Benzotriazole-driven graphene oxide-coated microcapsules and their preparation and application

By improving the coating rate and bonding force of graphene oxide on the surface of microcapsules through electrostatic adsorption, the problem of poor bonding force between graphene oxide and inert microcapsules is solved, and a highly efficient self-healing coating for corrosion protection and substrate protection is achieved.

CN118406401BActive Publication Date: 2024-11-05NASURFAR BIOMATERIAL TECH (CHANGSHU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410881732.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-05
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

In the existing technology, the inert microcapsule shell prepared by the solvent evaporation method has low surface interaction force, resulting in low encapsulation rate and poor interfacial bonding force. Furthermore, the curing agent lags behind the microfracture of the coating, and cannot effectively protect the substrate from corrosion.

Method used

By introducing benzotriazole to electrostatically adsorb graphene oxide, the encapsulation rate and binding force of graphene oxide on the surface of microcapsules are improved. By utilizing the synergistic effect of benzotriazole and healing agent, the substrate is protected in real time during the healing process, thus preparing benzotriazole-driven graphene oxide-encapsulated microcapsules.

Benefits of technology

This improved the coating's coverage and interfacial bonding of graphene oxide on the microcapsule surface, enhanced the barrier properties of the coating, and effectively protected the substrate during the healing process, significantly improving the corrosion resistance and healing efficiency of the self-healing coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118406401B_ABST
    Figure CN118406401B_ABST
Patent Text Reader

Abstract

This invention relates to benzotriazole-driven graphene oxide-coated microcapsules, their preparation, and applications. The microcapsules of this invention comprise a core, a core wall, and an outer coating layer. The outer coating layer is composed of a surfactant, benzotriazole, and graphene oxide. Benzotriazole and graphene oxide are coated onto the surface of the core wall via electrostatic adsorption. This invention efficiently encapsulates graphene oxide onto the surface of inert self-healing microcapsules prepared by solvent evaporation under benzotriazole-driven conditions, forming microcapsules with a composite shell structure. These microcapsules, combined with bio-based coatings, can form long-life, high-performance self-healing coatings. This invention achieves efficient coating of graphene oxide onto the surface of inert microcapsule shells by benzotriazole-driven graphene oxide, solving not only the problem of decreased coating barrier performance caused by the addition of self-healing microcapsules but also the challenge of effectively protecting the substrate from corrosion during the coating healing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of graphene oxide materials, bio-based materials and self-repairing coatings, and in particular to benzotriazole-driven graphene oxide-coated microcapsules and preparation and application thereof. Background Art

[0002] Self-healing anti-corrosion coatings can repair micro-cracks caused by external collisions in real time, thereby greatly extending the service life of the anti-corrosion coating. In the field of harsh corrosive environments such as marine heavy corrosion protection, self-healing coatings are receiving more and more attention and application.

[0003] Self-healing mainly includes intrinsic self-healing and external self-healing. Intrinsic self-healing mainly relies on the introduction of dynamic chemical bonds such as hydrogen bonds to achieve healing after defects occur, while external self-healing mainly achieves self-healing by adding microcapsule materials containing healing agents. When defects occur, the healing agents fill the defective parts to achieve self-healing. In the field of anti-corrosion coatings, due to the demand for high mechanical and high barrier properties, current research is mainly focused on the field of external self-healing materials, mainly self-healing microcapsule materials.

[0004] Microcapsule materials achieve self-healing of the coating by embedding unhealed healing agent materials. Therefore, adding self-healing microcapsules to the coating will significantly reduce the barrier properties of the coating itself (the low-frequency impedance in salt water is reduced by 1-2 orders of magnitude), thereby reducing the service life of the coating and causing serious corrosion. Coating the surface of microcapsules with flexible, high-density two-dimensional materials such as graphene oxide (GO) is an effective solution. Graphene oxide materials contain a high-density, flexible carbon skeleton and are rich in functional groups such as hydroxyl, epoxy, and carboxyl groups on the surface. They have been widely used in anti-corrosion coatings, composite materials and other fields.

[0005] Liu et al. synthesized UF-PGO-LO / ER microcapsules encapsulating modified graphene oxide and linseed oil by in situ polymerization, with a core material loading of 79.6%. The electrochemical impedance value of the coating with 15 wt% of the above microcapsules reached 6.46×10 8 Ω·cm 2, 13 times higher than that of ordinary self-healing microcapsule coatings, and still has good anti-corrosion performance after immersion for 504 hours. When the coating is scratched, it can be completely repaired once within 4 hours, and the healing rate reaches 95.95%, achieving a dual improvement in anti-corrosion performance and self-healing function. Since the shell material will undergo polymerization reaction at the oil-water interface during the preparation process of the in-situ polymerization method, the graphene oxide rich in hydroxyl and carboxyl functional groups on the surface can easily participate in the polymerization reaction and achieve efficient coating on the surface of the microcapsule. However, the in-situ polymerization method is only applicable to shell material systems that can undergo interfacial polymerization reactions. For single-component microcapsule systems containing high reactivity, solvent evaporation method is usually used for preparation. The solvent evaporation method dissolves inert polymers such as polymethyl acrylate and polyethylene in a specific volatile solvent to form an emulsion. During the evaporation of the microdroplet solvent, the polymer undergoes phase separation, thereby obtaining microcapsules with an inert shell encapsulating the healing agent.

[0006] In the prior art, by introducing graphene oxide materials with different functional modifications in the process of preparing self-healing microcapsules by solvent evaporation method, self-healing microcapsule materials containing modified graphene oxide in both capsule core and capsule wall are prepared, which not only enhances the bonding force between microcapsules and coatings, but also enables microcapsules to be better opened when microcracks occur on the coating surface, thereby releasing healing factors and inhibiting the penetration of corrosion factors. However, in the process of preparing self-healing microcapsules by solvent evaporation method, graphene oxide is mostly physically adsorbed on the surface of microcapsules. Since the surface of microcapsules prepared by solvent evaporation method is highly inert, the graphene oxide encapsulation rate is very low; and graphene oxide has only van der Waals force with the inert microcapsule surface, resulting in insufficient bonding force; another difficulty of external self-healing anti-corrosion coating is that the curing of the self-healing agent lags behind the occurrence of microcracks in the coating, so the substrate cannot be effectively protected from corrosion during the curing of the self-healing agent. Summary of the invention

[0007] The surface force of the inert microcapsule shell prepared by the method of graphene oxide and solvent volatilization is low, resulting in low coverage, poor interface bonding strength, and the inability to effectively protect the substrate from corrosion during the curing of the healing agent. The present invention provides microcapsules coated with graphene oxide driven by benzotriazole and their preparation and application, including a method for preparing microcapsules coated with graphene oxide driven by benzotriazole and a self-healing coating and a self-healing coating composed of the microcapsules and the microcapsules and the coating. The present invention introduces molecules such as benzotriazole to electrostatically adsorb with graphene oxide to improve the coverage rate and bonding strength of graphene oxide on the surface of microcapsules and the real-time anti-corrosion of the substrate during the healing period.

[0008] The technical solution adopted by the present invention is as follows:

[0009] The first object of the present invention is to provide a benzotriazole driven graphene oxide wrapped microcapsule, comprising a capsule core, a capsule wall coated on the capsule core and an outer layer coated on the capsule wall;

[0010] The outer layer is composed of a surfactant, benzotriazole and graphene oxide;

[0011] The benzotriazole and graphene oxide are coated on the surface of the capsule wall by electrostatic adsorption.

[0012] In one embodiment of the present invention, the capsule core is a self-curing healing agent;

[0013] The material for preparing the capsule wall is selected from one or more of polymethyl methacrylate, polystyrene, polysulfone and polylactic acid; preferably polymethyl methacrylate or polystyrene;

[0014] Wherein, the polymethyl methacrylate, Mw: 150000~200000; the polystyrene, Mw: 200000~400000; the polysulfone, Mw: 50000~100000; the lactic acid, Mw: 100000~300000;

[0015] In one embodiment of the present invention, the self-curing healing agent is selected from one or more of an isocyanate-based curing agent, a castor oil-based curing agent, and an epoxy resin anion catalyst-type curing agent; preferably an isocyanate-based curing agent or an epoxy resin anion catalyst-type curing agent.

[0016] In one embodiment of the present invention, the surfactant is selected from one or more of polyvinyl alcohol, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and cardanol surfactants; preferably sodium dodecylbenzene sulfonate;

[0017] The cardanol surfactant includes anionic cardanol surfactant (such as cardanol polyoxyethylene ether ammonium sulfate, etc.) and nonionic cardanol surfactant (such as cardanol polyoxyethylene ether, etc.);

[0018] And / or, the mass ratio of the surfactant to the graphene oxide is 2:0.01-0.03; preferably 2:0.01;

[0019] And / or, the mass ratio of the benzotriazole to the graphene oxide is 1:1-3; preferably 1:2;

[0020] In one embodiment of the present invention, the mass ratio of the capsule wall, the capsule core and the outer cladding is 1-2:1-2:70-100, preferably 2:1:80.

[0021] In one embodiment of the present invention, the particle size of the microcapsules is 1 μm~30 μm; preferably, microcapsules with a particle size of 5 μm~20 μm can achieve the best self-healing performance of the coating, and microcapsules of appropriate size and uniform particle size are dispersed in the coating, which uniformly improves the mechanical properties of the coating and ensures the stability of the release rate after the microcapsules are ruptured.

[0022] The second object of the present invention is to provide a method for preparing the microcapsules, comprising the following steps:

[0023] (1) Using water as solvent, adding surfactant, stirring until the solid material is completely dissolved, and obtaining an emulsifier aqueous solution;

[0024] (2) dissolving benzotriazole, the self-curing healing agent and the material for preparing the capsule wall in an organic solvent, and dispersing the mixture by ultrasonication to obtain an oil phase;

[0025] (3) adding graphene oxide to the aqueous emulsifier solution obtained in part of step (1), and dispersing by ultrasonication to obtain an aqueous phase;

[0026] (4) adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), stirring and mixing to form an emulsion;

[0027] (5) adding the emulsion obtained in step (4) to the remaining emulsifier aqueous solution obtained in step (1), stirring for reaction, and after the reaction is completed, post-treating the reaction solution to obtain the benzotriazole-driven graphene oxide-wrapped microcapsules.

[0028] In one embodiment of the present invention, in step (1), the mass ratio of the surfactant to water is 1 to 5:100; preferably 4:100;

[0029] And / or, the mass ratio of the surfactant to graphene oxide is 2:0.01-0.03;

[0030] In one embodiment of the present invention, in step (2), the mass ratio of the sum of the mass of the benzotriazole, the self-curing healing agent and the material for preparing the capsule wall to the mass of the organic solvent is 1:2-10;

[0031] And / or, the mass ratio of the benzotriazole to the self-curing healing agent is 0.01-0.04:1-2, preferably 0.02:1;

[0032] And / or, the mass ratio of the benzotriazole to the material for preparing the capsule wall is 0.01-0.04:1-2, preferably 0.01:1;

[0033] And / or, the mass volume ratio of the benzotriazole to the organic solvent is 0.01 g:10 mL~30 mL, preferably 0.01 g:15 mL; the organic solvent is selected from one or more of dichloromethane, toluene and xylene.

[0034] In one embodiment of the present invention, in step (3), the mass volume ratio of the graphene oxide to the emulsifier aqueous solution is 0.01 g to 0.05 g: 80 mL, preferably 0.04 g: 80 mL; the graphene oxide is in the form of a mixed solution, the solvent in the mixed solution is water; the concentration of the graphene oxide in the mixed solution is 5 g / L to 10 g / L, preferably 8 g / L;

[0035] And / or, the temperature of the ultrasonic dispersion is room temperature, the frequency of the ultrasound is 30 kHz to 80 kHz, and the time of the ultrasound is 0.5 h to 2 h. Preferably, the ultrasound frequency is 80 kHz.

[0036] In one embodiment of the present invention, in step (4), the mass ratio of the material for preparing the capsule wall in the oil phase to the graphene oxide in the water phase is 1-2:0.01-0.03;

[0037] And / or, the stirring speed is 300 r / min~1000 r / min, and the stirring time is 10 min~20 min.

[0038] Preferably, in step (4), the mass ratio of the material for preparing the capsule wall in the oil phase to the graphene oxide in the water phase is 1:0.02; and the stirring and mixing is performed at a stirring rate of 700 r / min and a stirring time of 15 min.

[0039] In one embodiment of the present invention, in step (5), the stirring reaction is carried out at a temperature of 30°C to 50°C, for a time of 3 h to 5 h, and at a rate of 300 r / min to 500 r / min.

[0040] Preferably, in step (5), the stirring reaction is carried out at a stirring temperature of 40° C., a stirring time of 4 h, and a stirring rate of 400 r / min.

[0041] In one embodiment of the present invention, in step (5), the reaction solution is post-treated by centrifugation, washing, and vacuum drying.

[0042] The third object of the present invention is to provide the use of the microcapsules in the preparation of self-healing coatings.

[0043] The fourth object of the present invention is to provide a self-healing coating, which is prepared by stirring and mixing microcapsules wrapped in benzotriazole-driven graphene oxide with the coating; the mass fraction of the microcapsules wrapped in benzotriazole-driven graphene oxide in the self-healing coating is 5 wt%~20 wt%.

[0044] The coating includes petroleum-based bisphenol A epoxy resin coating, petroleum-based bisphenol F epoxy resin coating, and bio-based coating; the bio-based coating includes cardanol coating, castor oil coating or soybean oil epoxy resin coating.

[0045] Preferably, the coating is a cardanol coating; the total mass of microcapsules in the self-healing coating is 20 wt%.

[0046] A fifth object of the present invention is to provide a self-healing coating, which is prepared by coating the self-healing coating on the surface of a metal substrate.

[0047] The capsule core of the microcapsule of the present invention is prepared from an isocyanate-based curing agent, a castor oil-based curing agent or an epoxy resin anion catalyst-type curing agent that has a repairing effect on the self-healing coating, and is encapsulated in a capsule wall material; when microcracks appear in the self-healing coating, the capsule wall of the microcapsule ruptures to release the capsule core material to heal the crack area, and the curing agent contained in the capsule core is dispersed in the healing area to achieve self-healing of the coating; during the curing of the healing agent, the corrosion inhibition factor benzotriazole between the graphene oxide and the microcapsule shell is released, and a protective film can be formed on the metal surface, thereby achieving real-time protection of the substrate material during the self-healing period.

[0048] The above-mentioned benzotriazole-driven graphene oxide-wrapped microcapsules are applied to coatings, and the obtained coatings are coated on the surface of a metal substrate to obtain a self-healing coating with high-efficiency anti-corrosion and self-healing capabilities.

[0049] In one embodiment of the present invention, microcapsules can be added to the coating by stirring and dispersing. The coating with added microcapsules is coated on a metal substrate to obtain a self-healing coating. When microcracks appear on the surface of the self-healing coating due to external force, the microcapsules are ruptured due to stress expansion, releasing the encapsulated healing agent to repair the crack area, thereby improving the anti-corrosion and mechanical properties of the bio-based coating, and the corrosion inhibition factor benzotriazole between the graphene oxide and the microcapsule shell can achieve real-time protection of the substrate material during self-healing.

[0050] The above technical solution of the present invention has the following advantages compared with the prior art:

[0051] The present invention provides microcapsules encapsulated with graphene oxide driven by benzotriazole, and preparation and application thereof. The present invention introduces benzotriazole to interact with graphene oxide electrostatically (specifically, the NH functional group in benzotriazole interacts electrostatically with the hydroxyl group in graphene oxide), so that graphene oxide is efficiently coated on the surface of the microcapsule by electrostatic adsorption during the formation of the self-healing microcapsule, thereby improving the coverage rate of graphene oxide on the surface of the single-component microcapsule, thereby solving the essential defect of low barrier performance of the self-healing microcapsule itself; at the same time, the interface bonding force between graphene oxide and the surface of the single-component microcapsule is improved; the above-mentioned microcapsules are added to the coating, and when microcracks appear in the coating, the microcapsules are opened, and the benzotriazole and the healing agent between the graphene oxide and the microcapsule interlayer are released at the same time, and the benzotriazole can achieve real-time protection of the substrate during the curing of the healing factor. After the healing agent is completely cured, the cracked part can be repaired to achieve a self-healing effect.

[0052] (2) The present invention drives graphene oxide by benzotriazole, thus solving the technical problem that graphene oxide is difficult to efficiently coat on the surface of the inert microcapsule shell. The flexible, high-barrier graphene oxide is coated on the outer surface of the microcapsule, solving the problem that the barrier performance of the coating decreases due to the addition of self-healing microcapsules; at the same time, the benzotriazole between the graphene oxide and the microcapsule interlayer can effectively protect the substrate from corrosion during the curing of the coating self-healing agent, solving the problem that the self-healing coating cannot effectively protect the substrate from corrosion during the healing period. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0054] Figure 1 is a SEM image of the microcapsules wrapped in graphene oxide driven without adding benzotriazole (Comparative Example 1) and with adding benzotriazole (Example 1);

[0055] Figure 2 is a SEM image of the microcapsules wrapped in graphene oxide driven without adding benzotriazole (Comparative Example 2) and with adding benzotriazole (Example 2);

[0056] Figure 3 is a SEM image of the microcapsules wrapped in graphene oxide driven without adding benzotriazole (Comparative Example 3) and with adding benzotriazole (Example 3);

[0057] Figure 4 is the energy spectrum diagram of benzotriazole successfully coated on the surface of microcapsules; a1 is the microcapsule shell wall thickness diagram; b1 is the morphology diagram of the microcapsules in Example 1; b2, b3 and b4 are the EDS diagrams of the three elements C, O and N respectively;

[0058] Figure 5 is a comparison diagram of electrochemical impedance Bode of the self-healing coating prepared in Example 1 and Comparative Example 1 after being immersed in a 3.5 wt% NaCl solution for 60 days;

[0059] Figure 6 is a comparison diagram of electrochemical impedance Bode of the self-healing coating prepared in Example 2 and Comparative Example 2 after being immersed in a 3.5 wt% NaCl solution for 60 days;

[0060] Figure 7 is a comparison diagram of electrochemical impedance Bode of the self-healing coating prepared in Example 3 and Comparative Example 3 after being immersed in a 3.5 wt% NaCl solution for 60 days;

[0061] Figure 8 This is the electrochemical impedance Bode diagram of the self-healing coating after making an "X" scratch on the surface and self-healing for 1 h at room temperature and then soaking in 3.5 wt% NaCl solution for 7 days;

[0062] Fig. 9 The "X" scratch was made on the surface of the self-healing coating of polymethyl methacrylate coated with isocyanate-based curing agent microcapsules doped with benzotriazole-driven graphene oxide. After self-healing for 1 h at room temperature, the electrochemical impedance Bode diagram after immersion in 3.5 wt% NaCl solution for 7 days was obtained.

[0063] Fig.10 The "X" scratch was made on the surface of the self-healing coating doped with benzotriazole-driven graphene oxide on the surface of polymethyl methacrylate coated with epoxy resin anion catalyst type curing agent microcapsules. After self-healing for 1 hour at room temperature, the electrochemical impedance Bode diagram after immersion in 3.5 wt% NaCl solution for 7 days was obtained.

[0064] Fig.11 An "X" scratch was made on the surface of a self-healing coating of polystyrene coated with isocyanate-based curing agent microcapsules doped with benzotriazole-driven graphene oxide. After self-healing for 1 h at room temperature, the electrochemical impedance spectroscopy Bode diagram was taken after immersion in 3.5 wt% NaCl solution for 7 days. DETAILED DESCRIPTION

[0065] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0066] The sources of the substances used in the examples of the present invention are as follows:

[0067] Polymethyl methacrylate, Mw~195000; purchased from Sane Chemical Technology (Shanghai) Co., Ltd.;

[0068] Polystyrene, Mw~300000; purchased from Sane Chemical Technology (Shanghai) Co., Ltd.;

[0069] Q235 carbon steel sheet was purchased from Changzhou Coatings Research Institute Co., Ltd.;

[0070] Sodium dodecyl sulfate was purchased from Shanghai Lingfeng Chemical Reagent Co., Ltd.;

[0071] Isocyanate-based curing agent (IPDI) was purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0072] References for the preparation of graphene oxide: Chen J, Yao B, Li C, et al. An improved Hummers method for eco-friendly synthesis of graphene oxide[J]. Carbon, 2013,64: 225-229;

[0073] Natural flake graphite (8000 mesh) was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0074] Epoxy resin anion catalyst type curing agent (DMP-30) was purchased from Shanghai MacLean Biochemical Co., Ltd.;

[0075] Benzotriazole was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0076] Cardanol-based epoxy anticorrosive coatings were purchased from Changshu Naisu Biomaterials Technology Co., Ltd.

[0077] Example 1: Preparation of graphene oxide@benzotriazole / polymethyl methacrylate-encapsulated isocyanate-based curing agent microcapsules and their self-healing coatings.

[0078] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0079] (2) Take 1 g of isocyanate curing agent (IPDI) and 2 g of polymethyl methacrylate in a mass ratio of 1:2, then take 20 mg of benzotriazole (BTA) and add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0080] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0081] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0082] (5) The emulsion obtained in step (4) was poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to completely evaporate, thereby obtaining a suspension of graphene oxide @ benzotriazole / polymethyl methacrylate-encapsulated isocyanate-based curing agent microcapsules. After centrifugation, washing, and vacuum drying, benzotriazole-driven graphene oxide-encapsulated microcapsules (graphene oxide @ benzotriazole / polymethyl methacrylate-encapsulated isocyanate-based curing agent microcapsules) were obtained.

[0083] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, and the surface is cleaned with ethanol and dried naturally in the air. The microcapsules prepared in step (5) are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0084] Example 2: Preparation of graphene oxide@benzotriazole / polymethyl methacrylate-encapsulated epoxy resin anion catalyst-type curing agent microcapsules and their self-healing coatings.

[0085] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0086] (2) Take 1 g of epoxy resin anion catalyst curing agent (DMP-30) and 2 g of polymethyl methacrylate in a mass ratio of 1:2, then take 20 mg of benzotriazole (BTA) and add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0087] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0088] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0089] (5) The emulsion obtained in step (4) was poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to evaporate completely, thereby obtaining a suspension of graphene oxide @ benzotriazole / polymethyl methacrylate-encapsulated epoxy resin anion catalyst-type curing agent microcapsules. After centrifugation, washing, and vacuum drying, benzotriazole-driven graphene oxide-encapsulated microcapsules (graphene oxide @ benzotriazole / polymethyl methacrylate-encapsulated epoxy resin anion catalyst-type curing agent microcapsules) were obtained.

[0090] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, cleaned with ethanol, and dried naturally in the air. The single-component self-healing microcapsules prepared above are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0091] Example 3: Preparation of graphene oxide@benzotriazole / polystyrene-encapsulated isocyanate-based curing agent microcapsules and their self-healing coatings.

[0092] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0093] (2) Take 1 g of isocyanate curing agent (IPDI) and 2 g of polystyrene in a mass ratio of 1:2, then take 20 mg of benzotriazole (BTA) and add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0094] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and perform ultrasonic treatment at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0095] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0096] (5) The emulsion obtained in step (4) was poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to completely evaporate, thereby obtaining a suspension of graphene oxide @ benzotriazole / polystyrene-encapsulated isocyanate-based curing agent microcapsules. After centrifugation, washing, and vacuum drying, benzotriazole-driven graphene oxide-encapsulated microcapsules (graphene oxide @ benzotriazole / polystyrene-encapsulated isocyanate-based curing agent microcapsules) were obtained.

[0097] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, cleaned with ethanol, and dried naturally in the air. The single-component self-healing microcapsules prepared above are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0098] Comparative Example 1: Preparation of graphene oxide / polymethyl methacrylate-coated isocyanate-based curing agent microcapsules and their self-healing coatings.

[0099] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0100] (2) Take 1 g of isocyanate curing agent (IPDI) and 2 g of polymethyl methacrylate in a mass ratio of 1:2, add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0101] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0102] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0103] (5) The emulsion obtained in step (4) is poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to completely evaporate, thereby obtaining a suspension of graphene oxide / polymethyl methacrylate-encapsulated isocyanate-based curing agent microcapsules. After centrifugation, washing, and vacuum drying, single-component self-healing microcapsules wrapped in graphene oxide (graphene oxide / polymethyl methacrylate-encapsulated isocyanate-based curing agent microcapsules) are obtained.

[0104] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, cleaned with ethanol, and dried naturally in the air. The single-component self-healing microcapsules prepared above are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0105] Comparative Example 2: Preparation of graphene oxide / polymethyl methacrylate-coated epoxy resin anion catalyst-type curing agent microcapsules and their self-healing coatings.

[0106] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0107] (2) Take 1 g of epoxy resin anion catalyst curing agent (DMP-30) and 2 g of polymethyl methacrylate in a mass ratio of 1:2, add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0108] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and perform ultrasonic treatment at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0109] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0110] (5) The emulsion obtained in step (4) is poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to completely evaporate, thereby obtaining a suspension of graphene oxide / polymethyl methacrylate-encapsulated epoxy resin anion catalyst-type curing agent microcapsules. After centrifugation, washing, and vacuum drying, single-component self-healing microcapsules wrapped in graphene oxide (graphene oxide / polymethyl methacrylate-encapsulated epoxy resin anion catalyst-type curing agent microcapsules) can be obtained.

[0111] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, cleaned with ethanol, and dried naturally in the air. The single-component self-healing microcapsules prepared above are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0112] Comparative Example 3: Preparation of graphene oxide / polystyrene-coated isocyanate-based curing agent microcapsules and their self-healing coatings.

[0113] (1) 8 g of a surfactant, sodium dodecyl sulfate, was added to 200 g of deionized water and stirred at room temperature until the solid material was completely dissolved to obtain an aqueous solution containing 4 wt% of sodium dodecyl sulfate;

[0114] (2) Take 1 g of isocyanate curing agent (IPDI) and 2 g of polystyrene in a mass ratio of 1:2, add them to 30 mL of dichloromethane, stir until completely dissolved, and ultrasonicate at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an oil phase;

[0115] (3) Add 5 mL of a water mixture containing graphene oxide (GO) (the concentration of graphene oxide in the mixture is 8 g / L) to 80 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and perform ultrasonic treatment at 80 kHz for 15 min at room temperature until the solid material is completely dispersed to obtain an aqueous phase;

[0116] (4) slowly adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), and mechanically stirring at 700 rpm for 15 min to form an emulsion;

[0117] (5) The emulsion obtained in step (4) is poured into 120 mL of an aqueous solution containing 4 wt% sodium dodecyl sulfate (prepared in step (1)), and stirred at 400 rpm for 4 h at 40°C to allow the dichloromethane to completely evaporate, thereby obtaining a suspension of graphene oxide / polystyrene-encapsulated isocyanate-based curing agent microcapsules. After centrifugation, washing, and vacuum drying, single-component self-healing microcapsules encapsulated in graphene oxide (graphene oxide / polystyrene-encapsulated isocyanate-based curing agent microcapsules) are obtained.

[0118] (6) The substrate material is a steel plate (Q235 carbon steel sheet). The surface of the steel plate is polished smooth with 800-grit sandpaper, and the surface is cleaned with ethanol and dried naturally in the air. The single-component self-healing microcapsules prepared above are added to the cardanol-based epoxy anticorrosive coating at 20 wt%, stirred evenly, and then the coating is scraped on the surface of the steel plate to scrape a 200 μm wet film coating. The self-healing coating is cured at room temperature for 24 h to obtain the self-healing coating.

[0119] Test Example 1

[0120] The surface morphology of the benzotriazole-driven graphene oxide-wrapped microcapsules obtained under different preparation conditions in the examples and comparative examples was characterized by scanning electron microscopy (SEM), and the strength of the interfacial bonding between graphene oxide and the surface of the microcapsules was determined by observing the surface morphology.

[0121] Figure 1-3 These are SEM images of microcapsules wrapped in graphene oxide without and with benzotriazole added. Figure 1-3 Figure A in the figure shows the microcapsules without adding benzotriazole ( Figure 1 A in the figure corresponds to the microcapsule of Example 1; Figure 2 A in the figure corresponds to the microcapsule of Example 2; Figure 3 A in the figure corresponds to the microcapsule of Example 3), and the surface of the microcapsule is relatively smooth and the degree of graphene oxide coating is relatively low. Figure 1-3 Figure B in the figure are all microcapsules with added benzotriazole ( Figure 1 B in the embodiment corresponds to the microcapsule in Example 1; Figure 2 B in the embodiment corresponds to the microcapsule in Example 2; Figure 3 B in the figure corresponds to the microcapsule in Example 3). After adding benzotriazole, it was clearly observed that the surface of the microcapsule showed more graphene oxide coating.

[0122] EDS characterization proved that benzotriazole was successfully coated on the surface of the microcapsules. The microcapsules prepared in Example 1 were sampled. The sampling depth of the EDS spectrum was within 1 μm, while the thickness of the microcapsule shell was greater than 1 μm. Figure 4 As shown in a1 in the figure, the core material elements of the microcapsule will not affect the analysis of C, O, and N elements by EDS energy spectrum.

[0123] From the EDS image, it can be seen that the surface of the microcapsule is mainly composed of three elements: C, O, and N ( Figure 4 b2-b4 in the figure), and the element distribution is limited to the location where the microcapsules exist. Among them, C and O occupy the main distribution, and N element distribution is slightly less. This may be because C and O elements mainly come from the shell wall material and GO wrapped on the outer surface of the microcapsule, while N element comes from BTA molecules adsorbed on the wrinkles of the GO surface and BTA reacting with GO. The above results show that BTA exists in the GO and PMMA interlayers.

[0124] Test Example 2

[0125] Figure 5 The figure is a comparison of the electrochemical impedance Bode of the self-healing coating prepared in comparative example 1 and example 1 after being immersed in a 3.5 wt% NaCl solution for 60 days. Figure 5 It can be seen that after adding 20 wt% benzotriazole to drive the self-healing coating of graphene oxide-wrapped microcapsules to 3.5 wt% NaCl solution for 60 days, the Bode diagram shows that the low-frequency impedance value remains at 2.8×10 10 Ω·cm -1 The electrochemical impedance value of the self-healing coating incorporating the single-component self-healing microcapsules without adding benzotriazole is 6.77×10 7 Ω·cm -1 , which is improved by 3 orders of magnitude, and the low-frequency impedance value is greatly improved, indicating that the anti-corrosion ability of the microcapsule coating efficiently wrapped by benzotriazole driven graphene oxide in the embodiment of the present invention is greatly enhanced.

[0126] Figure 6 The figure is a comparison of the electrochemical impedance Bode of the self-healing coating prepared in comparative example 2 and example 2 after being immersed in a 3.5 wt% NaCl solution for 60 days. Figure 6 It can be seen that the electrochemical impedance spectroscopy value of the self-healing coating of graphene oxide-wrapped microcapsules driven by the addition of benzotriazole is 2.09×1010 Ω·cm -1 , while the electrochemical impedance value of the self-healing coating of the single-component self-healing microcapsules without adding benzotriazole was 4.53×10 9 Ω·cm -1 , an order of magnitude improvement.

[0127] Figure 7 The following is a comparison of the electrochemical impedance Bode of the self-healing coating prepared by adding comparative example 3 and example 3 after being immersed in 3.5 wt% NaCl solution for 60 days. Figure 7 It can be seen that the electrochemical impedance spectroscopy value of the self-healing coating of graphene oxide-wrapped microcapsules driven by the addition of benzotriazole is 2.49×10 10 Ω·cm -1 , while the electrochemical impedance value of the self-healing coating of the single-component self-healing microcapsules without adding benzotriazole was 8.56×10 7 Ω·cm -1 , an improvement of 3 orders of magnitude.

[0128] Test Example 3

[0129] Figure 8 The electrochemical impedance Bode diagram of the self-healing coating without microcapsules after making an "X" scratch on the surface and self-healing for 1 h at room temperature and then immersed in 3.5 wt% NaCl solution for 7 days. When the scratch occurred, the metal substrate was not corroded by the salt water, and the electrochemical impedance value remained at 2.28×10 10 Ω·cm -1 On the 7th day of corrosion, the electrochemical impedance value dropped to 7.86×10 5 Ω· cm -1 , indicating that the coating has been penetrated by the corrosive medium and has lost its anti-corrosion ability.

[0130] Fig. 9 The "X" scratch was made on the surface of the self-healing coating of polymethyl methacrylate coated with isocyanate-based curing agent microcapsules by adding benzotriazole-driven graphene oxide in Example 1. After self-healing for 1 h at room temperature, the electrochemical impedance Bode diagram after immersion in 3.5 wt% NaCl solution for 7 days was obtained. When the scratch occurred on the first day, the electrochemical impedance value was 4.15×10 10 Ω·cm -1 Due to the synergistic effect of BTA and GO, the BTA between GO and microcapsules can achieve real-time protection of the substrate during the curing of the healing factor, and the corrosive medium cannot enter the coating. The coating still remains at 4.14×10 10 Ω·cm -1 , achieving scratch self-healing effect.

[0131] Fig.10 The "X" scratch was made on the surface of the self-healing coating of polymethyl methacrylate coated with epoxy resin anion catalyst type curing agent microcapsules by adding benzotriazole-driven graphene oxide in Example 2. After self-healing for 1 h at room temperature, the electrochemical impedance Bode diagram after immersion in 3.5 wt% NaCl solution for 7 days was obtained. When the scratch occurred on the first day, the electrochemical impedance value was 2.20×10 10 Ω·cm -1 Then, graphene oxide and benzotriazole cooperated to block the corrosion medium from invading the coating, and the concentration slowly decreased to 1.47×10 8 Ω·cm -1 , and then stabilized at 6.69×10 7 Ω·cm -1 Compared with the pure bio-based coating, the electrochemical impedance value on the 7th day increased by 2 orders of magnitude.

[0132] Fig.11 The "X" scratch was made on the surface of the self-healing coating of polystyrene coated with isocyanate-based curing agent microcapsules by adding benzotriazole-driven graphene oxide in Example 3. After self-healing for 1 h at room temperature, the electrochemical impedance Bode diagram after immersion in 3.5 wt% NaCl solution for 7 days was obtained. When the scratch occurred on the first day, the electrochemical impedance value was 4.15×10 10 Ω·cm -1 ,, then graphene oxide and benzotriazole cooperated to block the corrosion medium from invading the coating, and then stabilized at 5.33×10 8 Ω·cm -1 Compared with the pure bio-based coating, the electrochemical impedance value on the 7th day increased by 3 orders of magnitude.

[0133] Test Example 4

[0134] Table 1 shows the healing efficiency of the self-healing coatings in different embodiments and comparative examples obtained through TDCB testing. According to the method of Cho et al., a fracture test was carried out on a conical double cantilever beam (TDCB) specimen using a universal materials testing machine. The specimen was first cured at room temperature for 24 hours, and then a pre-crack was cut with a blade. The fracture tests of all specimens were carried out on a universal materials testing machine model KJ-1065 at a speed of 10 mm / min. The specimen was mounted on a load frame, and as the load increased, the pre-crack expanded along the center line of the specimen until the maximum tensile strength could not be obtained. S original Next, the specimen was unloaded to allow the crack surfaces to re-contact. The specimen was stored and cured at room temperature for 24 hours. The strength of the healed specimen was then tested and marked as S healedThe healing efficiency is defined as the ratio of the maximum tensile strength of the healed specimen to that of the original specimen: .

[0135] Table 1 Healing efficiency of comparative examples and embodiments

[0136] experiment Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Healing efficiency 85% 90% 92% 65% 45% 58%

[0137] It can be seen from Table 1 that the healing efficiency of the self-healing coatings prepared in Example 1, Example 2 and Example 3 is much higher than that of the comparative example.

[0138] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A benzotriazole-driven graphene oxide-encapsulated microcapsule, characterized in that: It comprises a capsule core, a capsule wall coated on the capsule core and an outer layer coated on the capsule wall; The outer layer is composed of a surfactant, benzotriazole and graphene oxide; The benzotriazole and graphene oxide are coated on the surface of the capsule wall by electrostatic adsorption; The capsule core is a self-curing healing agent; the self-curing healing agent is selected from one or more of an isocyanate-based curing agent, a castor oil-based curing agent, and an epoxy resin anion catalyst-based curing agent; The material for preparing the capsule wall is selected from one or more of polymethyl methacrylate, polystyrene, polysulfone and polylactic acid; The surfactant is selected from one or more of polyvinyl alcohol, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate and cardanol surfactant; The method for preparing the microcapsules comprises the following steps: (1) Using water as solvent, adding surfactant, stirring until the solid material is completely dissolved, and obtaining an emulsifier aqueous solution; (2) dissolving benzotriazole, the self-curing healing agent and the material for preparing the capsule wall in an organic solvent, and performing ultrasonic dispersion to obtain an oil phase; (3) adding graphene oxide to the aqueous emulsifier solution obtained in part of step (1), and dispersing by ultrasonication to obtain an aqueous phase; (4) adding the oil phase obtained in step (2) to the aqueous phase obtained in step (3), stirring and mixing to form an emulsion; (5) adding the emulsion obtained in step (4) to the remaining emulsifier aqueous solution obtained in step (1), stirring for reaction, and after the reaction is completed, post-treating the reaction solution to obtain the benzotriazole-driven graphene oxide-wrapped microcapsules; In step (2), the mass ratio of the sum of the mass of the benzotriazole, the self-curing healing agent and the material for preparing the capsule wall to the mass of the organic solvent is 1:2-10; The mass ratio of the benzotriazole to the self-curing healing agent is 0.01-0.04:1-2; The mass ratio of the benzotriazole to the material for preparing the capsule wall is 0.01-0.04:1-2; The mass volume ratio of the benzotriazole to the organic solvent is 0.01 g: 10 mL to 30 mL; the organic solvent is selected from one or more of dichloromethane, toluene and xylene; In step (3), the mass volume ratio of the graphene oxide to the emulsifier aqueous solution is 0.01 g to 0.05 g: 80 mL; the graphene oxide is in the form of a mixed solution, the solvent in the mixed solution is water, and the concentration of the graphene oxide in the mixed solution is 5 g / L to 10 g / L; In step (4), the mass ratio of the material for preparing the capsule wall in the oil phase to the graphene oxide in the water phase is 1-2:0.01-0.

03.

2. The microcapsule according to claim 1, characterized in that The mass ratio of the surfactant to the graphene oxide is 2:0.01-0.

03.

3. The microcapsule according to claim 1, characterized in that The mass ratio of the benzotriazole to the graphene oxide is 1:1-3.

4. The microcapsule according to claim 1, characterized in that The mass ratio of the capsule wall, the capsule core and the outer cladding is 1-2:1-2:70-100.

5. The microcapsule according to claim 1, characterized in that In step (3), the temperature of the ultrasonic dispersion is room temperature, the frequency of the ultrasound is 30 kHz to 80 kHz, and the time of the ultrasound is 0.5 h to 2 h.

6. The microcapsule according to claim 1, characterized in that In step (4), the stirring speed is 300 r / min~1000 r / min, and the stirring time is 10 min~20 min.

7. Use of the microcapsule according to any one of claims 1 to 6 in the preparation of a self-healing coating.

8. A self-healing coating, characterized in that: The self-healing coating is prepared by stirring and mixing the microcapsules wrapped in benzotriazole-driven graphene oxide according to any one of claims 1 to 6 with a coating; the mass fraction of the microcapsules wrapped in benzotriazole-driven graphene oxide in the self-healing coating is 5 wt% to 20 wt%.

9. A self-healing coating, characterized in that: The self-healing coating is prepared by coating the self-healing coating according to claim 8 on the surface of a metal substrate.