Preparation method and application of iron-carbon primary battery adsorbent

The preparation of iron-carbon primary cell adsorbent by mixing cerium, manganese, iron salt and biomass powder has solved the problem of low pollutant treatment efficiency in the prior art, achieved the effect of efficient removal of pollutants in water, and simplified preparation process reduces costs.

CN118437286BActive Publication Date: 2024-11-12CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410904191.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The existing iron-carbon primary cell adsorbents are inefficient in contaminant treatment, making it difficult to effectively remove heavy metal ions and organic pollutants in water, and the preparation process is complex and costly.

Method used

The mixture of cerium, manganese, iron salt and biomass powder is used to mix cerium, manganese, iron salt and biomass powder, and dried at a constant temperature and carbonized in a carbonization furnace to generate an iron-carbon primary cell adsorbent with multi-stage potential difference, and electrostatic adsorption, ion trapping and Chemical adsorption and other methods enhance the ability to remove pollutants.

Benefits of technology

The pollutant removal ability of iron-carbon primary cell adsorbent is significantly improved, especially the adsorption properties of COD, ammonia nitrogen, total phosphorus and heavy metal mercury in the waste leachate, simplifying the preparation process and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118437286B_ABST
    Figure CN118437286B_ABST
Patent Text Reader

Abstract

The present invention discloses a preparation method and application of an iron-carbon primary battery adsorbent. The method of the present invention has a simple preparation process, and the required raw materials and reagents are widely available and easy to obtain. The present invention simultaneously prepares activated carbon while achieving the reduction of cerium, manganese and iron, thereby preparing a new type of iron-carbon primary battery adsorbent material. The prepared new type of iron-carbon primary battery has significantly better adsorption performance than traditional iron-carbon primary batteries, and can effectively remove COD, ammonia nitrogen, total phosphorus and heavy metal pollutants in landfill leachate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of research and development of new adsorption materials, and in particular relates to a preparation method and application of an iron-carbon primary battery adsorbent. Background Art

[0002] In the context of increasingly severe environmental pollution and resource depletion, the development and application of new environmental protection technologies are particularly important. As a low-cost, high-efficiency energy conversion and pollutant treatment technology, the iron-carbon primary battery has received widespread attention. The performance and efficiency of the iron-carbon primary battery largely depend on the performance of its adsorbent. Therefore, the preparation of new iron-carbon primary battery adsorbents is of great significance for promoting the development of iron-carbon primary battery technology and solving environmental pollution problems. The iron-carbon primary battery is a battery based on the principle of metal corrosion. Its working principle is to generate current through the redox reaction between iron and carbon. As an environmentally friendly energy conversion and pollutant treatment technology, the iron-carbon primary battery has great potential in environmental governance. By preparing new iron-carbon primary battery adsorbents, the adsorption and removal capacity of iron-carbon primary batteries for pollutants can be further improved. The new adsorbent can more effectively adsorb and remove harmful substances such as heavy metal ions and organic pollutants in water, thereby achieving purification and repair of water bodies.

[0003] The preparation of new iron-carbon primary battery adsorbents involves knowledge and technology from multiple disciplines such as materials science and chemical engineering. During the preparation process, researchers need to constantly explore new materials, new preparation methods and new application fields. This can not only promote the development of materials science, but also provide new ideas and methods for research in other fields. With the increasing severity of the global energy crisis and environmental problems, countries are actively exploring new pollutant treatment technologies. Therefore, we should strengthen the research and development of the preparation of new iron-carbon primary battery adsorbents, constantly explore new materials, new preparation methods and new application fields, and make greater contributions to promoting the development of environmental undertakings. Summary of the invention

[0004] Purpose of the invention: The purpose of the present invention is to provide a preparation method and application of an iron-carbon primary battery adsorbent.

[0005] Technical solution: The preparation method of the iron-carbon primary battery adsorbent of the present invention comprises the following steps:

[0006] (1) mixing cerium salt, manganese salt and iron salt, and stirring evenly to obtain cerium-manganese-iron mixed salt;

[0007] (2) adding water to the cerium-iron-manganese mixed salt, mixing, and stirring to obtain a cerium-iron-manganese mixed solution;

[0008] (3) mixing the cerium-ferromanganese mixed liquid and the biomass powder, and stirring to obtain a cerium-ferromanganese biomass slurry;

[0009] (4) The cerium-ferromanganese biomass slurry is dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain an iron-carbon primary battery adsorbent.

[0010] Furthermore, it is characterized in that the molar ratio of cerium, manganese and iron in the cerium salt, manganese salt and iron salt in step (1) is 0.005~0.075:0.025~0.125:1.

[0011] Furthermore, the cerium salt described in step (1) is any one or more combinations of cerium chloride, cerium sulfate, cerium nitrate, ammonium cerium nitrate, ammonium cerium sulfate, and cerium acetate.

[0012] Furthermore, the manganese salt in step (1) is any one or more combinations of manganous sulfate, manganous chloride, potassium manganate and potassium permanganate.

[0013] Furthermore, the iron salt in step (1) is any one or more combinations of ferrous sulfate, ferric sulfate, ferrous chloride and ferric chloride.

[0014] Furthermore, the liquid-to-solid ratio of water and cerium-manganese-iron mixed salt in step (2) is 20-120:1 mL / g, and the stirring time is 0.25-0.75 hours.

[0015] Furthermore, the liquid-to-solid ratio of the cerium-ferromanganese mixed solution and the biomass powder in step (3) is 0.6-1.2:1 mL / g, and the stirring time is 0.5-2.5 hours.

[0016] Furthermore, the biomass powder in step (3) is any one or more combinations of straw powder, sawdust powder, bamboo powder, coconut shell powder, peanut shell powder, walnut shell powder, bagasse powder, and tea dregs powder, and the particle size of the biomass powder is 200-800 mesh.

[0017] Furthermore, the drying temperature in step (4) is 100-200° C., the drying time is 2-6 hours, the carbonization temperature is 350-850° C., and the carbonization time is 0.5-5.5 hours.

[0018] The iron-carbon primary battery adsorbent prepared by the preparation method of the present invention is used in purifying landfill leachate or mercury-containing pollutants.

[0019] Reaction mechanism: Mix the cerium-manganese-iron mixed liquid and biomass powder. During the stirring process, cerium, manganese, and iron ions are adsorbed on the particle surface and stem pores of the biomass powder. After the cerium-manganese-iron biomass slurry is dried at a constant temperature, it is placed in a carbonization furnace. Under the high temperature environment, the lignin, cellulose, hemicellulose, and other organic extracts in the biomass are fully degraded and pyrolyzed under the catalytic action of cerium, manganese, and iron, and the structure is rapidly carbonized to generate gas and liquid products. Under the high temperature environment, cerium, manganese, and iron further diffuse, and react with the generated organic gas and liquid products on the formed biocarbon-based surface, obtain electrons from the organic gas and liquid products, and reduce to form a mixture of elemental iron, cerium, and manganese, and the mixture of elemental iron, cerium, and manganese is dispersed on the surface and pores of the biocarbon-based material. For some cerium and manganese, the reduction reaction is not sufficient, and they will also combine with oxygen atoms to form oxide particles mixed with divalent manganese, trivalent manganese, tetravalent manganese, and trivalent cerium. Manganese and cerium oxide particles diffuse and dope in the mixture of elemental iron, cerium and manganese, and adhere to the surface and pores of the biocarbon base. During the adsorption process, the mixture of elemental iron, cerium and manganese and the carbonized material form a primary battery. The multi-level potential difference can accelerate the degradation of organic pollutants. At the same time, the manganese and cerium oxide particles doped on the surface and pores of the primary battery can also enhance the removal and adsorption of heavy metal pollutants in the waste liquid through electrostatic adsorption, ion capture, chemical adsorption and other methods.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the method of the present invention has a simple preparation process, and the required raw materials and reagents are widely available and easy to obtain. The present invention simultaneously prepares activated carbon while achieving the reduction of cerium, manganese and iron, thereby preparing a new type of iron-carbon primary battery adsorption material. The prepared new type of iron-carbon primary battery has significantly better adsorption performance than the traditional iron-carbon primary battery, and can effectively remove COD, ammonia nitrogen, total phosphorus and heavy metal pollutants in landfill leachate. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION

[0022] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.

[0023] Source of raw materials and composition description:

[0024] Sampling and basic properties of landfill leachate in the examples: The landfill leachate stock solution was taken from Zhuji Sanfeng Environmental Protection Energy Co., Ltd. The COD mass concentration of this batch of concentrated landfill leachate was 3639 mg / L, the total phosphorus concentration was 294 mg / L, and the ammonia nitrogen concentration was 1062 mg / L. 500 mg of mercury pollutant was dissolved in 1 L of landfill leachate stock solution to obtain landfill leachate for testing.

[0025] Example 1 Effect of the molar ratio of cerium, manganese and iron on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0026] According to the molar ratio of cerium, manganese and iron: 0.0025:0.025:1, 0.003:0.025:1, 0.004:0.125:1, 0.005:0.01:1, 0.005:0.015:1, 0.005:0.02:1, 0.005:0.025:1, 0.04:0.025:1, 0.075:0.025:1, 0.005:0.075:1, 0.04:0.075:1, 0.075:0.075:1 , 0.005:0.125:1, 0.04:0.125:1, 0.075:0.125:1, 0.075:0.15:1, 0.075:0.175:1, 0.075:0.2:1, 0.08:0.125:1, 0.085:0.125:1, 0.09:0.125:1 Weigh cerium salt, manganese salt, and iron salt respectively, mix, and stir evenly to obtain a cerium-manganese-iron mixed salt, wherein the cerium salt is cerium chloride, the manganese salt is manganous sulfate, and the iron salt is ferrous sulfate. Mix water and cerium-manganese-iron mixed salt according to a liquid-solid ratio of 20:1 mL / g, stir for 0.25 hours, and obtain a cerium-manganese-iron mixed solution. The cerium-ferromanganese mixed liquid and the biomass powder were mixed at a liquid-solid ratio of 0.6:1 mL / g and stirred for 0.5 hours to obtain a cerium-ferromanganese biomass slurry, wherein the biomass powder was straw powder and the particle size of the biomass powder passed a 200-mesh sieve. The cerium-ferromanganese biomass slurry was dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain a new iron-carbon primary battery adsorbent, wherein the drying temperature was 100°C, the drying time was 2 hours, the carbonization temperature was 350°C, and the carbonization time was 0.5 hours.

[0027] Adsorption test: The prepared adsorbent and the test landfill leachate were mixed at a solid-liquid ratio of 1:1 g / L, stirred at 120 rpm for half an hour, and centrifuged at 5000 rpm for 5 minutes to obtain a supernatant and a separation slurry.

[0028] COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection: The chemical oxygen demand (COD) concentration in the solution is determined in accordance with the national standard "Determination of Chemical Oxygen Demand in Water Quality - Dichromate Method" (GB 11914-1989); the ammonia nitrogen concentration in the solution is determined in accordance with the "Determination of Ammonia Nitrogen in Water Quality - Salicylic Acid Spectrophotometric Method" (HJ536-2009); the total phosphorus concentration in the solution is determined in accordance with the standard "Determination of Phosphate and Total Phosphorus in Water Quality - Continuous Flow - Ammonium Molybdate Spectrophotometric Method" (HJ 670-2013). The dissolved mercury concentration in the solution is determined in accordance with the standard "Determination of Mercury, Arsenic, Selenium, Bismuth and Antimony in Water Quality - Atomic Fluorescence Method" (HJ 695-2014). The adsorption performance of adsorbents for COD, ammonia nitrogen, total phosphorus, and mercury pollutants is calculated according to formula (1), where: is the pollutant adsorption capacity of the new iron-carbon primary battery adsorbent mg / g, and are the pollutant concentrations in the solution before and after the adsorption experiment in mg / L, V is the volume of the experimental leachate in L (1L), and m is the dosage of the new iron-carbon primary battery adsorbent (1g).

[0029] (1)

[0030] The test results of the adsorption capacity of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this embodiment are shown in Table 1.

[0031] Table 1 Effect of the molar ratio of cerium, manganese and iron on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0032]

[0033] It can be seen from Table 1 that when the molar ratio of cerium, manganese and iron is less than 0.005:0.025:1 (such as in Table 1, the molar ratio of cerium, manganese and iron = 0.004:0.125:1, 0.003:0.025:1, 0.0025:0.025:1, 0.005:0.02:1, 0.005:0.015:1, 0.005:0.01:1 and lower ratios not listed in Table 1), less cerium salt and manganese salt are added, the synergistic catalytic performance of cerium, manganese and iron decreases during the carbonization process, and the amount of cerium-manganese mixed oxide generated decreases, which reduces the adsorption performance of the prepared new iron-carbon primary battery adsorbent, resulting in a significant decrease in the adsorption capacity for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the molar ratio of cerium, manganese and iron decreases. When the molar ratio of cerium, manganese and iron is equal to 0.005~0.075:0.025~0.125:1 (as in Table 1, the molar ratio of cerium, manganese and iron = 0.005:0.025:1, 0.04:0.025:1, 0.075:0.025:1, 0.005:0.075:1, 0.04:0.075:1, 0.075:0.075:1, 0.005:0.125:1, 0.04:0.125:1, 0.075:0.125:1), the cerium-manganese-iron mixed solution and the biomass powder are mixed. During the stirring process, the cerium, manganese and iron ions are adsorbed on the particle surface and stem pores of the biomass powder. After the cerium-manganese-iron biomass slurry is dried at a constant temperature, it is placed in a carbonization furnace. Under high temperature conditions, the lignin, cellulose, hemicellulose and other organic extracts in the biomass are fully degraded and pyrolyzed under the catalytic action of cerium, manganese and iron, and the structure is rapidly carbonized to generate gas and liquid products. Under high temperature conditions, cerium, manganese and iron further diffuse, and react with the generated organic gas and liquid products on the formed biological carbon-based surface, obtain electrons from the organic gas and liquid products, and reduce to form a mixture of elemental iron, cerium and manganese, and the mixture of elemental iron, cerium and manganese is dispersed on the surface and pores of the biological carbon-based material. For some cerium and manganese, the reduction reaction is insufficient, and they will also combine with oxygen atoms to form oxide particles mixed with divalent manganese, trivalent manganese, tetravalent manganese and trivalent cerium. Manganese and cerium oxide particles diffuse and are doped in the mixture of elemental iron, cerium and manganese, and adhere to the surface and pores of the biological carbon-based material. Finally, the prepared iron-carbon primary battery adsorbents had COD adsorption capacity greater than 1678 mg / g, ammonia nitrogen adsorption capacity greater than 342 mg / g, total phosphorus adsorption capacity greater than 109 mg / g, and heavy metal mercury adsorption capacity greater than 214 mg / g.When the molar ratio of cerium, manganese and iron is greater than 0.075:0.125:1 (as in Table 1, the molar ratio of cerium, manganese and iron = 0.075:0.15:1, 0.075:0.175:1, 0.075:0.2:1, 0.08:0.125:1, 0.085:0.125:1, 0.09:0.125:1 and higher ratios not listed in Table 1), excessive addition of cerium salt and manganese salt will lead to decreased synergistic catalytic performance of cerium, manganese and iron during carbonization, resulting in decreased adsorption performance of the prepared new iron-carbon primary battery adsorbent, resulting in a significant decrease in the adsorption capacity for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the molar ratio of cerium, manganese and iron further increases.

[0034] Therefore, in summary, considering the benefits and costs, when the molar ratio of cerium, manganese and iron is equal to 0.005~0.075:0.025~0.125:1, it is most conducive to improving the adsorption performance of the prepared new iron-carbon primary battery adsorbent.

[0035] Example 2 Effect of the liquid-to-solid ratio of cerium-manganese-iron mixed solution and biomass powder on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0036] According to the molar ratio of cerium, manganese and iron of 0.075:0.125:1, cerium salt, manganese salt and iron salt are weighed respectively, mixed and stirred evenly to obtain a cerium-manganese-iron mixed salt, wherein the cerium salt is cerium sulfate, the manganese salt is manganous chloride, and the iron salt is ferric sulfate. Water and cerium-manganese-iron mixed salt are mixed according to a liquid-solid ratio of 70:1 mL / g, stirred for 0.5 hours, and a cerium-manganese-iron mixed solution is obtained. According to the liquid-solid ratio of 0.35:1 mL / g, 0.4:1 mL / g, 0.45:1 mL / g, 0.6:1 mL / g, 0.9:1 mL / g, 1.2:1 mL / g, 1.3:1 mL / g, 1.4:1 mL / g, 1.5:1 mL / g, the cerium-manganese-iron mixed solution and biomass powder are mixed and stirred for 1.5 hours to obtain a cerium-manganese-iron biomass slurry, wherein the biomass powder is sawdust powder, and the particle size of the biomass powder passes through a 500 mesh sieve. The cerium-manganese-iron biomass slurry is dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain a new type of iron-carbon primary battery adsorbent, wherein the drying temperature is 150°C, the drying time is 4 hours, the carbonization temperature is 600°C, and the carbonization time is 3 hours.

[0037] The adsorption test, COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection are all the same as in Example 1. The adsorption capacity detection results of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 2.

[0038] Table 2 Effect of liquid-to-solid ratio of cerium-manganese-iron mixed solution and biomass powder on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0039]

[0040] It can be seen from Table 2 that when the liquid-to-solid ratio of cerium-manganese-iron mixed solution and biomass powder is less than 0.6:1 mL / g (such as in Table 2, the liquid-to-solid ratio of cerium-manganese-iron mixed solution and biomass powder = 0.45:1 mL / g, 0.4:1 mL / g, 0.35:1 mL / g and lower ratios not listed in Table 2), less cerium-manganese-iron mixed solution is added, the synergistic catalytic performance of cerium, manganese and iron decreases during the carbonization process, and the amount of cerium-manganese mixed oxide generated decreases, which reduces the adsorption performance of the prepared new iron-carbon primary battery adsorbent, resulting in a significant decrease in the adsorption capacity for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the liquid-to-solid ratio of cerium-manganese-iron mixed solution and biomass powder decreases. When the liquid-solid ratio of ferro-cerium manganese mixed liquid and biomass powder is equal to 0.6~1.2:1mL / g (as in Table 2, the liquid-solid ratio of ferro-cerium manganese mixed liquid and biomass powder = 0.6:1mL / g, 0.9:1mL / g, 1.2:1mL / g), mix the ferro-cerium manganese mixed liquid and biomass powder. During the stirring process, cerium, manganese, and iron ions are adsorbed on the particle surface and stem pores of biomass powder. After the ferro-cerium manganese biomass slurry is dried at a constant temperature, it is placed in a carbonization furnace. Under high temperature, the lignin, cellulose, hemicellulose and other organic extracts in the biomass are fully degraded and pyrolyzed under the catalytic action of cerium, manganese and iron, and the structure is rapidly carbonized to generate gas and liquid products. Under high temperature environment, cerium, manganese and iron further diffuse and react with the generated organic gas and liquid products on the formed biocarbon-based surface, obtain electrons from the organic gas and liquid products, and reduce to form a mixture of elemental iron, cerium and manganese, and the elemental iron, cerium and manganese mixture is dispersed on the surface and pores of the biocarbon-based material. For some cerium and manganese, the reduction reaction is not sufficient, and they will also combine with oxygen atoms to form oxide particles mixed with divalent manganese, trivalent manganese, tetravalent manganese and trivalent cerium. Manganese and cerium oxide particles diffuse and dope in the mixture of elemental iron, cerium and manganese, and adhere to the surface and pores of the biocarbon-based material. Finally, the prepared iron-carbon primary battery adsorbent has an adsorption capacity of more than 1823 mg / g for COD of landfill leachate, more than 393 mg / g for ammonia nitrogen, more than 141 mg / g for total phosphorus, and more than 249 mg / g for heavy metal mercury. When the liquid-to-solid ratio of cerium-ferromanganese mixed solution and biomass powder is greater than 1.2:1mL / g (such as in Table 2, the liquid-to-solid ratio of cerium-ferromanganese mixed solution and biomass powder = 1.3:1mL / g, 1.4:1mL / g, 1.5:1mL / g and higher ratios not listed in Table 2), too much cerium-ferromanganese is added, and the biomass powder is relatively small. The synergistic catalytic performance of cerium, manganese and iron decreases during the carbonization process, and the carbonization effect becomes worse, resulting in a decrease in the adsorption performance of the prepared new iron-carbon primary battery adsorbent, resulting in a significant decrease in the adsorption capacity for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the liquid-to-solid ratio of cerium-ferromanganese mixed solution and biomass powder further increases.

[0041] Therefore, in summary, considering the benefits and costs, when the liquid-to-solid ratio of the cerium-manganese-iron mixed solution and the biomass powder is equal to 0.6~1.2:1mL / g, it is most conducive to improving the adsorption performance of the prepared new iron-carbon primary battery adsorbent.

[0042] Example 3 Effect of carbonization time on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0043] According to the molar ratio of cerium, manganese and iron of 0.075: 0.125: 1, cerium salt, manganese salt and iron salt are weighed respectively, mixed and stirred evenly to obtain cerium-ferromanganese mixed salt, wherein the cerium salt is cerium nitrate, the manganese salt is potassium manganate, and the iron salt is ferrous chloride. Water and cerium-ferromanganese mixed salt are mixed according to a liquid-solid ratio of 120: 1mL / g, stirred for 0.75 hours, and cerium-ferromanganese mixed solution is obtained. According to a liquid-solid ratio of 1.2: 1mL / g, the cerium-ferromanganese mixed solution and biomass powder are mixed and stirred for 2.5 hours to obtain cerium-ferromanganese biomass slurry, wherein the biomass powder is bamboo powder, and the particle size of the biomass powder passes through an 800 mesh sieve. The cerium-manganese-iron biomass slurry was dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain a new iron-carbon primary battery adsorbent, wherein the drying temperature was 200°C, the drying time was 6 hours, the carbonization temperature was 850°C, and the carbonization time was 0.25 hour, 0.3 hour, 0.4 hour, 0.5 hour, 3 hours, 5.5 hours, 5.75 hours, 6 hours, and 6.25 hours.

[0044] The adsorption test, COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection are all the same as in Example 1. The adsorption capacity detection results of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 3.

[0045] Table 3 Effect of carbonization time on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0046]

[0047] It can be seen from Table 3 that when the carbonization time is less than 0.5 hours (such as in Table 3, carbonization time = 0.4 hours, 0.3 hours, 0.25 hours and lower values ​​not listed in Table 3), the carbonization time is short, the synergistic catalytic performance of cerium, manganese and iron decreases during the carbonization process, and the amount of cerium-manganese mixed oxide generated decreases, which makes the adsorption performance of the prepared new iron-carbon primary battery adsorbent decrease, resulting in a significant decrease in the adsorption capacity of COD, ammonia nitrogen, total phosphorus and mercury pollutants as the carbonization time decreases. When the carbonization time is equal to 0.5~5.5 hours (such as in Table 3, carbonization time = 0.5 hours, 3 hours, 5.5 hours), the cerium-manganese-iron biomass slurry is dried at a constant temperature and placed in a carbonization furnace. Under high temperature conditions, lignin, cellulose, hemicellulose and other organic extracts in the biomass are fully degraded and pyrolyzed under the catalytic action of cerium, manganese and iron, and the structure is rapidly carbonized to generate gas and liquid products. Under high temperature environment, cerium, manganese and iron further diffuse and react with the generated organic gas and liquid products on the formed biocarbon-based surface, obtain electrons from the organic gas and liquid products, and reduce to form a mixture of elemental iron, cerium and manganese, and the elemental iron, cerium and manganese mixture is dispersed on the surface and pores of the biocarbon-based material. For some cerium and manganese, the reduction reaction is not sufficient, and they will also combine with oxygen atoms to form oxide particles mixed with divalent manganese, trivalent manganese, tetravalent manganese and trivalent cerium. Manganese and cerium oxide particles diffuse and dope in the mixture of elemental iron, cerium and manganese, and adhere to the surface and pores of the biocarbon-based material. Finally, the prepared iron-carbon primary battery adsorbent has an adsorption capacity of more than 1921 mg / g for COD of landfill leachate, ammonia nitrogen adsorption capacity of more than 430 mg / g, total phosphorus adsorption capacity of more than 162 mg / g, and heavy metal mercury adsorption capacity of more than 273 mg / g. When the carbonization time is greater than 5.5 hours (as in Table 3, carbonization time = 5.75 hours, 6 hours, 6.25 hours and higher values ​​not listed in Table 3), the carbonization time is too long, the material cokes and hardens, the synergistic catalytic performance of cerium, manganese and iron decreases during the carbonization process, and the carbonization effect becomes worse, resulting in a decrease in the adsorption performance of the prepared new iron-carbon primary battery adsorbent, resulting in a significant decrease in the adsorption capacity for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the carbonization time further increases.

[0048] Therefore, in summary, considering the benefits and costs, when the carbonization time is equal to 0.5~5.5 hours, it is most conducive to improving the adsorption performance of the prepared new iron-carbon primary battery adsorbent.

[0049] Example 4 Effect of cerium salt type on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0050] According to the molar ratio of cerium, manganese and iron of 0.075:0.125:1, cerium salt, manganese salt and iron salt are weighed respectively, mixed and stirred evenly to obtain cerium-manganese-iron mixed salt, wherein the cerium salt is any one of cerium chloride, cerium sulfate, cerium nitrate, ammonium cerium nitrate, ammonium cerium sulfate and cerium acetate, the manganese salt is potassium permanganate, and the iron salt is ferric chloride. Water and cerium-manganese-iron mixed salt are mixed according to a liquid-solid ratio of 120:1mL / g, stirred for 0.75 hours, and cerium-manganese-iron mixed liquid is obtained. According to the liquid-solid ratio of 1.2:1mL / g, the cerium-manganese-iron mixed liquid and biomass powder are mixed and stirred for 2.5 hours to obtain cerium-manganese-iron biomass slurry, wherein the biomass powder is coconut shell powder, and the particle size of the biomass powder passes through an 800 mesh sieve. The cerium-manganese-iron biomass slurry is dried at a constant temperature, and then placed in a carbonization furnace for carbonization treatment to obtain a new type of iron-carbon primary battery adsorbent, wherein the drying temperature is 200°C, the drying time is 6 hours, the carbonization temperature is 850°C, and the carbonization time is 5.5 hours.

[0051] The adsorption test, COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection are all the same as in Example 1. The adsorption capacity detection results of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 4.

[0052] Table 4 Effect of cerium salt types on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0053]

[0054] It can be seen from Table 4 that when the cerium salt is any one of cerium chloride, cerium sulfate, cerium nitrate, ammonium cerium nitrate, ammonium cerium sulfate, and cerium acetate, there is no significant difference in the adsorption performance of the prepared new iron-carbon primary battery adsorbent. In the adsorption process, the elemental iron, cerium, manganese mixture and carbonized material constitute the primary battery, and the multi-level potential difference can accelerate the degradation of organic pollutants. At the same time, the manganese and cerium oxide particles doped on the surface and pores of the primary battery can also enhance the removal and adsorption of heavy metal pollutants in the waste liquid by electrostatic adsorption, ion capture, chemical adsorption, etc.

[0055] Example 5 Effect of biomass powder type on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0056] According to the molar ratio of cerium, manganese and iron of 0.075:0.125:1, cerium salt, manganese salt and iron salt are weighed respectively, mixed and stirred evenly to obtain a cerium-ferromanganese mixed salt, wherein the cerium salt is ammonium cerium sulfate, the manganese salt is potassium permanganate, and the iron salt is ferric chloride. Water and cerium-ferromanganese mixed salt are mixed according to a liquid-solid ratio of 120:1 mL / g, stirred for 0.75 hours, and a cerium-ferromanganese mixed solution is obtained. The cerium-ferromanganese mixed solution and biomass powder are mixed according to a liquid-solid ratio of 1.2:1 mL / g, stirred for 2.5 hours, and a cerium-ferromanganese biomass slurry is obtained, wherein the biomass powder is any one of straw powder, sawdust powder, bamboo powder, coconut shell powder, peanut shell powder, walnut shell powder, bagasse powder, and tea slag powder, and the particle size of the biomass powder passes through an 800 mesh sieve. The cerium-ferromanganese biomass slurry was dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain a new type of iron-carbon primary battery adsorbent, wherein the drying temperature was 200°C, the drying time was 6 hours, the carbonization temperature was 850°C, and the carbonization time was 5.5 hours.

[0057] The adsorption test, COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection are all the same as in Example 1. The adsorption capacity detection results of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 5.

[0058] Table 5 Effect of biomass powder type on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0059]

[0060] It can be seen from Table 5 that when the biomass powder is any one of straw powder, sawdust powder, bamboo powder, coconut shell powder, peanut shell powder, walnut shell powder, bagasse powder, and tea residue powder, there is no significant difference in the adsorption performance of the prepared new iron-carbon primary battery adsorbent. In the adsorption process, the elemental iron, cerium, and manganese mixture and the carbonized material constitute the primary battery. The multi-level potential difference can accelerate the degradation of organic pollutants. At the same time, the manganese and cerium oxide particles doped on the surface and pores of the primary battery can also enhance the removal and adsorption of heavy metal pollutants in the waste liquid by electrostatic adsorption, ion capture, chemical adsorption, etc.

[0061] Effect of process type on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0062] The process of the present invention: according to the molar ratio of cerium, manganese and iron of 0.075:0.125:1, cerium salt, manganese salt and iron salt are weighed respectively, mixed and stirred evenly to obtain a cerium-manganese-iron mixed salt, wherein the cerium salt is cerium acetate, the manganese salt is potassium permanganate, and the iron salt is ferric chloride. Water and cerium-manganese-iron mixed salt are mixed according to a liquid-solid ratio of 120:1mL / g, stirred for 0.75 hours, and a cerium-manganese-iron mixed solution is obtained. The cerium-manganese-iron mixed solution and biomass powder are mixed according to a liquid-solid ratio of 1.2:1mL / g, stirred for 2.5 hours, and a cerium-manganese-iron biomass slurry is obtained, wherein the biomass powder is walnut shell powder, and the particle size of the biomass powder passes through an 800-mesh sieve. The cerium-manganese-iron biomass slurry is dried at a constant temperature, and then placed in a carbonization furnace for carbonization treatment to obtain a new iron-carbon primary battery adsorbent, wherein the drying temperature is 200°C, the drying time is 6 hours, the carbonization temperature is 850°C, and the carbonization time is 5.5 hours.

[0063] Comparative process 1: According to the molar ratio of manganese to iron of 0.125:1, manganese salt and iron salt were weighed respectively, mixed, and stirred evenly to obtain a manganese-iron mixed salt, wherein the manganese salt was potassium permanganate and the iron salt was ferric chloride. Water and manganese-iron mixed salt were mixed at a liquid-solid ratio of 120:1 mL / g and stirred for 0.75 hours to obtain a manganese-iron mixed solution. The manganese-iron mixed solution and biomass powder were mixed at a liquid-solid ratio of 1.2:1 mL / g and stirred for 2.5 hours to obtain a manganese-iron biomass slurry, wherein the biomass powder was walnut shell powder, and the particle size of the biomass powder passed through an 800-mesh sieve. The manganese-iron biomass slurry was dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain a new type of iron-carbon primary battery adsorbent, wherein the drying temperature was 200°C, the drying time was 6 hours, the carbonization temperature was 850°C, and the carbonization time was 5.5 hours.

[0064] Comparative process 2: According to the molar ratio of cerium, manganese and iron of 0.075:0.125:1, cerium salt, manganese salt and iron salt were weighed respectively, mixed and stirred evenly to obtain a cerium-manganese-iron mixed salt, wherein the cerium salt is cerium acetate, the manganese salt is potassium permanganate, and the iron salt is ferric chloride. Water and cerium-manganese-iron mixed salt were mixed at a liquid-solid ratio of 120:1mL / g and stirred for 0.75 hours to obtain a cerium-manganese-iron mixed solution. The cerium-manganese-iron mixed solution and biomass powder were mixed at a liquid-solid ratio of 1.2:1mL / g and stirred for 2.5 hours to obtain a cerium-manganese-iron biomass slurry, wherein the biomass powder was walnut shell powder, and the particle size of the biomass powder passed through an 800-mesh sieve. The cerium-manganese-iron biomass slurry was dried at a constant temperature to obtain a new iron-carbon primary battery adsorbent, wherein the drying temperature was 200°C and the drying time was 6 hours.

[0065] The adsorption test, COD, ammonia nitrogen, total phosphorus, and mercury pollutant concentration detection are all the same as in Example 1. The adsorption capacity detection results of the new iron-carbon primary battery adsorbent for COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 6.

[0066] Table 6 Effect of process type on the adsorption performance of the prepared iron-carbon primary battery adsorbent

[0067]

[0068] The adsorption capacity of the novel iron-carbon primary battery adsorbent prepared by the process of the present invention for COD, total phosphorus, ammonia nitrogen and mercury pollutants is significantly higher than that of the comparative process 1 and the comparative process 2 and higher than the sum of the two.

Claims

1. A method for preparing an iron-carbon primary battery adsorbent, characterized in that: The following steps are involved: (1) mixing cerium salt, manganese salt and iron salt, and stirring evenly to obtain cerium-manganese-iron mixed salt; The molar ratio of cerium, manganese and iron in the cerium salt, manganese salt and iron salt is 0.005-0.075:0.025-0.125:1; (2) adding water to the cerium-iron-manganese mixed salt, mixing, and stirring to obtain a cerium-iron-manganese mixed solution; (3) mixing the cerium-ferromanganese mixed liquid and the biomass powder, and stirring to obtain a cerium-ferromanganese biomass slurry; The liquid-to-solid ratio of the cerium-ferromanganese mixed solution and the biomass powder is 0.6-1.2:1 mL / g, and the stirring time is 0.5-2.5 hours; (4) The cerium-ferromanganese biomass slurry is dried at a constant temperature and then placed in a carbonization furnace for carbonization treatment to obtain an iron-carbon primary battery adsorbent.

2. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The cerium salt described in step (1) is any one or more combinations of cerium chloride, cerium sulfate, cerium nitrate, ammonium cerium nitrate, ammonium cerium sulfate, and cerium acetate.

3. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The manganese salt in step (1) is any one or more combinations of manganous sulfate, manganous chloride, potassium manganate and potassium permanganate.

4. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The iron salt described in step (1) is any one or more combinations of ferrous sulfate, ferric sulfate, ferrous chloride and ferric chloride.

5. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The liquid-to-solid ratio of water to the cerium-manganese-iron mixed salt in step (2) is 20-120:1 mL / g, and the stirring time is 0.25-0.75 hours.

6. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The biomass powder in step (3) is any one or more combinations of straw powder, sawdust powder, bamboo powder, coconut shell powder, peanut shell powder, walnut shell powder, bagasse powder, and tea dregs powder, and the particle size of the biomass powder is 200-800 meshes.

7. The method for preparing the iron-carbon primary battery adsorbent according to claim 1, characterized in that: The drying temperature in step (4) is 100-200° C., the drying time is 2-6 hours, the carbonization temperature is 350-850° C., and the carbonization time is 0.5-5.5 hours.

8. Use of the iron-carbon primary battery adsorbent prepared by the preparation method according to claims 1 to 7 in purifying landfill leachate or mercury-containing pollutants.