A method for preparing austenitic stainless steel seamless pipe
Through the process of electroslag remelting, forging and silicone modified coating, the problem of corrosion of austenitic stainless steel seamless pipes in highly corrosive media is solved, its mechanical properties and corrosion resistance are improved, and its service life is extended. Long life and stable in acid, alkali and salt solvents.
Patent Information
- Application Number
- CN202410449559.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Austenitic stainless steel seamless pipes are prone to corrosion when exposed to highly corrosive media, resulting in shortened material life and reduced production efficiency.
After smelting by electroslag remelting process and high-temperature homogenization heat treatment, the raw pipe is prepared through forging and cold rolling processes, and the surface and wall of the steel pipe are coated with silicone modified coating, using ethylene carbonate, polymethylmethacrylate The amine-terminated silicon-containing prepolymer is prepared from raw materials such as hydrogen siloxane and mixed with epoxy resin to form a weather-resistant and hydrophobic coating.
Significantly improve the mechanical properties and corrosion resistance of austenitic stainless steel seamless pipes, extend the service life, the coating does not foam or fall off in acid, alkali and salt solvents, and has excellent chemical resistance and hydrolysis resistance .
Smart Images

Figure BDA0004792166080000121 
Figure BDA0004792166080000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel seamless pipes, in particular to a method for preparing an austenitic stainless steel seamless pipe. Background Art
[0002] Austenitic stainless steel seamless pipe is a pipe material used to transport fluids or gases. It is made of austenitic stainless steel and is made using a seamless processing technology. Austenitic stainless steel is a stainless steel structure with good corrosion resistance and mechanical properties. It shows excellent durability in various environments, so it is often used in chemical, petroleum, natural gas, aerospace, pharmaceutical and other fields.
[0003] Although austenitic stainless steel seamless pipes have the characteristics of corrosion resistance, high temperature resistance, and pressure resistance, and are often considered to be suitable for various harsh environments and high-demand working conditions, in industrial applications, if austenitic stainless steel is in direct contact with highly corrosive media such as salt water containing chloride ions, acidic solutions, and alkaline solutions, the material is still at risk of corrosion, which not only increases the cost of material replacement, but also seriously affects the efficiency of industrial production and operations. Coating the surface of austenitic stainless steel seamless pipes with resin materials such as epoxy resin for protection is a cheap, convenient and effective method that can effectively extend the service life of austenitic stainless steel seamless pipes. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing an austenitic stainless steel seamless pipe to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0006] Step 1:
[0007] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high temperature homogenization heat treatment at 1180-1250°C for 90-100 hours. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1050-1200°C, the final forging temperature is 850-950°C, and the total forging elongation coefficient is 3-5. The tube blanks are cut to a certain length, end-face drilled, machined, and hot extruded at 1190-1220°C to obtain rough tubes.
[0008] Step 2:
[0009] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1060-1080℃, the holding time is 30-35min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1080-1090℃, the holding time is 15-20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 15-25s;
[0010] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1-1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0011] S1: Disperse ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, raise the temperature to 60-70°C under nitrogen protection, add polymethylhydrogensiloxane dropwise with stirring for 1-1.5h, raise the temperature to 80-85°C, react for 9-12h, and then distill under reduced pressure to obtain organosilicon grafted carbonate;
[0012] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 10 to 15 minutes, and then the temperature is raised to 35 to 40°C, and a mixed solution of hydrogen peroxide and phosphoric acid is added dropwise. After the addition is completed, the temperature is further raised to 60 to 65°C, and the mixture is reacted for 2 to 3 hours. After the reaction is completed, the mixture is washed until it becomes neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation.
[0013] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize, stir and heat, maintain the pressure for 12 to 15 hours, remove impurities and obtain carbonate castor oil;
[0014] S4: adding organic silicon grafted carbonate to carbonate castor oil to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine, heating to 80-90° C. to react for 6-8 hours, and performing reduced pressure distillation to obtain an amine-terminated silicon-containing prepolymer;
[0015] S5: using an organic mixed solution to dilute the terminal amine-containing silicon-containing prepolymer to obtain a curing agent, and mixing the epoxy resin E51 and the curing agent.
[0016] Furthermore, in S1, active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:(0.8-1).
[0017] Furthermore, in S2, the weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid and urea is 100:(70-75):(2-2.5):(25-28):(0.3-0.5).
[0018] Furthermore, in S3, the reaction pressure is 2-2.5 MPa, and the reaction temperature is 120-130°C.
[0019] Furthermore, in S4, in the carbonate mixture, the weight ratio of the organosilicon grafted carbonate to the carbonate castor oil is 1:(8-10).
[0020] Furthermore, in S4, the carbonate mixture and ethylenediamine are reacted at a molar ratio of carbonate group to amine group of 1:(2.3-2.5).
[0021] Furthermore, in S5, the contents of the components in the organic mixed solvent are, by weight percentage, 50-60% of xylene, 20-30% of n-butanol, and 20-30% of benzyl alcohol.
[0022] Furthermore, in S5, the solid content of the curing agent is 65-75%.
[0023] Furthermore, in S5, the epoxy resin E51 and the curing agent are mixed in a weight ratio of (0.75-0.8):1.
[0024] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention uses an electroslag remelting process to smelt stainless steel materials, casts them into steel ingots, performs high-temperature homogenization heat treatment, and then performs upsetting, drawing, forging and blanking on the steel ingots, and hot extrusion to obtain rough pipes; the rough pipes are straightened, surface deburred, pickled, and then subjected to two cold rolling processes to obtain the desired finished product specifications. The austenitic stainless steel seamless pipes forged by the process of the present invention have good mechanical properties and corrosion resistance.
[0025] In order to further extend the service life of austenitic stainless steel seamless pipes, the present invention coats an organosilicon modified coating on the surface and wall of a steel pipe respectively. The organosilicon modified coating uses vinyl ethylene carbonate and polymethyl hydrogen siloxane as raw materials, uses chloroplatinic acid as a catalyst, and introduces carbonate groups into polymethyl hydrogen siloxane through the reaction of active hydrogen and carbon-carbon double bonds to obtain organosilicon grafted carbonate; uses castor oil as a raw material, first reacts carboxylic acid with hydrogen peroxide in the presence of hydrogen ions in the system to generate peroxycarboxylic acid, and the peroxycarboxylic acid reacts with unsaturated double bonds in castor oil to generate epoxy castor oil to achieve epoxy group modification, and then introduces carbon dioxide gas to generate cyclic carbonate by reacting epoxy groups with carbon dioxide to obtain carbonate castor oil; adds organosilicon grafted carbonate to carbonate castor oil to obtain a carbonate mixture, and reacts carbonate groups with ethylenediamine to make the ethylenediamine excessive, so that the organosilicon grafted carbonate and carbonate castor oil are polymerized to obtain an amine-terminated silicon-containing prepolymer.
[0026] By using terminal amine-containing silicon-containing prepolymer as a curing agent and mixing it with epoxy resin, flexible segments can be introduced into the epoxy resin to improve its mechanical properties. At the same time, in the terminal amine-containing silicon-containing prepolymer, silicone and castor oil can be synergistically modified to improve the hydrophobicity, thermal stability and weather resistance of the epoxy resin. In the process of polymerization of the carbonate group and the amine group, a hydroxyl group will be formed in the molecule, forming hydrogen bonds within or between the molecules, thereby enhancing the interaction between the molecules, making the epoxy resin more resistant to chemical corrosion, and its chemical resistance and hydrolysis resistance are relatively excellent. The formed coating can be in acid, alkali and salt solvents for a long time without bubbling or falling off.
[0027] In addition, it should be noted that when the carbonate mixture is reacted with ethylenediamine to prepare the terminal amine-containing silicon-containing prepolymer, the weight ratio of the organosilicon grafted carbonate to the carbonate castor oil in the carbonate mixture needs to be controlled to be 1: (8-10). If the amount of organosilicon grafted carbonate is too high, it will lead to the presence of more polysiloxane structures in the side chains of the terminal amine-containing silicon-containing prepolymer. Since the surface energy of the Si-O-Si segment is low, it is easy to migrate to the surface during the curing film formation process with the epoxy resin, and the large molecular weight polysiloxane structure has an obvious steric hindrance effect, which will affect the curing film effect, resulting in reduced adhesion and poor corrosion resistance. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Materials used in the present invention and their sources: polymethyl hydrogen siloxane comes from Guangzhou Yuanda New Materials Co., Ltd., with an active hydrogen content of 16 mmol / g; epoxy resin E51 brand is Wuxi Phoenix brand, item number ph0443.
[0030] Embodiment 1: A method for preparing an austenitic stainless steel seamless pipe comprises the following steps:
[0031] Step 1:
[0032] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1180℃ for 90h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1050℃, the final forging temperature is 850℃, and the total forging elongation coefficient is 5. The tube billet is cut to a fixed length, end-face drilled, machined, and hot extruded at 1190℃ to obtain a rough tube.
[0033] Step 2:
[0034] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1060℃, the holding time is 30min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1080℃, the holding time is 15min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 15s;
[0035] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0036] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, under nitrogen protection, heat to 65°C, add polymethyl hydrogen siloxane dropwise with stirring for 1 hour, heat to 80°C, react for 9 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0037] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 10 minutes and then heated to 35°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 60°C after the addition is complete, and the mixture is reacted for 2 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0038] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2MPa, stir and heat to 120°C, maintain the pressure reaction for 12h, remove impurities and obtain carbonate castor oil;
[0039] S4: adding organic silicon grafted carbonate to carbonate castor oil at a weight ratio of 1:10 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 80° C. to react for 6 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0040] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0041] Embodiment 2: A method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0042] Step 1:
[0043] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1200℃ for 95h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1100℃, the final forging temperature is 900℃, and the total forging elongation coefficient is 5. The tube blanks are cut to a fixed length, end-face drilled, machined, and hot extruded at 1200℃ to obtain rough tubes.
[0044] Step 2:
[0045] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1070℃, the holding time is 30min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1085℃, the holding time is 20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 20s;
[0046] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0047] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, heat to 70°C under nitrogen protection, add polymethyl hydrogen siloxane dropwise with stirring for 1.5 hours, heat to 85°C, react for 10 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0048] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 15 minutes and then heated to 40°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 65°C after the addition is complete, and the mixture is reacted for 2.5 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0049] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2.5 MPa, stir and heat to 125°C, maintain the pressure reaction for 13 hours, remove impurities and obtain carbonate castor oil;
[0050] S4: adding organic silicon grafted carbonate to carbonate castor oil at a weight ratio of 1:10 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 85° C. to react for 7 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0051] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0052] Embodiment 3: A method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0053] Step 1:
[0054] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1250°C for 100 hours. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1200°C, the final forging temperature is 950°C, and the total forging elongation coefficient is 5. The tube blanks are cut to a fixed length, end-face drilled, machined, and hot extruded at 1220°C to obtain rough tubes.
[0055] Step 2:
[0056] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1080℃, the holding time is 35min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1090℃, the holding time is 20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 25s;
[0057] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0058] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, under nitrogen protection, heat to 60°C, add polymethyl hydrogen siloxane dropwise with stirring for 1.5 hours, heat to 85°C, react for 12 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0059] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 15 minutes, then heated to 40°C, and a mixed solution of hydrogen peroxide and phosphoric acid is added dropwise. After the addition is complete, the mixture is heated to 65°C and reacted for 3 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0060] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2.5 MPa, stir and heat to 130°C, maintain the pressure reaction for 15 hours, remove impurities and obtain carbonate castor oil;
[0061] S4: adding organosilicon-grafted carbonate to carbonate castor oil at a weight ratio of 1:10 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 90° C. to react for 8 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0062] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0063] Embodiment 4: A method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0064] Step 1:
[0065] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1190℃ for 90h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1080℃, the final forging temperature is 850℃, and the total forging elongation coefficient is 5. The tube billet is cut to a fixed length, end-face drilled, machined, and hot extruded at 1210℃ to obtain a rough tube.
[0066] Step 2:
[0067] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1065℃, the holding time is 35min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1085℃, the holding time is 20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 15s;
[0068] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0069] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, under nitrogen protection, heat to 65°C, add polymethyl hydrogen siloxane dropwise with stirring for 1 hour, heat to 80°C, react for 9 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0070] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 10 minutes and then heated to 35°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 60°C after the addition is complete, and the mixture is reacted for 2 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0071] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2MPa, stir and heat to 120°C, maintain the pressure reaction for 12h, remove impurities and obtain carbonate castor oil;
[0072] S4: adding organic silicon grafted carbonate to carbonate castor oil at a weight ratio of 1:9 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 80° C. to react for 6 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0073] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0074] Embodiment 5: A method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0075] Step 1:
[0076] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1190℃ for 95h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1200℃, the final forging temperature is 850℃, and the total forging elongation coefficient is 5. The tube blanks are cut to a fixed length, end-face drilled, machined, and hot extruded at 1220℃ to obtain rough tubes.
[0077] Step 2:
[0078] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1060℃, the holding time is 30min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1085℃, the holding time is 15min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 20s;
[0079] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0080] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, under nitrogen protection, heat to 60°C, add polymethyl hydrogen siloxane dropwise with stirring for 1 hour, heat to 80°C, react for 9 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0081] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 12 minutes and then heated to 37°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 65°C after the addition is complete, and the mixture is reacted for 2 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0082] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2.2MPa, stir and heat to 125°C, maintain the pressure reaction for 14h, remove impurities and obtain carbonate castor oil;
[0083] S4: adding organic silicon grafted carbonate to carbonate castor oil at a weight ratio of 1:9.5 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 80° C. to react for 6 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0084] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0085] Embodiment 6: A method for preparing an austenitic stainless steel seamless pipe, comprising the following steps:
[0086] Step 1:
[0087] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1250℃ for 100 hours. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1050℃, the final forging temperature is 850℃, and the total forging elongation coefficient is 5. The tube blanks are cut to a fixed length, end-face drilled, machined, and hot extruded at 1220℃ to obtain rough tubes.
[0088] Step 2:
[0089] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1080℃, the holding time is 35min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1090℃, the holding time is 15min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 20s;
[0090] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0091] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, under nitrogen protection, heat to 70°C, add polymethyl hydrogen siloxane dropwise with stirring for 1.5 hours, heat to 85°C, react for 9 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0092] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 10 minutes and then heated to 38°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 65°C after the addition is complete, and the mixture is reacted for 3 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0093] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2.5 MPa, stir and heat to 130°C, maintain the pressure reaction for 12 hours, remove impurities and obtain carbonate castor oil;
[0094] S4: adding organosilicon-grafted carbonate to carbonate castor oil at a weight ratio of 1:8 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 80° C. to react for 6 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0095] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0096] Comparative Example 1: Ethylenediamine was directly used as the curing agent, and the other parameters were the same as those in Example 1.
[0097] Step 1:
[0098] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1180℃ for 90h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1050℃, the final forging temperature is 850℃, and the total forging elongation coefficient is 5. The tube billet is cut to a fixed length, end-face drilled, machined, and hot extruded at 1190℃ to obtain a rough tube.
[0099] Step 2:
[0100] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1060℃, the holding time is 30min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1080℃, the holding time is 15min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 15s;
[0101] Step 3: After mixing epoxy resin E51 and ethylenediamine in a weight ratio of 0.75:1, a coating with a thickness of 1.5 mm is applied to the surface and wall of the cooled and dried steel pipe, and then cured to obtain an austenitic stainless steel seamless pipe.
[0102] Comparative Example 2: The content of organosilicon grafted carbonate in the carbonate mixture was increased, and the other parameters were the same as those in Example 2.
[0103] Step 1:
[0104] The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high-temperature homogenization heat treatment at 1200℃ for 95h. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1100℃, the final forging temperature is 900℃, and the total forging elongation coefficient is 5. The tube blanks are cut to a fixed length, end-face drilled, machined, and hot extruded at 1200℃ to obtain rough tubes.
[0105] Step 2:
[0106] After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1070℃, the holding time is 30min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1085℃, the holding time is 20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 20s;
[0107] Step 3: After the cooled steel pipe is dried, the surface and the wall of the pipe are coated with a 1.5 mm thick organic silicon modified coating, and cured to obtain an austenitic stainless steel seamless pipe; wherein the preparation method of the organic silicon modified coating is:
[0108] S1: Disperse vinyl ethylene carbonate in isopropanol, use chloroplatinic acid as a catalyst, heat to 70°C under nitrogen protection, add polymethyl hydrogen siloxane dropwise with stirring for 1.5 hours, heat to 85°C, react for 10 hours, and then distill under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:1;
[0109] S2: Castor oil is added to an acetic acid solution, urea is used as a stabilizer, and the mixture is stirred for 15 minutes and then heated to 40°C. A mixed solution of hydrogen peroxide and phosphoric acid is added dropwise, and the mixture is heated to 65°C after the addition is complete, and the mixture is reacted for 2.5 hours. After the reaction is completed, the mixture is washed until it is neutral, the oil layer is separated, and the epoxy-modified castor oil is obtained by vacuum distillation. The weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:70:2:25:0.5.
[0110] S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize to 2.5 MPa, stir and heat to 125°C, maintain the pressure reaction for 13 hours, remove impurities and obtain carbonate castor oil;
[0111] S4: adding organosilicon-grafted carbonate to carbonate castor oil at a weight ratio of 1:3 to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine at a molar ratio of carbonate group to amine group of 1:2.5, heating to 85° C. to react for 7 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer;
[0112] S5: Using an organic mixed solution, the terminal amine-containing silicon-containing prepolymer is diluted into a curing agent with a solid content of 70%, and mixed at a weight ratio of epoxy resin E51 and curing agent of 0.75:1; wherein the content of each component in the organic mixed solvent, by weight percentage, is 50% xylene, 30% n-butanol, and 20% benzyl alcohol.
[0113] Experiment: According to the preparation methods in Examples 1 to 6 and Comparative Examples 1 to 2, austenitic stainless steel seamless pipes with a length of 20 cm, an outer diameter of 5 cm, and a wall thickness of 0.3 cm were prepared for testing. The experimental results are shown in the following table.
[0114] Adhesion test: Test according to GB / T9286;
[0115] Corrosion resistance test: prepare 10% sulfuric acid solution, 10% sodium hydroxide solution and 5% sodium chloride solution respectively, immerse the sample completely in them, and observe the changes of the surface coating.
[0116]
[0117]
[0118] Conclusion: The data of Examples 1 to 6 and Comparative Examples 1 to 2 show that the austenitic stainless steel seamless pipe prepared by the present invention has good corrosion resistance. The data of Example 1 and Comparative Example 1 show that replacing the conventional curing agent with the terminal amine-containing silicon prepolymer prepared by the present invention can improve the tolerance of the coating under acid, alkali and salt conditions, and can ensure that it will not fall off during long-term use, thereby achieving the effect of protecting the steel pipe body; the data of Example 2 and Comparative Example 2 show that the excessive amount of organosilicon grafted carbonate in the terminal amine-containing silicon prepolymer has an adverse effect on the coating effect, which will lead to a decrease in adhesion and corrosion resistance.
[0119] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an austenitic stainless steel seamless pipe, characterized in that: The following steps are involved: Step 1: The stainless steel material is smelted by electroslag remelting process, cast into steel ingots, and then subjected to high temperature homogenization heat treatment at 1180-1250°C for 90-100 hours. After water cooling, the steel ingots are upset and stretched, and finally forged. The initial forging temperature is 1050-1200°C, the final forging temperature is 850-950°C, and the total forging elongation coefficient is 3-5. The tube blanks are cut to a certain length, end-face drilled, machined, and hot extruded at 1190-1220°C to obtain rough tubes. Step 2: After straightening, surface deburring and pickling of the rough pipe, two cold rolling processes are carried out to obtain the required finished product specifications. After each cold rolling, degreasing, solid solution heat treatment, straightening, pickling, internal and external surface inspection, grinding, internal and external polishing are carried out; the temperature of the first solid solution heat treatment is 1060-1080℃, the holding time is 30-35min, and the water is immersed in cooling; the temperature of the second solid solution heat treatment is 1080-1090℃, the holding time is 15-20min, and the water is immersed in cooling; after each solid solution heat treatment, the time interval from the steel pipe leaving the furnace to immersing in water is 15-25s; Step 3: After the cooled steel pipe is dried, the surface and the wall of the steel pipe are coated with a 1-1.5 mm thick organic silicon modified coating, and the coating is cured to obtain an austenitic stainless steel seamless pipe; the preparation method of the organic silicon modified coating comprises the following steps: S1: dispersing vinyl ethylene carbonate in isopropanol, using chloroplatinic acid as a catalyst, under nitrogen protection, heating to 60-70°C, adding polymethyl hydrogen siloxane dropwise with stirring for 1-1.5h, heating to 80-85°C, reacting for 9-12h, and distilling under reduced pressure to obtain organosilicon grafted carbonate; wherein the active hydrogen of polymethyl hydrogen siloxane and vinyl ethylene carbonate react in a molar ratio of 1:(0.8-1); S2: Add castor oil to acetic acid solution, use urea as a stabilizer, stir for 10-15 minutes, then heat to 35-40°C, add a mixed solution of hydrogen peroxide and phosphoric acid dropwise, continue to heat to 60-65°C after the addition, and react for 2-3 hours; after the reaction is completed, wash until it is neutral, separate the oil layer, and distill under reduced pressure to obtain epoxy-modified castor oil; wherein the weight ratio of castor oil, hydrogen peroxide, phosphoric acid, acetic acid, and urea is 100:(70-75):(2-2.5):(25-28):(0.3-0.5); S3: Take epoxy-modified castor oil, use tetrabutylammonium bromide as a catalyst, mix and pressurize, stir and heat, maintain the pressure for 12 to 15 hours, remove impurities and obtain carbonate castor oil; S4: adding organic silicon grafted carbonate to carbonate castor oil to obtain a carbonate mixture; dispersing the carbonate mixture in toluene, adding ethylenediamine, heating to 80-90° C. for reaction for 6-8 hours, and distilling under reduced pressure to obtain an amine-terminated silicon-containing prepolymer; wherein the carbonate mixture and ethylenediamine react at a molar ratio of carbonate group to amine group of 1:(2.3-2.5); in the carbonate mixture, the weight ratio of organic silicon grafted carbonate to carbonate castor oil is 1:(8-10); S5: using an organic mixed solution to dilute the terminal amine-containing silicon-containing prepolymer to obtain a curing agent, and mixing the epoxy resin E51 and the curing agent.
2. The method for preparing an austenitic stainless steel seamless pipe according to claim 1, characterized in that: In S3, the reaction pressure is 2-2.5 MPa, and the reaction temperature is 120-130°C.
3. The method for preparing an austenitic stainless steel seamless pipe according to claim 1, characterized in that: In S5, the content of each component in the organic mixed solvent is, by weight percentage, 50-60% of xylene, 20-30% of n-butanol, and 20-30% of benzyl alcohol.
4. The method for preparing an austenitic stainless steel seamless pipe according to claim 1, characterized in that: In S5, the solid content of the curing agent is 65-75%; the epoxy resin E51 and the curing agent are mixed in a weight ratio of (0.75-0.8):
1.
5. An austenitic stainless steel seamless pipe prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Austenitic stainless steel seamless tube for reactor internal of sodium-cooled fast reactor and manufacturing method
CN112322971A