A kind of high heat resistance, high plasticity and corrosion resistance aluminum alloy material and preparation method thereof

By adding Y element and Si to the Al-Sc-Zr alloy, a multi-layer core-shell structure Al3 (Sc, Zr, Y) phase is formed, and the process is optimized to solve the problem of strength and plasticity of existing heat-resistant aluminum alloy materials at high temperatures. The problem of insufficient performance matching is achieved by achieving high strength, good plasticity and corrosion resistance of materials at high temperatures to meet high-end manufacturing needs.

CN118422015BActive Publication Date: 2024-10-18GRIMAT ENG INST CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410896187.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-18
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Existing heat-resistant aluminum alloy materials have insufficient strength and plasticity performance at high temperatures and poor corrosion resistance, making it difficult to meet the needs of high-end manufacturing in aerospace, transportation, electronics and electricity.

Method used

By adding a trace amount of Y element to the Al-Sc-Zr alloy, adjusting the proportions of Sc, Zr, and Y, a dispersed multi-layered core-shell structure of Al3 (Sc, Zr, Y) phase is formed, which is significantly promoted by the participation of Si. Precipitate, control the Mg element content to ensure the role of Si, optimize the composition and heat treatment process, and prepare a high-density nanoscale (Al, Si) 3 (Sc, Zr, Y) phase to improve the heat resistance, plasticity and corrosion resistance of the material. .

Benefits of technology

It realizes that aluminum alloy materials can maintain high strength and good plasticity at high temperatures, and at the same time have excellent corrosion resistance, meet the stringent requirements of high-end manufacturing for heat-resistant aluminum alloys, and provide an ideal material selection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422015B_ABST
    Figure CN118422015B_ABST
Patent Text Reader

Abstract

The present invention discloses a high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material and a preparation method thereof, and belongs to the field of aluminum alloy and preparation and processing. The aluminum alloy contains: Si 0.01-0.35wt%, Sc 0.01-2.2wt%, Zr 0.01-2.3wt%, Y 0.01-2.1wt%, Mg<0.01wt%, the total content of Ti, V, Cr, Mn, Ni, and Ca elements is ≤0.03wt%, and the rest is Al. The preparation method of the alloy deformation processed material comprises the following steps: (1) manufacturing an aluminum alloy ingot; (2) performing homogenization heat treatment on the ingot; (3) rapidly cooling the ingot subjected to homogenization heat treatment to room temperature; (4) performing artificial aging heat treatment on the ingot; (5) hot processing the ingot into a desired processed material form, or hot deforming the ingot into a pre-processed material; (6) optionally reheating the pre-processed material and processing it into a processed material through cold deformation; (7) optionally performing stress relief annealing on the processed material. The aluminum alloy contains a high-density precipitated (Al, Si) 3 (Sc, Zr, Y) phase, and the material exhibits excellent plasticity, heat resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an aluminum alloy material and a preparation method thereof, in particular to a high heat-resistant, high-plasticity, and corrosion-resistant Al-Sc-Zr-Y-Si series aluminum alloy material and a preparation method thereof, belonging to the technical field of aluminum alloys and their preparation and processing. Background Art

[0002] Aluminum alloys have the characteristics of light weight, high specific strength, controllable cost, and easy processing. They are widely used in aerospace, transportation, electronic power and other fields. Heat-resistant aluminum alloys generally refer to a type of aluminum alloy material that can still maintain its strength level and comprehensive performance at temperatures above 150°C. They can partially replace steel and titanium alloys to achieve significant low cost and weight reduction effects. With the development of various industries, the structural design of new equipment, more stringent service environment, and cost control of industrial applications have put forward higher requirements for heat-resistant aluminum alloys. There is an urgent need to develop new aluminum alloy materials with high heat resistance, high plasticity, and corrosion resistance.

[0003] In the field of aerospace, commonly used heat-resistant aluminum alloys mainly include Al-Cu-Mg-Fe-Si, Al-Cu-Mn, Al-Cu-Mg-Ag series deformed aluminum alloys and Al-Fe-(V-Si) series aluminum alloys prepared by rapid solidification. Al-Cu-Mg-Fe-Si and Al-Cu-Mn series alloys can be used at 150~200℃, and have been industrialized in China. At present, they have relatively mature preparation and processing systems and some product specifications, but there are problems such as poor product performance stability and high production and preparation costs. Al-Cu-Mg-Ag series alloys can be used at 200~250℃. The addition of precious metal Ag leads to high alloy costs, and they are only used in a small range at home and abroad. Al-Fe-(V-Si) series aluminum alloys prepared by rapid solidification can be used at 300~350℃, but their preparation method leads to the alloys having disadvantages such as poor fatigue fracture performance, small size specifications, and high cost. In the field of transportation, it mainly includes Al-Si-Cu, Al-Si-Mg, and Al-Cu-Mn series cast aluminum alloys. Among them, Al-Si-Cu and Al-Si-Mg series alloys are used at 150~300℃, but the strength level of the alloys in different temperature ranges is low, and the effect of adding rare earth elements on improving the strength of the alloys is not ideal; Al-Cu-Mn series alloys can be used at 300℃, but the corrosion resistance of the alloys is poor, and the size and shape of the products are limited. In the field of electricity, Al-Zr series alloys are commonly used, which can be used at 150~200℃ and have been widely used in China. However, there are currently no alloys and products that meet the needs of heat-resistant aluminum alloys for conductors with higher strength levels and long-term use temperatures above 200℃ in China.

[0004] Adding trace rare earth / transition elements to aluminum alloy for microalloying, a new type of L12 structure Al3X (X=rare earth / transition element) precipitation phase particles are precipitated in the α-Al matrix through the classic solid solution-aging method to strengthen the alloy. Since rare earth / transition elements have extremely slow diffusion rate and small solid solubility in the α-Al matrix, the corresponding Al3X phase still has excellent coarsening resistance and very small dissolution tendency at high temperatures up to 300°C. At the beginning of this century, a series of Al-Sc-based heat-resistant aluminum alloy materials have been proposed abroad. The Al3Sc precipitation phase in the Al-Sc alloy can usually maintain good stability at 300°C, but it coarsens severely at 400°C. By wrapping the Al3Sc precipitation phase with an Al3Zr layer to form the so-called "core-shell" structure, the service temperature of the Al3 (Sc, Zr) precipitation phase can be greatly increased, and the corresponding improved Al-Sc-Zr alloy has reached the 400°C mark. However, due to the small number of precipitation phases in the alloy at this time, the alloy strength is insufficient. Then, new microalloying elements are added to promote the precipitation of Al3X phase. The construction of this type of phase can increase the volume fraction of the precipitated phase, thereby improving the precipitation strengthening effect. In addition, a series of Si microalloying studies in recent years have found that the precipitation of Al3X phase can be greatly accelerated by trace amounts of Si, thereby further improving the alloy hardening effect. The multi-component composite microalloyed Al-Sc-X based alloy developed based on the above characteristics is currently the most classic and effective means to achieve the service of aluminum alloy materials at temperatures of 300~400℃ and above. For example: Patent document CN102965550A discloses a high-strength, high-conductivity, heat-resistant aluminum alloy, whose basic composition range is: Zr 0.15~0.40wt.%, Tm 0.50~0.80wt.%, Fe 0.50~0.95wt.%, Si<0.05wt.%, the sum of impurity elements Ti, V, Cr, and Mn is less than 0.01wt.%, the second phase of the alloy is a fine granular Al(Tm,Fe) phase and a dispersed core-shell structured Al3(Tm,Zr) phase, the tensile strength is above 185MPa, and the long-term heat resistance temperature reaches 210°C. Patent document CN105734353A discloses a lightweight, high-conductivity, heat-resistant aluminum alloy, whose basic composition range is: B 0.035~0.06wt.%, Zr 0.1~0.2wt.%, Er0.2~0.4wt.%, but not including 0.2wt.%, Ti, V, Cr, Mn impurity elements total content ≤0.01wt.%, the second phase of the alloy is Al3(Zr, Er) ternary composite phase with a core-shell structure, the tensile strength is greater than or equal to 165MPa, and the long-term operating temperature can be as high as 210°C.Patent document CN102021444A discloses a highly conductive and heat-resistant aluminum alloy, whose basic composition range is: Zr 0.1~0.3wt.%, Y 0.02~0.2wt.%, Sc 0.01~0.15wt.%, and the total amount of other inevitable impurity elements does not exceed 0.15wt.%. The tensile strength of the alloy is not less than 160MPa, the elongation is not less than 1.8%, and the heat resistance performance reaches above 150°C for long-term operation. Patent document CN115595474A discloses a super heat-resistant aluminum alloy, whose basic composition range is: Zr 0.55~1.00wt.%, Si 0.18~0.25wt.%, Sc0.07~0.12wt.%, Yb 0.03~0.06wt.%, Fe≤0.15wt.%, and the sum of other inevitable trace impurity elements ≤0.05wt.%. The alloy has a tensile strength of ≥180MPa and an elongation at break of ≥5%. When maintained at a high temperature of 310°C for 400 hours, its tensile strength retention rate is not less than 95% of the initial measured value at room temperature. Patent document CN106834814A discloses a high-conductivity, heat-resistant and corrosion-resistant alloy, whose basic composition range is: Er 0.05~0.30wt.%, Sc 0.10~0.20wt.%, Zr 0.05~0.15wt.%, Si0.05~0.10wt.%, the inevitable impurity Fe content is less than 0.03wt.%, and the total content of impurities Ti, V, Cr, and Mn is less than 0.01wt.%. The second phase of the alloy is a nano-precipitated phase Al3 (Sc, Zr, Er) with a core-double shell structure, with a tensile strength greater than or equal to 190MPa, a long-term operating temperature of up to 210°C, a strength residual rate of 230°C / 1h greater than 90%, and excellent corrosion resistance.

[0005] Although the research and development of heat-resistant alloys based on Al3X phase has achieved certain results in recent years, there is still a lot of room for improvement in the excellent matching of key properties such as heat resistance, strength, plasticity and corrosion resistance of the alloy. For example, in most research works, the amount of Al3X phase precipitation is not enough, resulting in a low strength level of the alloy; some work focuses on adding new alloying elements to improve the strength of the alloy, but due to the formation of multiple or a large number of incoherent brittle phases, although the strength of the alloy is improved, the plasticity is significantly deteriorated; in some research works, the types and amounts of alloying elements added are unreasonable, resulting in obvious consumption of rare earth / transition elements in the alloy and the formation of coarse second phases, which significantly reduces the plasticity of the alloy. In addition, the harsh service environment with both medium corrosion and high temperature puts forward requirements for the corrosion resistance of heat-resistant alloys, but few studies have focused on this aspect in the early stage.

[0006] Therefore, it is necessary to further research and develop new Al-Sc aluminum alloy materials with excellent matching of key properties such as high heat resistance, high plasticity and corrosion resistance. Summary of the invention

[0007] The present invention has found through a large number of studies that by adding a trace amount of Y element to the Al-Sc-Zr alloy and adjusting the ratio of Sc, Zr and Y elements to be within a suitable range, a dispersed Al3(Sc, Zr, Y) phase with a multi-layer core-shell structure can be formed in the alloy, and its size is significantly smaller than the Al3(Sc, Zr) phase in the Al-Sc-Zr alloy, and the number density of the precipitated phase is significantly greater than the latter. Si can participate in the formation of the dispersed phase and significantly promote its precipitation, and at the same time cause the dispersed phase to grow and coarsen. On this basis, by adding an appropriate amount of Si element and controlling the upper limit of the addition amount of Si element, a large amount of (Al, Si)3(Sc, Zr, Y) phase can be formed in the alloy and the dispersed phase does not grow and coarsen significantly. In addition, the content of elements such as Mg is strictly controlled to ensure that it will not "consume" the Si element, resulting in the inability to exert the effect of Si promoting precipitation. Compared with the Al-Sc-Zr-Y alloy, the size of the precipitated phase of the Al-Sc-Zr-Y-Si alloy is further reduced and the precipitation density is significantly increased. Fine optimization of the composition range and ratio of each element of the alloy is an important guarantee for achieving excellent performance matching. Through reasonable composition and heat treatment process design, the alloy can obtain a nano-scale (Al, Si) 3 (Sc, Zr, Y) phase with high-density precipitation, small size, and coherent with the matrix during the aging process, so that the Al-Sc-Zr-Y-Si alloy of the present invention can maintain a high strength level while achieving good heat resistance, plasticity and corrosion resistance.

[0008] The purpose of the present invention is to overcome the shortcomings of the comprehensive performance matching of the existing Al-Sc series aluminum alloy materials, and to provide an ideal material for the high-end manufacturing industry of an Al-Sc-Zr-Y-Si series aluminum alloy that takes into account strength, plasticity, heat resistance and corrosion resistance through the optimization design of the composition and the preparation and processing technology.

[0009] The primary technical problem to be solved by the present invention is to propose a high-strength, high-heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material; the second technical problem to be solved by the present invention is to propose a method for preparing the aluminum alloy material; the third technical problem to be solved by the present invention is to propose that the aluminum alloy material is welded with itself or other alloys to form a new product; the fourth technical problem to be solved by the present invention is to propose that the aluminum alloy material is processed into a final component through various surface treatments, stamping and machining methods; the fifth technical problem to be solved by the present invention is to propose the application of the final component.

[0010] The invention relates to a high-heat-resistant, high-plasticity and corrosion-resistant aluminum alloy material. The aluminum alloy contains: Si 0.01-0.35wt%, Sc 0.01-2.2wt%, Zr 0.01-2.3wt%, Y 0.01-2.1wt%, Mg<0.01wt%, the total content of Ti, V, Cr, Mn, Ni and Ca impurity elements is ≤0.03wt%, and the rest is Al and unavoidable impurities.

[0011] A first preferred embodiment of the present invention is that the aluminum alloy contains: Si 0.01-0.30wt%, Sc 0.01-2.0wt%, Zr 0.01-2.0wt%, Y 0.01-2.0wt%, Mg<0.01wt%, the total content of impurity elements Ti, V, Cr, Mn, Ni, and Ca is ≤0.03wt%, and the rest are Al and unavoidable impurities.

[0012] As a second preferred embodiment of the present invention, the aluminum alloy contains: Si 0.01-0.28wt%, Sc 0.03-1.7wt%, Zr 0.03-1.8wt%, and Y 0.02-1.8wt%.

[0013] As a third preferred embodiment of the present invention, the aluminum alloy contains: Si 0.02-0.26wt%, Sc 0.05-1.4wt%, Zr 0.07-1.5wt%, and Y 0.03-1.3wt%.

[0014] As a fourth preferred embodiment of the present invention, the aluminum alloy contains: Si 0.03-0.24wt%, Sc 0.06-1.0wt%, Zr 0.10-1.2wt%, and Y 0.04-0.9wt%.

[0015] As a fifth preferred embodiment of the present invention, the aluminum alloy contains: Si 0.04-0.22wt%, Sc 0.07-0.6wt%, Zr 0.12-0.9wt%, and Y 0.05-0.5wt%.

[0016] As a sixth preferred embodiment of the present invention, the aluminum alloy contains: Si 0.05-0.20wt%, Sc 0.08-0.3wt%, Zr 0.15-0.5wt%, and Y 0.05-0.3wt%.

[0017] As a seventh preferred embodiment of the present invention, in the aluminum alloy, the contents of Sc, Zr and Y satisfy the relationship: 1.5≤[(3×Sc)+(2×Zr)] / (3×Y)≤4.5.

[0018] As an eighth preferred embodiment of the present invention, in the aluminum alloy, the Mg element needs to satisfy: Mg≤0.008wt%; preferably satisfies: Mg≤0.005wt%; and further preferably satisfies: Mg≤0.003wt%.

[0019] As a ninth preferred embodiment of the present invention, the aluminum alloy contains: Ti 0.001-0.01wt%.

[0020] As a tenth preferred embodiment of the present invention, the aluminum alloy contains: V 0.001-0.01wt%.

[0021] As an eleventh preferred embodiment of the present invention, the aluminum alloy contains: 0.005-0.02wt% Cr.

[0022] As a twelfth preferred embodiment of the present invention, the aluminum alloy contains: Mn 0.001-0.02wt%.

[0023] As a thirteenth preferred embodiment of the present invention, the aluminum alloy contains: Ni 0.005-0.02wt%.

[0024] As a fourteenth preferred embodiment of the present invention, the aluminum alloy contains: Ca 0.001-0.01wt%.

[0025] As the fifteenth preferred embodiment of the present invention, the unavoidable impurities contained in the aluminum alloy include elements unintentionally introduced as impurities during the manufacturing process of the alloy ingot, which must satisfy Fe≤0.20wt%, other impurity elements each ≤0.10wt%, and the total ≤0.30wt%. Preferably, Fe≤0.15wt%, other impurity elements each ≤0.05wt%, and the total ≤0.20wt%. It is further preferred that Fe≤0.10wt%.

[0026] The present invention also relates to a preparation method for producing the above-mentioned aluminum alloy material. The basic preparation process of the aluminum alloy deformation material can be described as "alloy preparation and smelting - semi-continuous casting to prepare ingots - homogenization heat treatment of ingots - ingot quenching - ingot aging treatment - hot deformation processing - (intermediate annealing) - (cold deformation processing) - (annealing treatment) - supply of products"; the basic preparation process of the aluminum alloy casting can be described as "alloy preparation and smelting - casting molding of castings - homogenization heat treatment of castings - casting quenching - casting aging treatment - supply of products".

[0027] The method for producing the aluminum alloy deformed material comprises the following steps:

[0028] (1) Producing a semi-continuously cast ingot as described in the present invention;

[0029] (2) performing homogenization heat treatment on the obtained ingot;

[0030] (3) Rapidly cooling the ingot after homogenization heat treatment to room temperature;

[0031] (4) performing artificial aging heat treatment on the cooled ingot;

[0032] (5) hot deforming the ingot into a desired processed material form, or hot deforming the ingot into a pre-processed material, by one or more hot deformation processing methods selected from extrusion, rolling and forging;

[0033] (6) optionally reheating the pre-processed material and cold-forming it into the desired processed material form;

[0034] (7) Optionally, the processed material may be subjected to stress relief annealing.

[0035] In step (1), the ingot is manufactured by smelting, degassing, removing inclusions and semi-continuous casting. During the smelting process, the content and proportion of alloy elements are quickly adjusted through online composition detection and analysis, and the entire ingot manufacturing process is completed.

[0036] In step (2), the homogenization heat treatment is a single-stage homogenization heat treatment performed at a temperature in the range of 600-640° C. for a total time of 16-72 hours.

[0037] In step (3), the ingot is rapidly cooled to room temperature by using a self-selected cooling medium such as spray quenching, immersion quenching, strong wind cooling, or a combination thereof, with a cooling rate of ≥50°C / s.

[0038] In step (4), the temperature of the artificial aging heat treatment is 370-430°C and the time is 16-48 hours.

[0039] In steps (4) and (5), the preheating temperature before each thermal deformation process is 350-400°C, and the processing time is 1-6 hours.

[0040] In step (6), the cold deformation process also includes an intermediate annealing treatment of 330-370°C / 0.5-6h.

[0041] In step (7), the stress relief annealing treatment is performed at a temperature of 300-400°C and for a time of 3-6 hours.

[0042] After step (7), the method further includes the following steps: straightening the processed material after stress relief annealing treatment, using roller straightening, stretch straightening, stretch bending straightening and a combination thereof to improve the straightness of the processed material for subsequent processing and application.

[0043] Through the preparation method of the present invention, the processed material is a rod, a tube, a wire / line material, a plate or a forging product.

[0044] The density of the high heat-resistant, high plasticity and corrosion-resistant aluminum alloy material of the present invention is ≤2.73 g / cm 3 , room temperature tensile strength ≥180MPa, elongation ≥18%; after being kept at 400℃ for 100h, the room temperature tensile strength ≥170MPa, the elongation ≥17%, and the exfoliation corrosion resistance grade is not lower than PB grade. Preferably, the room temperature tensile strength of the aluminum alloy material is ≥190MPa, and the elongation ≥19%; after being kept at 400℃ for 100h, the room temperature tensile strength is ≥175MPa, the elongation ≥18%, and the exfoliation corrosion resistance grade is not lower than PA grade. Further preferably, the room temperature tensile strength of the aluminum alloy material is ≥200MPa, and the elongation ≥20%; after being kept at 400℃ for 100h, the room temperature tensile strength is ≥180MPa, the elongation ≥19%, and the exfoliation corrosion resistance grade is not lower than N grade.

[0045] The present invention also relates to a preparation method for producing the aluminum alloy casting, comprising the following steps:

[0046] (1) Aluminum alloy castings are prepared by smelting, degassing, removing inclusions, sand mold, metal mold casting, or die casting. During the smelting process, the content and ratio of alloy elements are quickly adjusted through online component detection and analysis, and the entire casting manufacturing process is completed;

[0047] (2) subjecting the obtained aluminum alloy casting to a homogenization heat treatment at a temperature in the range of 600 to 640° C. for a total time of 16 to 72 hours;

[0048] (3) After homogenization, the aluminum alloy castings are rapidly cooled to room temperature by spray quenching, immersion quenching, strong wind cooling or a combination thereof using a self-selected cooling medium, with a cooling rate of ≥40°C / s;

[0049] (4) Perform artificial aging heat treatment on the aluminum alloy castings, the artificial aging temperature is 370~430℃, and the time is 16~48h.

[0050] The aluminum alloy material of the present invention can be welded with itself or other alloys to form a new product; the welding methods include stir friction welding, fusion welding, brazing, electron beam welding, and laser welding. It can also be processed into a final component through various surface treatments, stamping, and machining; the final component is a heat-resistant structural part.

[0051] The beneficial effects of the present invention are:

[0052] (1) By optimizing the composition of Al-Sc-Zr-Y-Si aluminum alloy and using a matching preparation method, nanoscale (Al,Si)3(Sc,Zr,Y) phases are precipitated in the alloy. These phases are coherent with the matrix, have small size, and high volume fraction. This allows the material to have high strength and good corrosion resistance while ensuring good heat resistance and high plasticity. The material exhibits excellent comprehensive properties and is an ideal material for various heat-resistant structural parts. It can meet the stringent requirements of various high-end manufacturing for high heat-resistant aluminum alloy materials.

[0053] (2) The present invention realizes high-density precipitation of heat-resistant phases through multi-component composite microalloying of Zr, Y and Si in Al-Sc alloys, and has a good strengthening effect. It provides a new idea for the development of heat-resistant aluminum alloys, helps promote the development of aerospace, transportation, electronic power and other fields, and has important social and economic benefits.

[0054] (3) The material of the present invention has excellent performance, the preparation method is simple and practical, the operability is strong, it is easy to industrialize and promote, and the market prospect is promising. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 This is a TEM photograph of the intragranular precipitation phase of the 48# alloy in the aged state in Example 5 of the present invention.

[0056] Figure 2 This is a 3DAP photograph of the precipitated phase composition of the 48# alloy in Example 5 of the present invention.

[0057] Figure 3 The figure is a comparison of the room temperature strength and elongation of the alloy of the present invention and the typical alloy of the existing patent.

[0058] Figure 4 The room temperature strength and corrosion resistance of the alloy of the present invention are compared with those of the typical alloy of the existing patent.

[0059] Figure 5 The figure is a comparison of the room temperature strength and the strength after heat exposure of the alloy of the present invention and the typical alloy of the prior patent. DETAILED DESCRIPTION

[0060] The technical solution of the present invention is further described in detail below in conjunction with embodiments.

[0061] Example 1

[0062] Alloy extruded rods were prepared on a laboratory scale to demonstrate the principle of the present invention. The composition of the experimental alloys is shown in Table 1.

[0063] Through the well-known alloy smelting, degassing, inclusion removal, and simulated semi-continuous casting conditions, the φ210mm round ingot is prepared. The homogenization heat treatment system of the ingot is selected as 630±5℃ / 36h, the average quenching cooling rate is 60℃ / s, and the aging treatment is immediately carried out at 400±5℃ / 24~30h after water quenching. After the aging treatment, the ingot is peeled, milled, and sawed to obtain the φ180mm extrusion billet. The billet is preheated at 400±10℃ for 1h, and the φ30mm extruded rod is obtained by extrusion deformation. The extrusion temperature is controlled at about 400℃. The extruded rod is annealed at 350±10℃ / 4h.

[0064] The annealed extruded bars were subjected to a heat exposure treatment at 400°C / 100h.

[0065] Samples were cut according to relevant methods, and the alloys were tested for tensile properties (GB / T16865) and exfoliation corrosion (GB / T 22639) according to relevant test standards, which were used as common performance indicators of the alloys for evaluation. The results are shown in Table 2.

[0066] surface Test alloy composition

[0067]

[0068] Table 2 Performance test results of experimental alloys

[0069]

[0070] As can be seen from Table 2, 1#, 2#, 3#, 4#, 5#, 6#, 7#, 8#, 9#, 10#, 11#, 12#, 13#, 14#, 15#, 16#, 17#, 18#, 19#, 20#, 21, 22#, 23#, 24#, 25#, 26#, 27#, 28# alloys all have a good match of strength-plasticity-heat resistance-corrosion resistance: the room temperature tensile strength is higher than 180MPa, the elongation is higher than 18%, and the alloy exfoliation corrosion grade is not lower than PB grade; the room temperature tensile strength after heat exposure is higher than 180MPa, and the elongation is higher than 17%. However, the performance of 29#, 30#, 31#, 32#, 33#, 34#, 35#, 36#, 37#, 38# alloys does not meet the good match of strength-plasticity-heat resistance-corrosion resistance.

[0071] Alloy 29 has a high Si content, and its tensile strength and plasticity deteriorate significantly after thermal exposure, and its exfoliation corrosion resistance is poor. Alloy 30 has more Ca elements, and its room temperature strength is significantly lower, and its exfoliation corrosion resistance is poor. Alloys 31, 32, and 33 have different contents of Mg elements, and their exfoliation corrosion resistance is poor. Among them, alloy 31 has high Sc, Zr, Y, and Si contents, and good room temperature tensile properties, but its strength deteriorates significantly after thermal exposure; alloy 32 has the highest Mg content, and its room temperature tensile strength and elongation, as well as its performance after thermal exposure are significantly lower than those of alloy 31; alloy 33 has the lowest room temperature performance and performance after thermal exposure. Alloy 34 has only Sc and Zr, and its strength at room temperature and thermal exposure is significantly lower, and its elongation is higher; accordingly, alloy 35 has significantly improved strength properties at room temperature and after thermal exposure after adding Si elements, and its elongation deteriorates. Alloy 36 only has Sc and Y, and its room temperature strength and elongation are low, and its performance deteriorates after heat exposure; accordingly, the performance of alloy 37 further deteriorates after adding Si element at room temperature and after heat exposure. Alloy 38 adds Sc, Zr, and Y at the same time, and its overall performance level at room temperature and after heat exposure is higher than that of alloys 34 and 36.

[0072] Example 2

[0073] Aluminum alloy rolled plates were prepared in the laboratory, and the composition of the experimental alloy is shown in Table 3.

[0074] The 100mm thick ingot is prepared by alloy smelting, degassing, inclusion removal, and simulating semi-continuous casting conditions as known in the industry. The ingot is homogenized at 630±5℃ / 24h, with an average quenching cooling rate of 70℃ / s. After water quenching, it is immediately aging treated at 400±5℃ / 20~26h. The ingot after aging treatment is peeled, milled, and sawed to obtain a rolled billet with a thickness of 80mm. The billet is preheated at 400±10℃ for 1.5h, and rolled to a thickness of about 10mm along the length of the ingot. The rolling temperature is controlled at about 400℃. The rolled plate is annealed at 350±10℃ / 2h.

[0075] The annealed rolled plate was subjected to a heat exposure treatment at 400°C / 100h.

[0076] Samples were cut according to relevant methods, and the alloys were tested for tensile properties (GB / T16865) and exfoliation corrosion (GB / T 22639) according to relevant test standards, which were used as common performance indicators of the alloys for evaluation. The results are shown in Table 4.

[0077] Table 3 Test alloy composition

[0078]

[0079] Table 4 Performance test results of experimental alloys

[0080]

[0081] It can be seen from Table 4 that the 39#, 40# and 41# alloys of the present invention all exhibit a good match of strength-plasticity-heat resistance-corrosion resistance, and are significantly better than the 42# alloy with Mg added.

[0082] Example 3

[0083] Small-sized aluminum alloy forgings were prepared on the pilot platform, and the alloy composition is shown in Table 5.

[0084] The φ470mm round ingot is prepared by the well-known alloy smelting, degassing, inclusion removal and semi-continuous casting conditions in the industry. The homogenization heat treatment system of the ingot is selected as 630±5℃ / 60h, the average quenching cooling rate is 45℃ / s, and the aging treatment is immediately carried out at 400±5℃ / 42~48h after water quenching. The ingot after aging treatment is peeled, milled and sawed to obtain a rolled billet with a thickness of φ430mm. The billet is preheated at 400±10℃ for 3h, extruded to obtain a φ200mm extruded bar billet, and then multi-sided forging to obtain a small-sized forging of 50×300×600mm. The extrusion and forging deformation temperature is controlled at 390~410℃. The forging is annealed at 350±10℃ / 4h.

[0085] The annealed forgings were subjected to a heat exposure treatment at 400°C for 100 h.

[0086] Samples were cut according to relevant methods, and the alloy was tested for tensile properties (GB / T16865) and exfoliation corrosion (GB / T 22639) according to relevant test standards, which were used as common performance indicators of the alloy for evaluation. The results are shown in Table 6.

[0087] Table 5 Test alloy composition

[0088]

[0089] Table 6 Performance test results of experimental alloys

[0090]

[0091] It can be seen from Table 6 that the 43# alloy of the present invention exhibits a good match of strength-plasticity-heat resistance-corrosion resistance.

[0092] Example 4

[0093] Aluminum alloy castings were prepared in the laboratory, and the alloy composition is shown in Table 7.

[0094] Through raw material preparation (high purity aluminum, Al-Sc master alloy, Al-Zr master alloy, Al-Y master alloy, Al-Si master alloy), tool and mold baking, high purity aluminum is melted at 750℃, Al-Sc master alloy is added first, stirred to make it completely melted; Al-Y master alloy and Al-Si master alloy are added, stirred to make it fully melted; Al-Zr master alloy is added, stirred to make it fully melted after standing for 4~6min, and then degassing and deslagging refining are carried out. After completion, the aluminum alloy melt is poured into the baked metal mold, and the mold temperature is about 180~200℃; the prepared aluminum alloy casting is loaded into a muffle furnace at 630℃, homogenized at 630±5℃ / 24h, water-cooled at a cooling rate of 60℃ / s, and then aging treated at 400±5℃ / 18~24h. The casting is annealed at 350±10℃ / 4h.

[0095] The annealed castings were subjected to a heat exposure treatment at 400°C for 100 h.

[0096] Samples were cut according to relevant methods, and the alloys were subjected to tensile properties (GB / T16865), exfoliation corrosion (GB / T 22639) and intergranular corrosion tests according to relevant test standards, which were used as common performance indicators of the alloys for evaluation. The results are shown in Table 8.

[0097] Table 7 Test alloy composition

[0098]

[0099] Table 8 Performance test results of experimental alloys

[0100]

[0101] It can be seen from Table 8 that, compared with 46# and 47# alloy castings, 44# and 45# alloys of the present invention show a good match of strength-plasticity-heat resistance-corrosion resistance.

[0102] Example 5

[0103] The alloy was prepared on an industrial scale, and the composition of the alloy is shown in Table 9.

[0104] Through the well-known alloy smelting, degassing, inclusion removal, and semi-continuous casting, φ480mm round ingots are prepared. The homogenization heat treatment system of 48#, 49# and 50# alloy ingots is selected as 630±5℃ / 60h, the average quenching cooling rate is 45℃ / s, and the aging treatment of 400±5℃ / 42~48h is immediately carried out after water quenching. After aging treatment, the ingot is peeled, milled and sawed to obtain φ460mm extruded billet. The billet is preheated at 400±10℃ for 4h, and the φ80mm extruded bar is obtained by extrusion deformation. The extrusion temperature is controlled at about 400℃. The extruded bar is annealed at 350±10℃ / 4h.

[0105] The 51# alloy ingot is directly subjected to aging treatment at 300℃ / 36h+400℃ / 48h. After aging treatment, the ingot is peeled, milled and sawed to obtain φ460mm extrusion billet. The billet is directly extruded into φ80mm extrusion bar after residual heat at 440℃ for 1h. The extrusion bar is annealed at 350±10℃ / 4h.

[0106] The alloy ingots of 52#, 53#, 54# and 55# are directly annealed at 320~480℃ / 4~36h. After annealing, the ingots are peeled, milled and sawed to obtain φ460mm extrusion billets. The billets are extruded into φ80mm extrusion bars at 400~440℃, and the extrusion bars can be annealed at 150~350℃ / 5~15h.

[0107] The annealed extruded bars were subjected to a heat exposure treatment at 400°C / 100h.

[0108] Samples were cut according to relevant methods, and the alloys were subjected to tensile properties (GB / T16865), exfoliation corrosion (GB / T 22639) and intergranular corrosion tests according to relevant test standards, which were used as common performance indicators of the alloys for evaluation. The results are shown in Table 10.

[0109] Table 9 Test alloy composition

[0110]

[0111] Note: The composition of 51# alloy adopts the alloy composition in patent document CN106834814A, the composition of 52# alloy adopts the alloy composition in patent document CN102965550A, the composition of 53# alloy adopts the alloy composition in patent document CN105734353A, the composition of 54# alloy adopts the alloy composition in patent document CN102021444A, and the composition of 55# alloy adopts the alloy composition in patent document CN115595474A.

[0112] Table 10 Performance test results of experimental alloys

[0113]

[0114] It can be seen from Table 10 that the 48#, 49# and 50# alloys of the present invention all have a good match of strength-plasticity-heat resistance-corrosion resistance. Compared with the 51# alloy (Al-Sc-Zr-Er-Si alloy), 52# alloy (Al-Zr-Tm-Fe-Si), 53# alloy (Al-Zr-Er-B), 54# alloy (Al-Sc-Zr-Y) and 55# (Al-Sc-Zr-Yb-Si) prepared under the same conditions, they have obvious comprehensive performance advantages, higher room temperature tensile strength and elongation, equivalent or better exfoliation corrosion resistance, and a high level of heat resistance.

[0115] Figure 1 This is a TEM photo of the intracrystalline precipitation phase morphology of the 48# alloy of the present invention. It can be found that there are a large number of densely distributed nanoscale precipitation phases in the alloy, which are small in size and high in volume fraction, ensuring that the alloy has good heat resistance, high plasticity, corrosion resistance and high strength. Figure 2 The 3DAP photo of the precipitated phase composition of the 48# alloy of the present invention, the leftmost picture is the phase of the screened analysis component, and the others are the distribution characteristics of different components. It can be found that the precipitated phase has a typical core-shell structure, in which Sc, Y, and Si are mainly distributed inside the precipitated phase, and Zr is mainly distributed on the surface of the precipitated phase. Figure 3 , Figure 4 and Figure 5 The room temperature strength and elongation, room temperature strength and exfoliation corrosion grade, room temperature strength and strength after heat exposure of the alloys 48#, 49#, 50# of the present invention and the typical alloys 51# (Al-Sc-Zr-Er-Si alloy), 52# (Al-Zr-Tm-Fe-Si), 53# (Al-Zr-Er-B), 54# (Al-Sc-Zr-Y), 55# (Al-Sc-Zr-Yb-Si) of the existing patents are compared. It can be seen that the alloy products of the present invention show a good match of strength-plasticity-heat resistance-corrosion resistance.

Claims

1. A high heat-resistant, high plasticity, and corrosion-resistant aluminum alloy material, characterized in that: The aluminum alloy contains: Si 0.03-0.24wt%, Sc 0.06-1.0wt%, Zr 0.10-1.2wt%, Y 0.04-0.9wt%, Mg<0.01wt%, the total content of impurity elements Ti, V, Cr, Mn, Ni, and Ca is ≤0.03wt%, and the rest is Al and unavoidable impurities. In the aluminum alloy, the contents of Sc, Zr, and Y satisfy the relationship: 1.5≤[(3×Sc)+(2×Zr)] / (3×Y)≤4.5; A method for producing an aluminum alloy material, comprising the following steps: (1) manufacturing an ingot of the aluminum alloy material; (2) performing homogenization heat treatment on the obtained ingot; (3) Rapidly cool the ingot after homogenization heat treatment to room temperature, with a cooling rate of ≥50°C / s; (4) performing artificial aging heat treatment on the cooled ingot at a temperature of 370-430°C for 16-48 hours; (5) hot deforming the ingot into a desired processed material form, or hot deforming the ingot into a pre-processed material, by one or more hot deformation processing methods selected from extrusion, rolling and forging; (6) The pre-processed material is reheated and cold-formed into the required processed material form.

2. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Si 0.04-0.22wt%, Sc 0.07-0.6wt%, Zr 0.12-0.9wt%, and Y 0.05-0.5wt%.

3. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 2, characterized in that: The aluminum alloy contains: Si 0.05-0.20wt%, Sc 0.08-0.3wt%, Zr 0.15-0.5wt%, and Y 0.05-0.3wt%.

4. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Mg≤0.008wt%.

5. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 4, characterized in that: The aluminum alloy contains: Mg≤0.005wt%.

6. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 5, characterized in that: The aluminum alloy contains: Mg≤0.003wt%.

7. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Ti 0.001-0.01wt%.

8. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: V 0.001-0.01wt%.

9. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: 0.005-0.02wt% Cr.

10. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Mn 0.001-0.02wt%.

11. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Ni 0.005-0.02wt%.

12. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The aluminum alloy contains: Ca 0.001-0.01wt%.

13. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The unavoidable impurities include elements unintentionally introduced as impurities during the process of manufacturing the alloy ingot, and Fe in the aluminum alloy is ≤0.20wt%, and other impurity elements are ≤0.10wt% each, and the total is ≤0.30wt%.

14. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 13, characterized in that: The unavoidable impurities include elements unintentionally introduced as impurities during the process of manufacturing the alloy ingot, and Fe in the aluminum alloy is ≤0.15wt%, and other impurity elements are ≤0.05wt% each, and the total is ≤0.20wt%.

15. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 14, characterized in that: In the aluminum alloy, Fe≤0.10wt%.

16. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: In step (1), the ingot is manufactured by means of smelting, degassing, removing inclusions and semi-continuous casting. During the smelting process, the content and proportion of alloy elements are quickly adjusted through online composition detection and analysis, and the entire ingot manufacturing process is completed.

17. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: In step (2), the homogenization heat treatment is a single-stage homogenization heat treatment performed at a temperature in the range of 600-640° C. for a total time of 16-72 hours.

18. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: In step (3), the ingot is rapidly cooled to room temperature by using a self-selected cooling medium such as spray quenching, immersion quenching, strong wind cooling, or a combination thereof.

19. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: In step (5), the preheating temperature before each thermal deformation process is 350-400°C, and the processing time is 1-6 hours.

20. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: In step (6), the cold deformation passes also include an intermediate annealing treatment at 330-370°C / 0.5-6h.

21. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The method further includes step (7), wherein the processed material obtained in step (5) or step (6) is subjected to stress relief annealing treatment.

22. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 21, characterized in that: In step (7), the stress relief annealing treatment is performed at a temperature of 300-400°C and for a time of 3-6 hours.

23. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 21, characterized in that: After step (7), the method further includes the following steps: straightening the processed material after stress relief annealing treatment, using roller straightening, stretch straightening, stretch bending straightening and a combination thereof to improve the straightness of the processed material for subsequent processing and application.

24. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 1, characterized in that: The processed material is a rod, a tube, a wire / cord, a plate or a forging product.

25. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to any one of claims 1 to 24, characterized in that: The aluminum alloy material density is ≤2.73g / cm 3 , room temperature tensile strength ≥180MPa, elongation ≥18%; after keeping at 400℃ for 100h, room temperature tensile strength ≥170MPa, elongation ≥17%, and anti-exfoliation corrosion grade is not lower than PB grade.

26. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 25, characterized in that: The room temperature tensile strength of the aluminum alloy material is ≥190 MPa, and the elongation is ≥19%; after being kept at 400°C for 100 hours, the room temperature tensile strength is ≥175 MPa, and the elongation is ≥18%, and the exfoliation corrosion resistance grade is not lower than PA grade.

27. The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to claim 26, characterized in that: The room temperature tensile strength of the aluminum alloy material is ≥200 MPa, and the elongation is ≥20%; after being kept at 400°C for 100 hours, the room temperature tensile strength is ≥180 MPa, and the elongation is ≥19%, and the exfoliation corrosion resistance grade is not lower than grade N.

28. A high heat-resistant, high plasticity, and corrosion-resistant aluminum alloy material, characterized in that: The aluminum alloy contains: Si 0.03-0.24wt%, Sc 0.06-1.0wt%, Zr 0.10-1.2wt%, Y 0.04-0.9wt%, Mg<0.01wt%, the total content of impurity elements Ti, V, Cr, Mn, Ni, and Ca is ≤0.03wt%, and the rest is Al and unavoidable impurities. In the aluminum alloy, the contents of Sc, Zr, and Y satisfy the relationship: 1.5≤[(3×Sc)+(2×Zr)] / (3×Y)≤4.5; The method for producing an aluminum alloy material comprises the following steps: (1) preparing aluminum alloy castings of the aluminum alloy material by smelting, degassing, removing inclusions and sand mold, or metal mold casting, or die casting; during the smelting process, quickly adjusting the content and ratio of alloy elements through online composition detection and analysis, and completing the entire casting manufacturing process; (2) subjecting the obtained aluminum alloy casting to a homogenization heat treatment at a temperature in the range of 600 to 640° C. for a total time of 16 to 72 hours; (3) After homogenization, the aluminum alloy castings are rapidly cooled to room temperature by spray quenching, immersion quenching, strong wind cooling or a combination thereof using a self-selected cooling medium, with a cooling rate of ≥40°C / s; (4) Perform artificial aging heat treatment on the aluminum alloy castings, the artificial aging temperature is 370~430℃, and the time is 16~48h.

29. A welding product, characterized in that: The product is formed by welding the high heat-resistant, high-plasticity and corrosion-resistant aluminum alloy material according to any one of claims 1 to 28 with itself or other alloys; the welding methods include stir friction welding, fusion welding, brazing, electron beam welding and laser welding.

30. A final component, characterized in that The high heat-resistant, high-plasticity, and corrosion-resistant aluminum alloy material according to any one of claims 1 to 28 is processed into a final component through various surface treatments, stamping, and machining.

31. The final component according to claim 30, characterized in that The final component is a heat-resistant structural component.

Citation Information

Patent Citations

  • High-conductive heat-resistant aluminium alloy conductor and preparation method thereof

    CN102021444A

  • High-strength high-conduction heat resistance aluminium conductor material and preparation method thereof

    CN102965550A

  • Light high-conductivity and heat-resistant aluminum conductor and preparation method thereof

    CN105734353A

  • High-conductivity heat-resisting and corrosion-proof aluminum alloy wire and preparation process and application

    CN106834814A

  • Super-heat-resistant aluminum alloy conductor, preparation method thereof and steel core super-heat-resistant aluminum alloy stranded wire