sample was tested according to GB / T 1732-2020 "Determination of Impact Resistance of Paint Film"; the wear resistance of the sample was tested according to GB / T1768-2006 "Determination of Wear Resistance of Paint and Varnish - Rotating Rubber Grinding Wheel Method", and the specific test results are shown in the following table:

[0080] ,

[0081] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 and Comparative Example 1 have excellent mechanical properties, flexibility and wear resistance; no functional filler was added to the samples prepared in Comparative Example 2 and Comparative Example 4, and the values ​​were greatly reduced compared with the embodiments, and the mechanical properties, flexibility and wear resistance of the samples were poor; basalt fiber and terminal hydroxyl polyether sulfone were added to the sample prepared in Comparative Example 3, and the mechanical properties, flexibility and wear resistance of the sample were average. It is speculated that in the preparation process of self-leveling colored sand, the compatibility between basalt fiber and matrix material is poor, and it cannot be evenly dispersed in the matrix, resulting in a decrease in the performance of the sample.

[0082] ② The self-leveling colored sand prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was tested for fluidity according to JB-T3998-1999 "Determination of coating leveling properties by scraping"; the self-leveling colored sand prepared in Examples 1 to 3 and Comparative Examples 1 to 4 was evenly coated on a tinplate that met the specifications to prepare a sample, and the sample was placed in an oven at 150° C. for 72 hours to observe whether the surface showed yellowing, blistering, cracks, etc. The specific test results are shown in the following table:

[0083] ,

[0084] From the test results in the above table, it can be seen that the samples prepared in Examples 1 to 3 and Comparative Examples 2 to 3 have good leveling performance and antioxidant properties. No composite additives were added to the samples prepared in Comparative Examples 1 and 4. Compared with the examples, the samples showed blistering and yellowing, and the leveling grade decreased. The antioxidant and leveling performance of the samples were average.

[0085] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A self-leveling colored sand, characterized in that: The invention comprises the following raw materials in parts by weight: 20 to 40 parts of epoxy resin, 10 to 15 parts of talc, 4 to 8 parts of functional fillers, 8 to 10 parts of composite additives, 10 to 30 parts of colored sand, 0.4 to 0.8 parts of tristearic acid glyceryl, 1 to 3 parts of dioctyl phthalate, 0.3 to 0.7 parts of polybutyl acrylate, 0.4 to 0.6 parts of hydrogenated castor oil, and 1 to 2 parts of polyoxyethylene polyoxypropylene pentaerythritol ether; The preparation method of the functionalized filler comprises the following steps: S1: placing the basalt fiber in an acetone solution, soaking for 30 to 50 minutes, taking it out and washing it with deionized water for 4 to 6 times to remove surface impurities, and then drying it in an oven at 70 to 90° C. for 2 to 4 hours to obtain pretreated basalt fiber; S2: adding deionized water and anhydrous ethanol into the reactor, mixing evenly, adding 3-chloropropyltrimethoxysilane, stirring evenly, and then adding the pretreated basalt fiber, reacting at 50-60° C. for 1-2 hours, discharging, centrifuging and separating the solid material, washing, and drying to obtain halogenated basalt fiber; S3: Dispersing the halogenated basalt fiber in N,N-dimethylformamide to form a uniform suspension, adding the hydroxy-terminated polyethersulfone and the accelerator to the suspension under stirring conditions, stirring and mixing evenly, and heat-treating at a temperature of 60 to 80° C. for 4 to 6 hours. After the reaction is completed, filtering, collecting the product, washing the product, and drying it to obtain a functional filler; The preparation method of the composite additive comprises the following steps: SS1: Add vinyl-terminated fluorinated silicone oil to toluene, stir evenly, then add 2-aminoethanethiol and a photoinitiator, place the system under a UV lamp for 20 to 40 minutes while stirring, and after the reaction is completed, remove the solvent by rotary evaporation to obtain a modified vinyl-terminated fluorinated silicone oil; SS2: Mix the modified vinyl-terminated fluorinated silicone oil with dimethyl sulfoxide, add ferulic acid, stir mechanically, add activator and condensing agent, stir at room temperature for 6 to 12 hours under nitrogen protection, remove nitrogen after the reaction, discharge the material, and obtain a composite additive; The mass ratio of the vinyl-terminated fluorinated silicone oil to 2-aminoethanethiol is 1:0.1-0.

4.

2. The self-leveling colored sand according to claim 1, characterized in that: In step S1, the diameter of the basalt fiber is 2-8 μm and the length is 1-4 mm.

3. The self-leveling colored sand according to claim 1, characterized in that: In step S3, the accelerator is any one of sodium carbonate, potassium carbonate or sodium bicarbonate.

4. The self-leveling colored sand according to claim 1, characterized in that: In step SS1, the photoinitiator is any one of benzoin ethyl ether, benzoin isopropyl ether or benzoin dimethyl ether.

5. The self-leveling colored sand according to claim 1, characterized in that: In step SS2, the activator is any one of 4-dimethylaminopyridine, N-hydroxysuccinimide or 1-hydroxybenzotriazole.

6. The self-leveling colored sand according to claim 1, characterized in that: In step SS2, the condensing agent is any one of N,N-dicyclohexylcarbodiimide, 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide or N,N'-diisopropylcarbodiimide.

7. A process for producing self-leveling colored sand as claimed in claim 1, characterized in that: The following steps are involved: (1) Add epoxy resin, talcum powder, functional filler and composite additives into a high-speed mixer and stir at high speed, control the stirring speed to 500-700 r / min, the stirring temperature to 40-60° C., stir for 20-40 min to obtain a premix; (2) Add colored sand, tristearate, dioctyl phthalate, polybutyl acrylate, hydrogenated castor oil and polyoxyethylene polyoxypropylene pentaerythritol ether to the premix and continue stirring for 30 to 50 minutes to obtain self-leveling colored sand.