A fire-resistant flame-retardant composite material board and preparation method thereof
By using a combination of porous carbon-based thermal insulation layer and modified ammonium polyphosphate in glass fiber reinforced thermoset composite materials, the problem of poor compatibility between traditional materials and flame retardant at high temperatures is solved, and high light transmission is achieved. The flame retardant and impact resistance are improved to achieve the effect of combustion grade B1.
Patent Information
- Application Number
- CN202410888132.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-04
AI Technical Summary
Traditional glass fiber reinforced thermoset composite materials are prone to combustion at high temperatures, and the addition of flame retardant will affect the mechanical properties of the material and increase costs. The compatibility of DOPO and ammonium polyphosphate in existing flame retardant coatings is poor, making it difficult to achieve high resistance. Fueling performance.
The water resistance and long-chain melamine-formaldehyde resin formed by a porous carbon-based insulation layer and modified ammonium polyphosphate is improved by modifying the combination of melamine, melamine, formaldehyde and ammonium polyphosphate. Effective flame retardancy and form a uniform flame retardant coating between the substrate layer and the refractory flame retardant layer.
It has achieved excellent flame retardant, impact resistance and tensile strength properties while having high light transmittance. The flame retardant effect reaches combustion grade B1 level, and the compatibility and flame retardant performance of the material are significantly improved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of board materials, and in particular to a fire-resistant and flame-retardant composite material board and a preparation method thereof. Background Art
[0002] Glass fiber reinforced thermosetting composites have excellent mechanical properties and low cost. However, thermosetting composites are easy to burn at high temperatures, which brings hidden dangers to safety during use. Therefore, research and development of glass fiber reinforced thermosetting composites with flame retardant properties has become one of the current research hotspots.
[0003] Traditional flame retardant methods include adding flame retardants, using flame retardant fillers and applying flame retardant coatings. Adding flame retardants is a common method that can reduce the combustion performance of materials through chemical reactions or physical effects. However, adding flame retardants will have a negative impact on the mechanical properties and processing properties of the material. In addition, the use of flame retardants will also increase the cost of the material. Compared with traditional flame retardant methods, flame retardant coatings are a more effective method.
[0004] Flame retardant coating can form a flame retardant protective layer on the surface of the material, thereby effectively improving the flame retardant performance of the material. Flame retardant coating can use inorganic flame retardants, organic flame retardants, nanomaterials, etc. as the main ingredients, and has the characteristics of fire prevention, flame retardancy, and high temperature resistance. Flame retardant coating can not only improve the flame retardant performance of the material, but also protect the surface of the material and extend the service life of the material.
[0005] Patent technical document CN106189566B discloses a flame retardant coating for the surface of engineering plastics and a preparation method thereof, which belongs to the technical field of flame retardant coatings. The flame retardant coating is made of DOPO, ammonium polyphosphate, a film former, a carbon former, a wetting agent and anhydrous ethanol. However, the compatibility between DOPO and ammonium polyphosphate is poor, and it is difficult to fully and evenly disperse them, which will lead to the need to add more flame retardants if higher flame retardant performance is to be achieved, which will inevitably affect the mechanical properties of the flame retardant layer. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a fire-resistant flame-retardant composite material board and a preparation method thereof, so as to provide a fire-resistant flame-retardant composite material board which has good light transmittance and is flame-retardant and impact-resistant.
[0007] Based on the above purpose, the present invention provides a porous carbon-based thermal insulation layer to isolate oxygen and temperature from the fire-resistant and flame-retardant composite material board, including a substrate layer and fire-resistant and flame-retardant layers located on the upper and lower surfaces.
[0008] Furthermore, the fire-resistant and flame-retardant layer is prepared from the following raw materials in parts by weight: 80-120 parts of base resin, 80-120 parts of fire-resistant and flame-retardant additives, 0.1-0.5 parts of antioxidants, 0.1-0.5 parts of anti-ultraviolet absorbers, 0.1-5 parts of lubricants, 1-3 parts of curing agents, and 1-3 parts of accelerators;
[0009] Preferably, the fire-resistant flame-retardant additive is obtained by mixing the following raw materials in parts by weight: 1-50 parts of pentaerythritol, 10-50 parts of melamine, and 10-50 parts of modified ammonium polyphosphate;
[0010] More preferably, the fire-resistant flame-retardant additive is obtained by mixing the following raw materials in parts by weight: 20-30 parts of pentaerythritol, 20-40 parts of melamine, and 40-50 parts of modified ammonium polyphosphate.
[0011] Preferably, the preparation steps of the modified ammonium polyphosphate are as follows:
[0012] S11: mixing stearyl chloride, melamine and N,N-dimethylformamide, then heating to 80° C., reacting for 5-7 hours, purifying and drying to obtain modified melamine;
[0013] S12: adding modified melamine, melamine and 37% formaldehyde aqueous solution into deionized water, adjusting the pH of the solution to between 8 and 9 with 10 wt% sodium carbonate, heating to 80° C., reacting for 30 to 40 minutes, and obtaining a modified melamine-formaldehyde prepolymer;
[0014] S13: 60 g of ammonium polyphosphate is dispersed in 150 g of ethanol, and then a modified melamine-formaldehyde prepolymer is added, and the pH value of the solution is adjusted to 3-4 with acetic acid, and the temperature is raised to 80° C., and the reaction is performed for 2-4 hours, and the modified ammonium polyphosphate is obtained by suction filtration, washing, and drying.
[0015] Preferably, the weight ratio of melamine, stearyl chloride and N,N-dimethylformamide in step S11 is 1.3:3:22.
[0016] Preferably, in step S12, the weight ratio of the modified melamine, melamine, 37% formaldehyde aqueous solution and deionized water is 3:7:20:50.
[0017] Preferably, in step S13, the weight ratio of ammonium polyphosphate, ethanol and modified melamine-formaldehyde prepolymer is 60:150:80.
[0018] Preferably, the substrate layer is glass fiber reinforced plastic.
[0019] Preferably, the thickness of the substrate layer is 0.5-10 mm, and the thickness of the fire-resistant and flame-retardant layer is 10-1000 μm.
[0020] More preferably, the thickness of the substrate layer is 1-5 mm, and the thickness of the fire-resistant and flame-retardant layer is 100-400 μm.
[0021] Preferably, the matrix resin is a thermosetting resin such as unsaturated polyester resin, epoxy resin, polyurethane resin, phenolic resin, acrylic resin, etc.
[0022] Preferably, the unsaturated polyester resin is any one of propylene glycol phthalate type, neopentyl glycol phthalate type, propylene glycol isophthalate type, and ethylene glycol isophthalate type.
[0023] Preferably, the antioxidant is one of hindered phenols, hydroxy compounds, phosphates, imines and the like.
[0024] Preferably, the lubricant is pentaerythritol stearate.
[0025] Preferably, the anti-ultraviolet absorber is one of triazine, salicylate, benzophenone, benzotriazole, nickel complex ultraviolet absorbers and the like.
[0026] Preferably, the curing agent is one of methyl ethyl ketone peroxide, cumene hydroperoxide, and benzoyl peroxide.
[0027] Preferably, the promoter is cobalt naphthenate.
[0028] Furthermore, the present invention also provides a method for preparing a fire-resistant and flame-retardant composite material board, and the specific preparation steps are as follows:
[0029] S21: uniformly mixing the base resin, the fire-resistant flame retardant additive, the antioxidant, the anti-ultraviolet absorber, the lubricant, the curing agent, and the accelerator to obtain a fire-resistant flame retardant coating;
[0030] S22: Apply the fire-resistant flame retardant coating on one side of the release film, then spread the substrate layer on the surface of the fire-resistant flame retardant coating away from the release film, then apply the fire-resistant flame retardant coating on the surface of the substrate layer away from the side of the fire-resistant flame retardant coating, and finally stick the release film on the surface of the fire-resistant flame retardant coating, roll and heat to obtain a fire-resistant flame retardant composite material board.
[0031] Beneficial effects of the present invention:
[0032] (1) Compared with the traditional glass fiber reinforced thermosetting composite material plate, the fire-resistant flame-retardant composite material plate provided by the present invention has an overall flame retardancy, and not only has excellent flame retardancy and high light transmittance, but also has excellent tensile strength and impact resistance.
[0033] (2) When the fire-resistant flame-retardant composite material board provided by the present invention encounters fire, a porous carbon-based heat-insulating flame-retardant layer with a certain thickness will be formed on the surface of the board, thereby ensuring that the flame retardant effect can reach the combustion classification B1 level.
[0034] (3) The present invention uses a melamine-formaldehyde resin containing a hydrophobic long chain formed by modified melamine, melamine, formaldehyde and ammonium polyphosphate to encapsulate ammonium polyphosphate, which effectively improves the water resistance and long-term flame retardancy of ammonium polyphosphate, and at the same time, improves the compatibility between ammonium polyphosphate and the matrix resin. DETAILED DESCRIPTION
[0035] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0036] In a specific embodiment of the present invention, the viscosity of the propylene glycol phthalate type unsaturated resin at 25° C. is 250 mPa·s.
[0037] Example 1: A method for preparing a fire-resistant and flame-retardant composite material board, the specific preparation steps are as follows:
[0038] (1) 3 g of stearyl chloride, 1 g of melamine and 22 g of N,N-dimethylformamide were mixed, then heated to 80°C, reacted for 6 h, purified and dried to obtain modified melamine;
[0039] (2) 3 g of modified melamine, 7 g of melamine, and 20 g of a 37% formaldehyde aqueous solution were added to 50 g of deionized water, and then the pH of the solution was adjusted to 8.3 with 10 wt% sodium carbonate, the temperature was raised to 80°C, and the reaction was carried out for 33 minutes to obtain a modified melamine-formaldehyde prepolymer;
[0040] (3) Dispersing 60 g of ammonium polyphosphate in 150 g of ethanol, then adding 80 g of modified melamine-formaldehyde prepolymer, adjusting the pH value of the solution to 3.2 with acetic acid, heating to 80°C, reacting for 2.5 h, filtering, washing, and drying to obtain modified ammonium polyphosphate;
[0041] (4) 80 g of propylene glycol phthalate type unsaturated resin, 20 g of pentaerythritol, 20 g of melamine, 40 g of modified ammonium polyphosphate, 0.1 g of antioxidant 1135, 0.1 g of anti-ultraviolet absorber Eversorb 41 FD, 0.1 g of pentaerythritol stearate, 2 g of methyl ethyl ketone peroxide, and 1 g of cobalt cyclohexane acid were mixed uniformly to obtain a fire-resistant flame-retardant coating;
[0042] (5) Apply the fire-resistant flame-retardant coating on one side of the release film, then spread the substrate layer on the surface of the fire-resistant flame-retardant coating on the side away from the release film, then apply the fire-resistant flame-retardant coating on the surface of the substrate layer on the side away from the fire-resistant flame-retardant coating, and finally attach the release film to the surface of the fire-resistant flame-retardant coating, roll-press, heat and shape, and obtain a fire-resistant flame-retardant composite material board.
[0043] Embodiment 2: A method for preparing a fire-resistant flame-retardant composite material board, the specific preparation steps are as follows:
[0044] (1) 3 g of stearoyl chloride, 1.3 g of melamine and 22 g of N,N-dimethylformamide were mixed, then heated to 80°C, reacted for 6 h, purified and dried to obtain modified melamine;
[0045] (2) 3 g of modified melamine, 7 g of melamine, and 20 g of a 37% formaldehyde aqueous solution were added to 50 g of deionized water, and then the pH of the solution was adjusted to 8.8 with 10 wt% sodium carbonate, the temperature was raised to 80°C, and the reaction was carried out for 35 minutes to obtain a modified melamine-formaldehyde prepolymer;
[0046] (3) Dispersing 60 g of ammonium polyphosphate in 150 g of ethanol, then adding 80 g of modified melamine-formaldehyde prepolymer, adjusting the pH value of the solution to 3.6 with acetic acid, heating to 80° C., reacting for 3 h, filtering, washing, and drying to obtain modified ammonium polyphosphate;
[0047] (4) 100 g of propylene glycol phthalate type unsaturated resin, 25 g of pentaerythritol, 30 g of melamine, 45 g of modified ammonium polyphosphate, 0.3 g of antioxidant 1135, 0.2 g of anti-ultraviolet absorber Eversorb 41 FD, 1.5 g of pentaerythritol stearate, 2 g of methyl ethyl ketone peroxide, and 2 g of cobalt cyclohexane acid were mixed uniformly to obtain a fire-resistant flame-retardant coating;
[0048] (5) Apply the fire-resistant flame-retardant coating on one side of the release film, then spread the substrate layer on the surface of the fire-resistant flame-retardant coating on the side away from the release film, then apply the fire-resistant flame-retardant coating on the surface of the substrate layer on the side away from the fire-resistant flame-retardant coating, and finally attach the release film to the surface of the fire-resistant flame-retardant coating, roll-press, heat and shape, and obtain a fire-resistant flame-retardant composite material board.
[0049] Embodiment 3: A method for preparing a fire-resistant flame-retardant composite material board, the specific preparation steps are as follows:
[0050] (1) 3 g of stearoyl chloride, 1.5 g of melamine and 22 g of N,N-dimethylformamide were mixed, then heated to 80°C, reacted for 6.5 h, purified and dried to obtain modified melamine;
[0051] (2) 3 g of modified melamine, 7 g of melamine, and 20 g of a 37% formaldehyde aqueous solution were added to 50 g of deionized water, and then the pH of the solution was adjusted to 8.8 with 10 wt% sodium carbonate, the temperature was raised to 80°C, and the reaction was carried out for 30-40 minutes to obtain a modified melamine-formaldehyde prepolymer;
[0052] (3) Dispersing 60 g of ammonium polyphosphate in 150 g of ethanol, then adding 80 g of modified melamine-formaldehyde prepolymer, adjusting the pH value of the solution to 3.8 with acetic acid, heating to 80°C, reacting for 3.5 h, filtering, washing, and drying to obtain modified ammonium polyphosphate;
[0053] (4) 120 g of propylene glycol phthalate type unsaturated resin, 30 g of pentaerythritol, 40 g of melamine, 50 g of modified ammonium polyphosphate, 0.5 g of antioxidant 1135, 0.5 g of anti-ultraviolet absorber Eversorb 41 FD, 5 g of pentaerythritol stearate, 3 g of methyl ethyl ketone peroxide, and 3 g of cobalt cyclohexane acid were mixed uniformly to obtain a fire-resistant flame-retardant coating;
[0054] (5) Apply the fire-resistant flame-retardant coating on one side of the release film, then spread the substrate layer on the surface of the fire-resistant flame-retardant coating on the side away from the release film, then apply the fire-resistant flame-retardant coating on the surface of the substrate layer on the side away from the fire-resistant flame-retardant coating, and finally attach the release film to the surface of the fire-resistant flame-retardant coating, roll-press, heat and shape, and obtain a fire-resistant flame-retardant composite material board.
[0055] Comparative Example 1:
[0056] The difference between Comparative Example 1 and Example 2 is that the modified ammonium polyphosphate in step (4) is replaced by ammonium polyphosphate.
[0057] Comparative Example 2:
[0058] The difference between Comparative Example 2 and Example 2 is that: (2) 7 g of modified melamine, 3 g of melamine, and 20 g of 37% formaldehyde aqueous solution are added to 50 g of deionized water, and then the pH of the solution is adjusted to 8.8 with 10 wt % sodium carbonate, the temperature is raised to 80° C., and the reaction is carried out for 35 minutes to obtain a modified melamine-formaldehyde prepolymer.
[0059] Comparative Example 3:
[0060] The difference between Comparative Example 3 and Example 2 is that the stearoyl chloride in step (1) is replaced by nonanoyl chloride. Performance test:
[0061] Light transmittance: Tested according to ASTM D1003 standard, the sample size is 90 mm × 80 mm × 3.2 mm, 5 different positions of the sample are selected for testing, and the final data is averaged. The test results are shown in Table 1;
[0062] Flame retardant performance test: UL-94 horizontal and vertical combustion test machine was used to test according to UL-94 test standard. The test results are shown in Table 1;
[0063] Impact strength test: The test was carried out using a plastic drop weight impact tester in accordance with GB / T1043-1993, at room temperature. The test results are shown in Table 1.
[0064] Tensile strength: The test was carried out using a universal tensile strength testing machine. The test results are shown in Table 1;
[0065] Fire resistance performance test: The fire resistance test was carried out according to GB / T 9978.1-2008 standard, the sample size was 500mm×500mm×3mm, and the test results are shown in Table 1.
[0066] Table 1 Performance test results of fire-resistant and flame-retardant composite panels prepared in Examples 1-3 and Comparative Examples 1-3
[0067]
[0068] Data analysis: It can be seen from Examples 1-3 in Table 1 that the fire-resistant and flame-retardant composite material plates prepared by the present invention have high transparency, impact strength and good tensile strength, the vertical combustion grade reaches V-0, and there is no molten dripping phenomenon during combustion, the fire resistance limit is ≥3h, and the combustion grade reaches B1.
[0069] It can be seen from Example 2 and Comparative Examples 1-3 that directly adding ammonium polyphosphate to the fire-resistant flame-retardant composite material board will lead to a decrease in flame retardancy and impact strength, which is mainly due to the agglomeration of ammonium polyphosphate and the poor compatibility between ammonium polyphosphate and the polycarbonate substrate. When the modified ammonium polyphosphate prepared by the present invention is used, the flame retardancy, impact strength and tensile strength are improved. This may be because the long hydrophobic chain improves the compatibility of ammonium polyphosphate with unsaturated resins. At the same time, the long hydrophobic chain can improve the elasticity of the melamine-formaldehyde resin on the surface of ammonium polyphosphate. After adding the unsaturated resin, the energy brought by the impact can be effectively released through elastic deformation, thereby improving the impact resistance. Moreover, the longer the chain length of the hydrophobic long chain, the greater the improvement in its impact resistance. When the proportion of modified melamine in the modified ammonium polyphosphate is large, it will lead to a significant decrease in impact resistance. This may be caused by the reduction in the cross-linking density of the system when the proportion of modified melamine is large.
[0070] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0071] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A fire-resistant and flame-retardant composite material board, characterized in that: It includes a base material layer and fire-resistant and flame-retardant layers located on the upper and lower surfaces; The fire-resistant and flame-retardant layer is prepared from the following raw materials in parts by weight: 80-120 parts of base resin, 80-120 parts of fire-resistant and flame-retardant additives, 0.1-0.5 parts of antioxidants, 0.1-0.5 parts of anti-ultraviolet absorbers, 0.1-5 parts of lubricants, 1-3 parts of curing agents, and 1-3 parts of accelerators; The fire-resistant flame-retardant additive is obtained by mixing the following raw materials in parts by weight: 1-50 parts of pentaerythritol, 10-50 parts of melamine, and 10-50 parts of modified ammonium polyphosphate; The preparation steps of the modified ammonium polyphosphate are as follows: S11: mixing stearyl chloride, melamine and N,N-dimethylformamide, then heating to 80° C., reacting for 5-7 hours, purifying and drying to obtain modified melamine; S12: adding modified melamine, melamine and 37% formaldehyde aqueous solution into deionized water, adjusting the pH of the solution to between 8 and 9 with 10 wt% sodium carbonate, heating to 80° C., reacting for 30 to 40 minutes, and obtaining a modified melamine-formaldehyde prepolymer; S13: dispersing 60 g of ammonium polyphosphate in 150 g of ethanol, then adding modified melamine-formaldehyde prepolymer, adjusting the pH value of the solution to 3-4 with acetic acid, heating to 80° C., reacting for 2-4 h, filtering, washing, and drying to obtain modified ammonium polyphosphate; The weight ratio of melamine, stearyl chloride and N,N-dimethylformamide in step S11 is 1-1.5:3:22; the weight ratio of modified melamine, melamine, 37% formaldehyde aqueous solution and deionized water in step S12 is 3:7:20:50; the weight ratio of ammonium polyphosphate, ethanol and modified melamine-formaldehyde prepolymer in step S13 is 60:150:80; The matrix resin is one of unsaturated polyester resin, epoxy resin, polyurethane resin, phenolic resin and acrylic resin.
2. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The substrate layer is glass fiber reinforced plastic.
3. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The thickness of the substrate layer is 0.5-10 mm, and the thickness of the fire-resistant and flame-retardant layer is 10-1000 μm.
4. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The antioxidant is one of hindered phenols, hydroxy compounds, phosphates and imines.
5. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The anti-ultraviolet absorber is one of triazine, salicylate, benzophenone, benzotriazole and nickel complex ultraviolet absorbers.
6. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The lubricant is pentaerythritol stearate.
7. The fire-resistant and flame-retardant composite material board according to claim 1, characterized in that: The curing agent is one of methyl ethyl ketone peroxide, cumene hydroperoxide and benzoyl peroxide.
8. A method for preparing a fire-resistant and flame-retardant composite material board according to any one of claims 1 to 7, characterized in that: The specific preparation steps are as follows: S21: uniformly mixing the base resin, the fire-resistant flame retardant additive, the antioxidant, the anti-ultraviolet absorber, the lubricant, the curing agent, and the accelerator to obtain a fire-resistant flame retardant coating; S22: Apply the fire-resistant flame retardant coating on one side of the release film, then spread the substrate layer on the surface of the fire-resistant flame retardant coating away from the release film, then apply the fire-resistant flame retardant coating on the surface of the substrate layer away from the side of the fire-resistant flame retardant coating, and finally stick the release film on the surface of the fire-resistant flame retardant coating, roll and heat to obtain a fire-resistant flame retardant composite material board.
Citation Information
Patent Citations
A kind of intumescent flame retardant coating used on the surface of engineering plastics and its preparation method
CN106189566B
Method for preparing phosphorus-nitrogen flame-retardant epoxy resin
CN107033549A
Composite fireproof coating and preparation method thereof
CN108948946A
Green energy-saving internal wall paint
CN109810600A
High-transmittance halogen-free flame-retardant composite board with sandwich structure