A method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution
Through the methods of swelling while stirring at room temperature and thermal swelling at rising temperatures, the problem of poor solubility of dry high molecular weight polyacrylonitrile spinning dope is solved, efficient spinning dope uniformity and stability are achieved, and production efficiency and product quality.
Patent Information
- Application Number
- CN202410876831.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-02
AI Technical Summary
It is difficult to effectively improve the dissolution performance of dry high molecular weight polyacrylonitrile spinning dope with existing technology, resulting in poor spinning quality and low production efficiency.
By swelling at room temperature while stirring, and then heating up for thermal swelling and dissolution, the stirring speed and heating rate are controlled to ensure full contact and uniform mixing of the polyacrylonitrile powder and the solvent, thereby improving dissolution efficiency and uniformity.
Significantly improves the solubility performance of dry high molecular weight polyacrylonitrile spinning dope, ensures product quality stability and production efficiency, and reduces scrap rate and thermal stress damage.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyacrylonitrile spinning, and particularly relates to a method for improving the solubility of dry-process high-molecular-weight polyacrylonitrile spinning stock solution. Background Art
[0002] Carbon fiber is an inorganic polymer fiber with a carbon content of more than 95%. Advanced composite materials with carbon fiber as reinforcement have a series of excellent properties such as high specific strength, high specific modulus, strong designability, high temperature resistance, corrosion resistance, fatigue resistance and small thermal expansion coefficient. Its excellent performance makes it widely used in aerospace, rail transportation, vehicle manufacturing, weapons and equipment, engineering machinery, wind energy, sports goods and other fields.
[0003] Polyacrylonitrile-based fiber is the most promising precursor for producing high-performance carbon fiber. It is formed by spinning, pre-oxidation, and carbonization of polyacrylonitrile. Carbon fiber prepared from polyacrylonitrile has excellent properties such as high tensile strength and high tensile modulus. High-quality polyacrylonitrile precursor is the primary condition for preparing high-performance polyacrylonitrile carbon fiber, and high-quality spinning solution is the key factor restricting the preparation of high-performance precursor. The rheology and spinnability of the spinning solution are important reference factors for judging spinning, and the solubility of the polymer is closely related to the spinning quality.
[0004] High-quality polyacrylonitrile precursor requires a higher degree of polymerization and molecular weight to increase the interaction between macromolecules, thereby obtaining a higher tensile strength. However, since polyacrylonitrile is a linear molecular chain polymer with coexistence of crystalline and amorphous states, during the dissolution process, it is more difficult for small solvent molecules to penetrate into the polyacrylonitrile molecular chain and for the molecular chain itself to diffuse into the solvent than for pure amorphous polymers. In addition, the dry spinning process requires that the molecular weight and solid content of polyacrylonitrile in the spinning solution are both high, which further increases the difficulty of dissolution.
[0005] At present, some literatures mention that adding a certain amount of water can help dissolve high molecular weight polyacrylonitrile, but the presence of water in the stock solution is not conducive to the swelling system and will reduce the viscosity of the stock solution. Some literatures also suggest reducing the concentration of polymers in the stock solution, but when the polymer concentration is too low, the viscosity of the stock solution will also decrease, resulting in insufficient solvent volatilization in the primary silk, easy formation of sticky silk, poor fiber molding stability, and poor quality of the finished fiber.
[0006] Patent CN114457448A introduces a method for improving the solubility of dry-process high molecular weight polyacrylonitrile by mixing three solvents: dimethylacetamide, dimethylformamide and dimethyl sulfoxide. Dimethylformamide has a strong dissolving ability but is highly toxic, and the mixed dissolution of the two solvents adds a certain degree of difficulty to the subsequent recovery of the solvent. Summary of the invention
[0007] In order to solve the technical problems existing in the background technology, the present invention provides a method for improving the solubility performance of dry-process high molecular weight polyacrylonitrile spinning solution. The process is simple and easy to operate. Under the premise of ensuring a high solid content of the polyacrylonitrile spinning solution, the swelling degree of the solution is increased, the uniformity of the spinning solution is improved, and thus the product quality of the primary silk is improved.
[0008] The technical solution adopted by the present invention to solve the technical problem is: a method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution, characterized in that the dissolution step comprises:
[0009] 1) Evenly dispersing polyacrylonitrile powder in dimethylacetamide solvent to prepare polyacrylonitrile solution, wherein the viscosity average molecular weight of the polyacrylonitrile powder is 60,000 to 100,000, and the solid content of the obtained polyacrylonitrile solution is 26% to 30%;
[0010] 2) Under stirring conditions, the polyacrylonitrile solution is swollen at room temperature for 1h~6h, and the stirring speed is 80r / min~240r / min;
[0011] 3) Raise the temperature to 60℃~80℃, continue thermal swelling for 1h~4h, and stir at a speed between 150r / min~300r / min;
[0012] 4) Heat to 85℃~105℃ for dissolution, dissolve for 4h~8h, and control the stirring speed at 150r / min~300r / min.
[0013] Due to the complex molecular shape and aggregate structure, the dissolution process of polymers is difficult and slow, and needs to go through two stages: swelling and dissolution. Swelling is the process in which the interaction between polymer macromolecules is continuously weakened under the action of solvents, and the solvent molecules gradually penetrate into the interior of the macromolecules from the outside to the inside, causing the polymer volume to expand. Dissolution is the process in which macromolecules gradually diffuse into the solvent to form a uniform solution.
[0014] If the high molecular weight polymer is dissolved without being fully swollen, a high viscosity layer will be formed at the polymer-solvent interface, hindering the diffusion of solvent molecules into the polymer and affecting the uniformity of the polymer solution.
[0015] The present invention first adopts a method of swelling while stirring at room temperature to allow solvent molecules to fully enter the interior of the polymer, and then heats the swelling-dissolving process to allow the polymer stock solution to reach a uniform swelling state, thereby further improving the dissolution rate of the polymer stock solution and providing uniform and high-quality spinning stock solution for subsequent products.
[0016] Preferably, the water content of the polyacrylonitrile powder in step 1) of the above dissolution method is less than 0.5%. Controlling the water content of the polyacrylonitrile powder to be less than 0.5% not only helps to improve the dissolution efficiency and product stability, but also reduces the occurrence of adverse reactions.
[0017] Preferably, the viscosity average molecular weight of the polyacrylonitrile powder in step 1) of the above dissolution method is 63,000 to 80,000, and the solid content of the obtained polyacrylonitrile solution is controlled to be 26% to 28%. The viscosity average molecular weight of the polyacrylonitrile powder and the solid content of the obtained polyacrylonitrile solution preferably within the above range are more conducive to improving the spinning performance, ensuring stable product quality, improving production efficiency and reducing the scrap rate.
[0018] Preferably, the swelling time at room temperature in step 2) of the above dissolution method is 3h to 5h; the stirring speed is 100r / min to 140r / min. Preferably, the polyacrylonitrile molecules can fully swell and absorb the solvent under the swelling at room temperature, ensuring the uniformity of the dissolution inside and outside the polyacrylonitrile molecules and reducing the difficulty of the subsequent thermal dissolution stage.
[0019] Preferably, the swelling temperature of the thermal swelling in step 3) of the above dissolution method is 60°C, 70°C or 80°C; when the swelling temperature is 60°C, the swelling time is 1h; when the swelling temperature is 70°C, the swelling time is 2h; when the swelling temperature is 80°C, the swelling time is 1h~2h. According to different swelling temperatures combined with different swelling times, the interaction between polyacrylonitrile molecules and solvents can be promoted, accelerating the dissolution process. Different swelling times at different temperatures can make polyacrylonitrile dissolve faster and more thoroughly.
[0020] Preferably, the dissolution temperature in step 4) of the above dissolution method is 90°C to 95°C, and the dissolution time is 5h to 7h. The preferred dissolution process conditions can ensure that the polyacrylonitrile is completely dissolved in the solvent, avoid the occurrence of residues or agglomeration, and ensure the uniformity and stability of the solution.
[0021] Preferably, the stirring speed during thermal swelling in step 3) of the above dissolution method is 170 r / min to 230 r / min; the stirring speed during dissolution in step 4) is 170 r / min to 230 r / min. During thermal swelling and dissolution, a more appropriate stirring speed can ensure uniform mixing of the solution and promote the dissolution of the polymer.
[0022] Preferably, the heating rate in step 3) and step 4) of the above dissolution method is controlled at 4.5°C / 30min~5.5°C / 30min. The heating rate is controlled to reduce the thermal stress on polyacrylonitrile during the heating process. The slow heating rate helps the polyacrylonitrile molecules absorb heat more evenly, avoiding stress concentration caused by excessive local temperature gradients, thereby reducing possible thermal stress damage and helping to improve the uniformity and quality stability of the product.
[0023] Compared with the prior art, the working principle and beneficial effects of the method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution of the present invention are as follows: the present invention significantly improves the solubility of dry-process high molecular weight polyacrylonitrile spinning solution by controlling key parameters such as dissolution temperature and time, stirring speed and heating rate in the optimization step. The dissolution temperature and time are precisely controlled to fully dissolve the polyacrylonitrile and ensure the uniformity and stability of dissolution; the appropriate stirring speed is adjusted to promote the diffusion and dissolution rate between molecules, and the dissolution efficiency and uniformity are improved; and the control of the heating rate can effectively reduce thermal stress, improve product quality stability, save energy, and improve operational safety and production efficiency. The dissolution method of the present invention can significantly improve the solubility of the product and improve production efficiency. DETAILED DESCRIPTION
[0024] The present invention is a method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution, which specifically comprises:
[0025] 1) Preparation of stock solution: Quickly remove the water from the polyacrylonitrile powder by flash drying, dry until the moisture content of the powder is less than 0.5%, crush the powder with a grinder, sieve it, and cool it to room temperature in a dryer. Pour the dimethylacetamide solvent into a stirring container, weigh the polyacrylonitrile powder, and slowly add it to the stirring container containing the dimethylacetamide solvent in batches, and pour it while stirring with a glass rod until the polyacrylonitrile powder is evenly dispersed in the solvent;
[0026] 2) Swelling at room temperature: The uniformly dispersed polyacrylonitrile solution is stirred and swelled at room temperature for 1h~6h at a speed of 80r / min~240r / min, until the polyacrylonitrile and dimethylacetamide solvent are evenly mixed to form a paste-like uniform solution;
[0027] 3) Thermal swelling: Heat the above homogenous solution to 60℃~80℃ and swell for 1h~4h, with the rotation speed controlled between 150r / min~300r / min, until the stock solution swells to a gelatinous state;
[0028] 4) Dissolution: Heat the above colloidal swelling stock solution to 85°C~105°C and dissolve it for 4h~8h, with the speed controlled at 150r / min~300r / min, until it dissolves into a transparent solution;
[0029] 5) Viscosity measurement: The viscosity of the above-mentioned clear solution was measured in a constant temperature water bath at 80°C using the falling ball method.
[0030] According to the above implementation mode, the following is further described through specific examples:
[0031] Example 1
[0032] Weigh 120g DMAC, add 43.27g polyacrylonitrile powder with a viscosity-average molecular weight of 65,300, evenly disperse the powder into the solvent to prepare a 26.5% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 3h, heat to 60℃ at a heating rate of 5.0℃ / 30min for swelling, adjust the speed to 200r / min and stir for 1h, heat to 70℃ at a heating rate of 5.0℃ / 30min and stir for 1h, heat to 80℃ and continue stirring for 1h, finally dissolve at 90℃ for 5h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0033] Example 2
[0034] Weigh 125g of DMAC, add 46.23g of polyacrylonitrile powder with a viscosity-average molecular weight of 65,800, evenly disperse the powder into the solvent to prepare a 27.0% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 4h, heat it to 70℃ at a heating rate of 5.0℃ / 30min for swelling, adjust the speed to 200r / min and stir for 2h, then heat it to 80℃ at a heating rate of 5.0℃ / 30min and continue stirring for 1h, finally dissolve it at 90-100℃ for 6h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0035] Example 3
[0036] Weigh 125g DMAC, add 45.07g polyacrylonitrile powder with a viscosity-average molecular weight of 68,000, evenly disperse the powder into the solvent to prepare a 26.5% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 5h, heat it to 70℃ at a heating rate of 5.0℃ / 30min for swelling, adjust the speed to 200r / min and stir for 2h, then heat it to 80℃ at a heating rate of 5.0℃ / 30min and continue stirring for 1h, finally dissolve it at 90-100℃ for 6h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0037] Example 4
[0038] Weigh 130g DMAC, add 50.55g polyacrylonitrile powder with a viscosity-average molecular weight of 63,000, evenly disperse the powder into the solvent to prepare a 28.0% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 4h, heat it to 70℃ at a heating rate of 4.5℃ / 30min for swelling, adjust the speed to 180r / min and stir for 2h, then heat it to 80℃ at a heating rate of 4.5℃ / 30min and continue stirring for 2h, finally dissolve it at 90-100℃ for 6h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0039] Example 5
[0040] Weigh 125g DMAC, add 43.92g polyacrylonitrile powder with a viscosity-average molecular weight of 77,600, evenly disperse the powder into the solvent to prepare a 26.0% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 4h, heat it to 70℃ at a heating rate of 5.5℃ / 30min for swelling, adjust the speed to 200r / min and stir for 2h, then heat it to 80℃ at a heating rate of 5.5℃ / 30min and continue stirring for 2h, finally dissolve it at 90-100℃ for 6h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0041] Example 6
[0042] Weigh 120g DMAC, add 43.27g polyacrylonitrile powder with a viscosity-average molecular weight of 65,300, evenly disperse the powder into the solvent to prepare a 26.5% uniform stock solution, swell while stirring at room temperature, the speed is 120r / min, after stirring for 3h, heat to 60℃ at a heating rate of 10℃ / 30min for swelling, adjust the speed to 200r / min and stir for 1h, heat to 70℃ at a heating rate of 10℃ / 30min and stir for 1h, heat to 80℃ and continue stirring for 1h, finally dissolve at 90℃ for 5h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0043] Comparative Example 1
[0044] Weigh 125g DMAC, add 46.23g polyacrylonitrile powder with a viscosity-average molecular weight of 65,600, evenly disperse the powder into the solvent to prepare a 27.0% uniform stock solution, heat to 60°C and swell at 160r / min for 1h, then heat to 70°C at a heating rate of 4.5°C / 30min~5.5°C / 30min, adjust the speed to 200r / min and stir for 2h, then heat to 80°C at a heating rate of 4.5°C / 30min~5.5°C / 30min and continue stirring for 1h, finally dissolve at 90-100°C for 5h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0045] Comparative Example 2
[0046] Weigh 125g DMAC, add 45.07g polyacrylonitrile powder with a viscosity-average molecular weight of 68,300, evenly disperse the powder into the solvent to prepare a 26.5% uniform stock solution, heat to 70℃ at a heating rate of 4.5℃ / 30min~5.5℃ / 30min, swell at 180r / min for 2h, heat to 80℃ at a heating rate of 4.5℃ / 30min~5.5℃ / 30min, adjust the speed to 200r / min and continue stirring for 1h, finally dissolve at 90-100℃ for 6h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0047] Comparative Example 3
[0048] Weigh 125g DMAC, add 43.92g polyacrylonitrile powder with a viscosity-average molecular weight of 77,600, evenly disperse the powder into the solvent to prepare a 26.0% uniform stock solution, heat to 70℃ at a heating rate of 4.5℃ / 30min~5.5℃ / 30min, swell at 180r / min for 2h, heat to 80℃ at a heating rate of 4.5℃ / 30min~5.5℃ / 30min, adjust the speed to 200r / min and continue stirring for 1h, finally dissolve at 90-100℃ for 7h, and measure the viscosity of the polymerization stock solution by the falling ball method.
[0049] Table 1 shows the spinnability and solubility of the spinning solutions prepared in the examples and comparative examples.
[0050]
[0051] From the test results in the above table we can see that:
[0052] Comparing samples with the same molecular weight and solid content, adding room temperature stirring swelling under the same dissolution process is beneficial to the full contact between the polyacrylonitrile powder and the solvent, forming a uniform stock solution, reducing the viscosity fluctuation of the polyacrylonitrile spinning stock solution, and preparing a transparent stock solution.
[0053] The dissolution process in Comparative Examples 1-3 did not adopt the method of the present invention. Compared with the samples of the same molecular weight and solid content in Examples 2, 3, and 5, it can be seen that the viscosity of the stock solution directly heated and swelled during the dissolution process is large, the climbing phenomenon is serious, the spinning continuity is poor, and the uniformity of the stock solution is also poor. This is because the overall polymer has not yet been fully contacted with the solvent, and the heating leads to inconsistent swelling and dissolution rates of the stock solution, which leads to uneven dissolution of the stock solution. The high viscosity leads to discontinuous spinning and easy formation of gel.
[0054] Based on the above, the embodiment of the method for improving the solubility of dry high molecular weight polyacrylonitrile spinning solution of the present invention is inspired. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of the present invention. The technical scope of the present invention is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution, characterized in that: The dissolution steps include: 1) Evenly dispersing polyacrylonitrile powder in dimethylacetamide solvent to prepare polyacrylonitrile solution, wherein the viscosity average molecular weight of the polyacrylonitrile powder is 60,000 to 100,000, and the solid content of the obtained polyacrylonitrile solution is 26% to 30%; 2) Under stirring conditions, the polyacrylonitrile solution is swollen at room temperature for 3h~5h, and the stirring speed is 100r / min~140r / min; 3) Raise the temperature to 60℃~80℃, continue thermal swelling for 1h~4h, and stir at a speed between 150r / min~300r / min; 4) Heat to 85℃~105℃ for dissolution, dissolve for 4h~8h, and control the stirring speed at 150r / min~300r / min.
2. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: The water content of the polyacrylonitrile powder in step 1) is lower than 0.5%.
3. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: The viscosity average molecular weight of the polyacrylonitrile powder in step 1) is 63,000 to 80,000, and the solid content of the obtained polyacrylonitrile solution is controlled to be 26% to 28%.
4. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: The swelling temperature of the thermal swelling in step 3) is 60°C, 70°C or 80°C; when the swelling temperature is 60°C, the swelling time is 1 hour; when the swelling temperature is 70°C, the swelling time is 2 hours; when the swelling temperature is 80°C, the swelling time is 1 hour to 2 hours.
5. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: The dissolution temperature in step 4) is 90°C to 95°C; and the dissolution time is 5h to 7h.
6. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: During the heat swelling in step 3), the stirring speed is 170 r / min to 230 r / min; during the dissolution in step 4), the stirring speed is 170 r / min to 230 r / min.
7. The method for improving the solubility of dry-process high molecular weight polyacrylonitrile spinning solution according to claim 1, characterized in that: The heating rate during heating in step 3) and step 4) is controlled at 4.5°C / 30min~5.5°C / 30min.
Citation Information
Patent Citations
Method for producing carbon fiber precursor fiber and carbon fiber
JP2009221647A