A toughened PP plastic barrel and preparation method thereof
By using loose agglomeration structure of POE resin and homemade composite toughener in polypropylene plastic barrels, combined with branched chain alkyl amide introduced by urethane exchange, the problem of easy damage of polypropylene plastic barrels is solved, and its strength is significantly improved and stability enhances the toughness and slip toughening effect of the material.
Patent Information
- Application Number
- CN202410663993.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Polypropylene plastic barrels are susceptible to external shocks and damage during shipment of large storage containers, resulting in media leakage, posing safety hazards, and limiting their application.
Using raw materials such as POE resin, homemade composite toughening agent and compatibility agent, the loose structure is formed through the agglomerated powder of bibranched silicone structure and ultramicro cordierite powder, and the branched chain-containing alkyl amide structure is introduced in combination with urethane exchange. Interface modification and β-phase crystallization are carried out to enhance the toughness of the PP substrate.
It significantly improves the strength and stability of PP plastic barrels, increases the toughness of the material, reduces the interfacial stress, reduces the initial microcrack generation, forms a slip toughening effect, and improves the tensile stress-strain curve performance of the material.
Smart Images

Figure CN118421008B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer composite materials, and in particular relates to a toughened PP plastic barrel and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a polymer formed by the addition polymerization of propylene. It is a colorless, translucent, thermoplastic, lightweight general-purpose plastic with chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear resistance processing properties. Compared with traditional polyethylene (PE), its strength and rigidity are better, making it an excellent material for barrel containers. However, polypropylene has average toughness, and it is inevitable that it will fail due to external impact during the transportation of large storage containers, which can easily cause leakage of the storage medium and pose a major safety hazard, greatly limiting the application of PP barrel materials. Summary of the invention
[0003] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a toughened PP plastic barrel and a preparation method thereof.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A toughened PP plastic barrel comprises the following raw materials in percentage by weight: 12-18wt% of POE resin, 5.5-8.5wt% of composite toughening agent, 0.25-0.3wt% of lubricant, 2.5-3.5% of compatibilizer, 0.1-0.15wt% of antioxidant and 0.1-0.12wt% of light stabilizer, and the balance is PP resin.
[0006] The composite toughening agent is prepared by the following method:
[0007] Step A1: premix diethyl diallylmalonate, dimethylphenylphosphine and anhydrous ethyl acetate, pass nitrogen gas for protection, then add 3-mercaptopropyltriethoxysilane and mix well, control the oil bath temperature at 45-55°C, apply 300-400W / m 2 UV irradiation, assisted by mechanical stirring at 80-120 rpm, reacted for 2.5-3 hours, and after the reaction was completed, ethyl acetate was removed by rotary evaporation to obtain a double-branched coupling matrix;
[0008] Furthermore, the dosage ratio of diallyl diethyl malonate, 3-mercaptopropyltriethoxysilane, dimethylphenylphosphine and anhydrous ethyl acetate is 0.1 mol: 0.202-0.206 mol: 80-100 mg: 150-200 mL, and under the initiation of dimethylphenylphosphine and ultraviolet radiation, the active thiol group of 3-mercaptopropyltriethoxysilane clicks with the unsaturated double bond of diallyl diethyl malonate.
[0009] Step A2: Mix the bibranched coupling matrix, dimethylacetamide and deionized water and stir and hydrolyze at room temperature for 30-40 minutes, then add ultrafine cordierite powder, disperse at 20-28kHz ultrasonic speed for 10-15 minutes, then stir at 360-420rpm for 20-30 minutes, centrifuge and take the precipitate to dry, to obtain a bridging precursor powder;
[0010] Furthermore, the dosage ratio of ultrafine cordierite powder, double-branched coupling matrix, dimethylacetamide and deionized water is 100g:6.5-9g:35-45mL:220-300mL. In the dimethylacetamide aqueous solution environment, the double-branched coupling matrix spontaneously hydrolyzes and couples with the ultrafine cordierite powder, and its double-branched siloxane structure couples the short-range particles to form a small-particle-size loose agglomerated powder.
[0011] Furthermore, the fineness of the ultrafine cordierite powder is 1250-2500 mesh, and the agglomerated loose powder at this particle size is more likely to produce deformation sliding to achieve a toughening effect.
[0012] Step A3: Mix the bridging precursor powder, di-n-butylamine and anhydrous tetrahydrofuran, introduce nitrogen protection, control the temperature of ice water bath to 0-10°C, add sodium hydride intermittently, control the total reaction time to 1.5-2.2h, and after the reaction, reduce the pressure and control the temperature to no more than 50°C to remove tetrahydrofuran by rotary evaporation to obtain a composite toughening agent;
[0013] Furthermore, the amount ratio of the bridging precursor powder, di-n-butylamine, sodium hydride and anhydrous tetrahydrofuran is 100g:12-18mL:0.15-0.21g:180-240mL, and sodium hydride is used as a catalyst to promote the amine ester exchange between di-n-butylamine and the organic matter grafted on the surface of the bridging precursor powder, thereby introducing an amide structure modification containing a branched alkyl group.
[0014] Furthermore, the compatibilizer is PP-g-MAH resin.
[0015] Furthermore, the lubricant is stearic acid.
[0016] A method for preparing a toughened PP plastic barrel comprises the following steps:
[0017] Step S1: mixing the raw materials according to the weight ratio, transferring them into a twin-screw extruder for blending, extrusion and granulation to obtain a composite masterbatch;
[0018] Step S2: Load the composite masterbatch into an injection molding machine, set the mold temperature to 55-70°C, the injection port temperature to 220-230°C, the injection pressure to 4.8-5.2MPa, and the holding pressure to 3.2-3.8MPa, and injection mold the composite masterbatch to obtain a toughened PP plastic barrel.
[0019] Beneficial effects of the present invention:
[0020] The PP plastic barrel disclosed by the present invention is toughened by POE resin and a self-made composite toughening agent. Compared with the existing high-efficiency toughened PP material, the PP plastic barrel has better toughness at room temperature, and gives the plastic barrel product of the storage medium higher stability and safety. The composite toughening agent is made of diethyl diallyl malonate and 3-mercaptopropyltriethoxysilane in an anhydrous environment by click reaction to prepare diethyl malonate with a double-branched siloxane structure, i.e., a double-branched coupling matrix. The hydrolysis coupling effect of the double-branched siloxane structure is utilized to load and capture ultrafine cordierite micropowder particles to form a small-particle-size loose agglomerated powder, i.e., a bridge precursor powder. Finally, di-n-butylamine is subjected to amine ester exchange with organic matter grafted on the surface of the bridge precursor powder under the catalysis of sodium hydride, and an amide structure modification containing a branched alkyl group is introduced to prepare the composite toughening agent. In the process of melt blending, the multi-branched alkyl group introduced on the surface of the composite toughening agent forms an interface modification, so that The composite toughener has good compatibility and dispersibility in the PP substrate; during the cooling process, the amide structure on the surface of the composite toughener strongly promotes the PP substrate to generate high-toughness β-phase crystals, and the β-phase crystals are enriched in the near layer of the composite toughener, which greatly reduces the interface stress between the composite toughener as a hard material and the substrate, weakens the splitting effect of the composite toughener as a defect in the substrate, and is not easy to generate initial microcracks under strong external forces; under the action of external forces, the PP substrate itself first produces plastic deformation, the cordierite in the composite toughener is a hard orthorhombic material, has a suitable mismatch with the PP crystal form, and can form slip toughening during the plastic deformation process. In addition, the cordierite particles in the present invention are a loose agglomerate structure, which strengthens the slip effect and forms secondary toughening. It can be clearly seen in the tensile stress-strain curve that secondary yield occurs at a deformation of about 200%, which greatly increases the toughness of the PP material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0022] Figure 1 This is the tensile stress-strain diagram of the plastic barrel according to the embodiment of the present invention. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1: Preparation of toughened PP plastic barrel, as follows:
[0025] 1) Preparation of composite toughening agent
[0026] Step A1: Diethyl diallylmalonate, dimethylphenylphosphine and anhydrous ethyl acetate were premixed, nitrogen was introduced for protection, and then 3-mercaptopropyltriethoxysilane was added and mixed. The oil bath temperature was controlled at 45°C, and the light intensity applied by UVA lamp was 300W / m 2 The reaction was carried out under ultraviolet irradiation and mechanical stirring at 80 rpm for 3 hours. During the reaction, the dosage ratio of diethyl diallylmalonate, 3-mercaptopropyltriethoxysilane, dimethylphenylphosphine and anhydrous ethyl acetate was 0.1 mol: 0.202 mol: 100 mg: 150 mL. After the reaction, the ethyl acetate was removed by rotary evaporation to obtain a double-branched coupling matrix.
[0027] Step A2: Take a double-branched coupling matrix, dimethylacetamide and deionized water, mix them and stir and hydrolyze them at room temperature for 40 minutes, then add ultrafine cordierite powder. In this embodiment, 1250 mesh ultrafine powder provided by Lingshou County Huiyan Mineral Products Processing Plant is used, ultrasonically dispersed at 28kHz for 15 minutes, and then switched to 420rpm medium speed stirring for 30 minutes, wherein the amount ratio of ultrafine cordierite powder, double-branched coupling matrix, dimethylacetamide and deionized water is 100g:6.5g:35mL:300mL, and then centrifuged to obtain the precipitate and dried to obtain a bridging precursor powder.
[0028] Step A3: Take a mixture of bridging precursor powder, di-n-butylamine and anhydrous tetrahydrofuran, introduce nitrogen protection, control the temperature at 0°C in an ice-water bath, divide the mass of sodium hydride into three portions and add them intermittently for 15 minutes. After complete addition, continue to stir the reaction at a constant temperature, and control the total reaction time of sodium hydride to be 2.2 hours. During the reaction, the amount ratio of bridging precursor powder, di-n-butylamine, sodium hydride and anhydrous tetrahydrofuran is 100g:12mL:0.15g:180mL. After the reaction is completed, reduce the pressure and control the temperature to no more than 50°C to remove tetrahydrofuran by rotary evaporation to obtain a composite toughening agent.
[0029] 2) Injection molding
[0030] Step S1: taking raw materials according to weight percentage, PP resin 73.52wt%, EPF31HR resin provided by North Huajin Chemical Industry Group Co., Ltd. is used in the implementation process of the present invention; POE resin 18wt%, DF840 resin provided by Mitsui Chemicals of Japan is used in the implementation process of the present invention; composite toughening agent 5.5wt%, which is self-made in this embodiment; lubricant 0.28wt%, stearic acid 1898 is used in the implementation process of the present invention; compatibilizer 2.5%, CMG9801 PP-g-MAH resin of Jiayirong Polymer (Shanghai) Co., Ltd. is used in the implementation process of the present invention; antioxidant 0.1wt%, antioxidant 1010 and antioxidant 168 are compounded in a mass ratio of 1:1 in the implementation process of the present invention; light stabilizer 0.1wt%, light stabilizer 662 is used in the implementation process of the present invention;
[0031] The above raw materials were added into a high speed mixer according to the weight ratio and mixed for 15 minutes, and then transferred into a twin-screw extruder for extrusion and granulation to obtain a composite masterbatch.
[0032] Step S2: Load the composite masterbatch into an injection molding machine. The key parameters of injection molding include: mold temperature of 70°C, injection port temperature of 220°C, injection pressure of 4.8MPa, and holding pressure of 3.2MPa. The composite masterbatch is injection molded to obtain a toughened PP plastic barrel.
[0033] Example 2, preparing a toughened PP plastic barrel, specifically as follows:
[0034] 1) Preparation of composite toughening agent
[0035] Step A1: Diethyl diallylmalonate, dimethylphenylphosphine and anhydrous ethyl acetate were premixed, nitrogen was introduced for protection, and then 3-mercaptopropyltriethoxysilane was added and mixed. The oil bath temperature was controlled at 52°C, and the light intensity applied by UVA lamp was 360W / m 2 The reaction was carried out under ultraviolet irradiation and mechanical stirring at 120 rpm for 2.5-3 h. During the reaction, the dosage ratio of diethyl diallylmalonate, 3-mercaptopropyltriethoxysilane, dimethylphenylphosphine and anhydrous ethyl acetate was 0.1 mol: 0.204 mol: 90 mg: 180 mL. After the reaction, the ethyl acetate was removed by rotary evaporation to obtain a double-branched coupling matrix.
[0036] Step A2: Take a double-branched coupling matrix, dimethylacetamide and deionized water, mix them and stir and hydrolyze them at room temperature for 35 minutes, then add ultrafine cordierite powder. In this embodiment, 2000 mesh ultrafine powder provided by Lingshou County Huiyan Mineral Products Processing Plant is used, ultrasonically dispersed at 25kHz for 12 minutes, and then switched to 420rpm medium speed stirring for 25 minutes, wherein the amount ratio of ultrafine cordierite powder, double-branched coupling matrix, dimethylacetamide and deionized water is 100g:8g:40mL:260mL, then centrifuged to take the low precipitate and dry it to obtain a bridging precursor powder.
[0037] Step A3: Take a mixture of bridging precursor powder, di-n-butylamine and anhydrous tetrahydrofuran, introduce nitrogen protection, control the temperature at 5°C in an ice-water bath, divide the mass of sodium hydride into three portions and add them intermittently for 15 minutes. After complete addition, continue to stir the reaction at a constant temperature, and control the total addition reaction time of sodium hydride to be 1.8 hours. During the reaction, the amount ratio of bridging precursor powder, di-n-butylamine, sodium hydride and anhydrous tetrahydrofuran is 100g:15mL:0.18g:220mL. After the reaction is completed, reduce the pressure and control the temperature to no more than 50°C to remove tetrahydrofuran by rotary evaporation to obtain a composite toughening agent.
[0038] 2) Injection molding
[0039] Step S1: taking raw materials according to weight percentage, PP resin 74.38wt%, POE resin 14wt%, composite toughening agent 7.9wt% (self-made in this embodiment), lubricant 0.25wt%, compatibilizer 3.2%, antioxidant 0.15wt% and light stabilizer 0.12wt%;
[0040] The above raw materials were added into a high speed mixer according to the weight ratio and mixed for 15 minutes, and then transferred into a twin-screw extruder for extrusion and granulation to obtain a composite masterbatch.
[0041] Step S2: Load the composite masterbatch into an injection molding machine. The key parameters of injection molding include: mold temperature of 65°C, injection port temperature of 230°C, injection pressure of 5.0 MPa, and holding pressure of 3.5 MPa. The composite masterbatch is injection molded to obtain a toughened PP plastic barrel.
[0042] Example 3, preparing a toughened PP plastic barrel, specifically as follows:
[0043] 1) Preparation of composite toughening agent
[0044] Step A1: Diethyl diallylmalonate, dimethylphenylphosphine and anhydrous ethyl acetate were premixed, nitrogen was introduced for protection, and then 3-mercaptopropyltriethoxysilane was added and mixed. The oil bath temperature was controlled at 55°C, and the light intensity applied by UVA lamp was 400W / m 2The reaction was carried out under ultraviolet irradiation and mechanical stirring at 120 rpm for 2.5 h. During the reaction, the dosage ratio of diethyl diallylmalonate, 3-mercaptopropyltriethoxysilane, dimethylphenylphosphine and anhydrous ethyl acetate was 0.1 mol: 0.206 mol: 80 mg: 200 mL. After the reaction, the ethyl acetate was removed by rotary evaporation to obtain a double-branched coupling matrix.
[0045] Step A2: Take a double-branched coupling matrix, dimethylacetamide and deionized water, mix them and stir and hydrolyze them at room temperature for 30 minutes, then add ultrafine cordierite powder. In this embodiment, 2500 mesh ultrafine powder provided by Lingshou County Huiyan Mineral Products Processing Plant is used, ultrasonically dispersed at 20kHz for 10 minutes, and then switched to 360rpm medium speed stirring for 20 minutes, wherein the amount ratio of ultrafine cordierite powder, double-branched coupling matrix, dimethylacetamide and deionized water is 100g:9g:45mL:220mL, and then centrifuged to obtain the precipitate and dried to obtain a bridging precursor powder.
[0046] Step A3: Take a mixture of bridging precursor powder, di-n-butylamine and anhydrous tetrahydrofuran, introduce nitrogen protection, control the temperature at 10°C in an ice-water bath, divide the mass of sodium hydride into three portions and add them intermittently for 15 minutes. After complete addition, continue to stir the reaction at a constant temperature, and control the total reaction time of sodium hydride to be 1.5 hours. During the reaction, the amount ratio of bridging precursor powder, di-n-butylamine, sodium hydride and anhydrous tetrahydrofuran is 100g:18mL:0.21g:240mL. After the reaction is completed, reduce the pressure and control the temperature to no more than 50°C to remove tetrahydrofuran by rotary evaporation to obtain a composite toughening agent.
[0047] 2) Injection molding
[0048] Step S1: taking raw materials according to weight percentage, PP resin 75.46wt%, POE resin 12wt%, composite toughening agent 8.5wt% (self-made in this embodiment), lubricant 0.3wt%, compatibilizer 3.5%, antioxidant 0.12wt% and light stabilizer 0.12wt%;
[0049] The above raw materials were added into a high speed mixer according to the weight ratio and mixed for 15 minutes, and then transferred into a twin-screw extruder for extrusion and granulation to obtain a composite masterbatch.
[0050] Step S2: Load the composite masterbatch into an injection molding machine. The key parameters of injection molding include: mold temperature of 55°C, injection port temperature of 220°C, injection pressure of 5.2MPa, and holding pressure of 3.8MPa. The composite masterbatch is injection molded to obtain a toughened PP plastic barrel.
[0051] In the comparative example, referring to the disclosed technology, the plastic barrel was prepared by modifying PP with coupled nano-silica and β-nucleating agent, as follows:
[0052] The raw materials are taken according to weight percentage, 69.58wt% of PP resin, 16wt% of POE resin, 7.5wt% of KH570 modified nano-silica (model JL-SiO2-N21, produced by Ningbo Jinlei Nanomaterial Technology Co., Ltd.), 2.2wt% of β-nucleating agent (TMB-5, produced by Shanxi Chemical Research Institute), 0.3wt% of lubricant, 4.2% of compatibilizer, 0.1wt% of antioxidant and 0.12wt% of light stabilizer. The raw materials are from the same batch as those in the embodiment; the specific injection molding process is the same as that in Example 3.
[0053] Samples were taken from the plastic barrels prepared above and tensile tests were performed according to GB / T 1040.2-2006 at a tensile rate of 100 mm / min. Figure 1 , is the tensile stress-strain curve of the samples of Example 1 to Example 3, and the tensile strength and elongation of the samples are measured; the impact test is carried out according to GB / T 1843-2008 standard, the impact energy is 4.4J, the notch depth of the spline is 2mm, and the test temperature is 25°C; the specific test results are shown in Table 1:
[0054] Table 1
[0055] Example 1 Example 2 Example 3 Comparative Example Tensile strength / MPa 27.86 28.08 28.71 28.25 Elongation / % 451.2 443.5 392.6 304.1 <![CDATA[Impact strength / kJ·m -2 > 61.5 63.7 59.6 51.7
[0056] From the test results in Table 1, it can be seen that the PP-based plastic barrel disclosed in the present invention has a tensile strength of 27.86-28.71 MPa, an elongation of 392.6-451.2%, and a room temperature impact strength of 59.6-63.7 kJ / m 2 Compared with the existing high-efficiency composite toughened polypropylene materials, it exhibits better strength and toughness.
[0057] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0058] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A toughened PP plastic barrel, characterized in that: The raw materials include the following by weight percentage: POE resin 12-18wt%, composite toughening agent 5.5-8.5wt%, lubricant 0.25-0.3wt%, compatibilizer 2.5-3.5%, antioxidant 0.1-0.15wt% and light stabilizer 0.1-0.12wt%, and the balance is PP resin; The composite toughening agent is prepared by the following method: Step A1: premix diethyl diallylmalonate, dimethylphenylphosphine and anhydrous ethyl acetate, pass nitrogen gas for protection, then add 3-mercaptopropyltriethoxysilane and mix well, control the oil bath temperature at 45-55°C, apply 300-400W / m 2 UV irradiation, stirring and reacting for 2.5-3h, after the reaction, ethyl acetate was removed by rotary evaporation to obtain a double-branched coupling matrix; Step A2: Mix the bibranched coupling matrix, dimethylacetamide and deionized water and stir and hydrolyze at room temperature for 30-40 minutes, then add ultrafine cordierite powder, disperse at 20-28kHz ultrasonic speed for 10-15 minutes, then stir at 360-420rpm for 20-30 minutes, centrifuge and take the precipitate to dry, to obtain a bridging precursor powder; Step A3: Mix the bridging precursor powder, di-n-butylamine and anhydrous tetrahydrofuran, introduce nitrogen protection, control the temperature at 0-10°C in an ice-water bath, add sodium hydride intermittently to mix, control the total reaction time to 1.5-2.2h, and after the reaction, reduce the pressure and control the temperature to no more than 50°C to remove tetrahydrofuran by rotary evaporation to obtain a composite toughening agent.
2. A toughened PP plastic barrel according to claim 1, characterized in that: The usage ratio of diethyl diallylmalonate, 3-mercaptopropyltriethoxysilane, dimethylphenylphosphine and anhydrous ethyl acetate is 0.1 mol: 0.202-0.206 mol: 80-100 mg: 150-200 mL.
3. A toughened PP plastic barrel according to claim 2, characterized in that: The dosage ratio of the ultrafine cordierite powder, the double-branched coupling matrix, dimethylacetamide and deionized water is 100g: 6.5-9g: 35-45mL: 220-300mL.
4. A toughened PP plastic barrel according to claim 3, characterized in that: The fineness of ultrafine cordierite powder is 1250-2500 mesh.
5. A toughened PP plastic barrel according to claim 4, characterized in that: The dosage ratio of the bridging precursor powder, di-n-butylamine, sodium hydride and anhydrous tetrahydrofuran is 100 g: 12-18 mL: 0.15-0.21 g: 180-240 mL.
6. The toughened PP plastic barrel according to claim 1, characterized in that: The compatibilizer is PP-g-MAH resin.
7. The toughened PP plastic barrel according to claim 1, characterized in that: The lubricant is stearic acid.
8. The method for preparing a toughened PP plastic barrel according to claim 1, characterized in that: The steps include: Step S1: mixing the raw materials according to the weight ratio, transferring them into a twin-screw extruder for blending, extrusion and granulation to obtain a composite masterbatch; Step S2: Load the composite masterbatch into an injection molding machine, set the mold temperature to 55-70°C, the injection port temperature to 220-230°C, the injection pressure to 4.8-5.2MPa, and the holding pressure to 3.2-3.8MPa, and injection mold the composite masterbatch to obtain a toughened PP plastic barrel.