A kind of polypropylene synthetic paper with anti-ultraviolet and anti-aging properties and preparation method thereof

By introducing specific anti-aging agents and antistatic agents into polypropylene synthetic paper and adopting extrusion tensile corona technology, the problem of insufficient anti-ultraviolet anti-aging performance of polypropylene synthetic paper is solved, and efficient anti-oxidation performance and machinery are achieved Performance improvement.

CN118438763BActive Publication Date: 2024-11-15烟台富利新材料科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897011.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-15
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

The existing polypropylene synthetic paper has poor UV resistance and aging resistance when used outdoors, which cannot meet the requirements of excellent UV resistance in increasing application scenarios.

Method used

Polypropylene synthetic paper including an outer surface layer, an intermediate layer and an inner surface layer, the outer surface layer and the inner surface layer contain the anti-aging agent 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N-[4-({ 4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionylamino]phenyl}amino)phenyl]propionamide, the intermediate layer contains antistatic agent AS11N or Armostat 400, by extrusion , stretching, corona and other processes to improve the anti-ultraviolet and anti-oxidation aging performance.

Benefits of technology

The polypropylene synthetic paper has significantly improved the anti-ultraviolet and anti-oxidation aging performance, and maintains excellent lateral and longitudinal mechanical properties after aging, with a lateral tensile strength higher than 110MPa and a longitudinal tensile strength higher than 65MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118438763B_ABST
    Figure CN118438763B_ABST
Patent Text Reader

Abstract

The present invention discloses a polypropylene synthetic paper with UV resistance and anti-aging properties and a preparation method thereof, and belongs to the technical field of synthetic paper. The polypropylene synthetic paper comprises an outer layer, an intermediate layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 30-40 parts of polypropylene, 1-2 parts of titanium dioxide, 2-3 parts of antioxidant, and 1-4 parts of calcium carbonate; the intermediate layer comprises: 40-50 parts of polypropylene, 1-2 parts of titanium dioxide, and 2-3 parts of antistatic agent; the raw materials and parts of the inner layer are the same as those of the outer layer; the antioxidant is prepared by acylation reaction of 4,4'-diaminodiphenylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride. The present invention improves the UV resistance and anti-oxidation aging performance of polypropylene synthetic paper by adopting the prepared antioxidant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of synthetic paper, and in particular to an anti-ultraviolet and anti-aging polypropylene synthetic paper and a preparation method thereof. Background Art

[0002] Polypropylene synthetic paper has many advantages, such as low carbon and environmental protection, low specific gravity, high strength, good weather resistance, good tear resistance, soft texture, excellent printing performance and durability. Polypropylene synthetic paper has been widely used in high-quality printing, high-end packaging and special uses because it has the characteristics of both plastic and paper. With the increase in the application scenarios of polypropylene synthetic paper, more requirements are put forward for polypropylene synthetic paper, such as excellent anti-UV and anti-aging performance when used outdoors.

[0003] A Chinese invention patent with publication number CN104943308A discloses a polypropylene synthetic paper and a production method thereof. The polypropylene synthetic paper includes an outer layer, an intermediate layer and an inner layer. The outer layer is mainly prepared from titanium dioxide, calcium carbonate and a modified polypropylene copolymer, the intermediate layer is mainly prepared from polypropylene, and the inner layer is mainly prepared from titanium dioxide, calcium carbonate and a modified polypropylene copolymer. The paper has excellent mechanical properties, but poor UV and anti-aging properties. Summary of the invention

[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a polypropylene synthetic paper that is UV-resistant and anti-aging and a preparation method thereof.

[0005] To achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A polypropylene synthetic paper with UV resistance and anti-aging properties, comprising an outer layer, an intermediate layer and an inner layer, wherein the outer layer comprises the following raw materials in parts by weight: 30-40 parts of polypropylene, 1-2 parts of titanium dioxide, 2-3 parts of antioxidant, and 1-4 parts of calcium carbonate;

[0007] The middle layer comprises the following raw materials in parts by weight: 40-50 parts of polypropylene, 1-2 parts of titanium dioxide, and 2-3 parts of antistatic agent;

[0008] The raw materials and the number of portions of the inner surface layer are the same as those of the outer surface layer;

[0009] The antioxidant is 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N-[4-({4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionylamino]phenyl}amino)phenyl]propionamide, which is prepared by acylation reaction of 4,4'-diaminodiphenylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride.

[0010] The antistatic agent is one of AS11N antistatic agent and Armostat 400 antistatic agent.

[0011] The antioxidant is prepared by the following method:

[0012] Dissolve 4,4'-diaminodiphenylamine in tetrahydrofuran, add triethylamine dropwise at 0-5°C, add a tetrahydrofuran solution of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride dropwise under nitrogen protection, heat to 50-60°C for reaction for 18-24h, and then post-treat to obtain the antioxidant, the reaction equation of which is as follows:

[0013]

[0014] The molar ratio of the 4,4'-diaminodiphenylamine to the 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 1:(3-5).

[0015] The molar ratio of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride to triethylamine is 1:(1-1.2).

[0016] A method for preparing UV-resistant and anti-aging polypropylene synthetic paper comprises the following steps:

[0017] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0018] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming;

[0019] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0020] Due to the adoption of the above technical solution, the beneficial effects of the present invention include:

[0021] The invention prepares a novel 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N-[4-({4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionylamino]phenyl}amino)phenyl]propionamide antioxidant and age-preserving agent through acylation reaction of 4,4'-diaminodiphenylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride. The invention improves the anti-ultraviolet and anti-oxidation ageing performance of polypropylene synthetic paper by adopting the prepared age-preserving agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the antioxidant prepared in Example 2. DETAILED DESCRIPTION

[0023] The invention will be further described below in conjunction with the embodiments, but the invention is not limited to these embodiments.

[0024] Example 1 Preparation of antioxidant

[0025] Dissolve 0.1 mol 4,4'-diaminodiphenylamine in 200 ml tetrahydrofuran, add 0.36 mol triethylamine dropwise at 0-5°C, and under nitrogen protection, add 0.3 mol 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18wt%) dropwise for 30 minutes. After the addition is completed, heat to 50°C and react for 24 hours. After post-treatment, an antioxidant is obtained.

[0026] Example 2 Preparation of antioxidant

[0027] Dissolve 0.1mol 4,4'-diaminodiphenylamine in 200ml tetrahydrofuran, add 0.48mol triethylamine dropwise at 0-5℃, and under nitrogen protection, add 0.4mol 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18wt%) dropwise for 30min. After the addition is complete, heat to 55℃ and react for 22h. After post-treatment, an antioxidant is obtained. The H-NMR spectrum data of the antioxidant are as follows: 1 H NMR (300 MHz, DMSO- d 6) δ 9.72 (s, 2H), 7.62 (s, 1H), 7.58 - 7.48 (m, 4H), 7.06 - 6.94 (m, 8H), 6.81 (s, 2H), 2.87 (tq, J = 7.0, 0.9 Hz, 4H),2.64 (td, J = 7.1, 0.7 Hz, 4H), 1.35 (s, 36H).

[0028] Example 3 Preparation of antioxidant

[0029] Dissolve 0.1 mol 4,4'-diaminodiphenylamine in 200 ml tetrahydrofuran, add 0.55 mol triethylamine dropwise at 0-5°C, and under nitrogen protection, add 0.5 mol 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18wt%) dropwise for 30 minutes. After the addition is completed, heat to 60°C and react for 18 hours. After post-treatment, an antioxidant is obtained.

[0030] The post-treatment steps involved in the above-mentioned Examples 1-3 are as follows: triethylamine and solvent are removed by reduced pressure distillation at 50°C to obtain a crude product 1; the crude product 1 is dissolved in 240ml of dichloromethane, washed twice with a 4.5wt% NaHCO3 aqueous solution (100ml each time), washed three times with 0.5M hydrochloric acid (80ml each time), and then washed twice with a saturated NaCl solution (100ml each time), and then distilled under reduced pressure at 50°C to obtain a crude product 2; the crude product 2 is dissolved in 200ml of anhydrous ethanol, and then 250ml of 1.75M sodium hydroxide solution is added to precipitate a solid, which is then washed with deionized water until neutral, and vacuum dried at 60°C for 10h to obtain a solid powder, which is an antioxidant.

[0031] Example 4

[0032] A polypropylene synthetic paper with UV resistance and anti-aging properties, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer has a raw material composition of 300 g polypropylene, 10 g titanium dioxide, 20 g antioxidant (prepared in Example 1), and 10 g calcium carbonate; the middle layer has a raw material composition of 400 g polypropylene, 10 g titanium dioxide, and 20 g antistatic agent (AS11N antistatic agent); and the inner layer has a raw material composition that is the same as that of the outer layer.

[0033] Example 5

[0034] A polypropylene synthetic paper with UV resistance and anti-aging properties, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer has a raw material composition of 350 g polypropylene, 15 g titanium dioxide, 25 g antioxidant (prepared in Example 2), and 25 g calcium carbonate; the middle layer has a raw material composition of 450 g polypropylene, 15 g titanium dioxide, and 25 g antistatic agent (Armostat 400 antistatic agent); and the inner layer has the same raw material composition as the outer layer.

[0035] Example 6

[0036] A polypropylene synthetic paper with UV resistance and anti-aging properties, with a thickness of 0.20 mm, an outer layer and an inner layer having a thickness of 0.06 mm, and a middle layer having a thickness of 0.08 mm; the outer layer is made of the following raw materials: 400 g of polypropylene, 20 g of titanium dioxide, 30 g of an antioxidant (prepared in Example 3), and 40 g of calcium carbonate; the middle layer is made of the following raw materials: 500 g of polypropylene, 20 g of titanium dioxide, and 30 g of an antistatic agent (Armostat 400 antistatic agent); and the inner layer has the same raw material composition as the outer layer.

[0037] Comparative Example 1

[0038] The preparation method of the UV-resistant and anti-aging polypropylene synthetic paper is substantially the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced by 25 g of 4,4'-diaminodiphenylamine.

[0039] Comparative Example 2

[0040] The preparation method of the UV-resistant and anti-aging polypropylene synthetic paper is basically the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced by 25 g of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride.

[0041] Comparative Example 3

[0042] The preparation method of the UV-resistant and anti-aging polypropylene synthetic paper is basically the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced by 19g of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and 7g of 4,4'-diaminodiphenylamine.

[0043] Comparative Example 4

[0044] The preparation method of the anti-ultraviolet and anti-aging polypropylene synthetic paper is basically the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced with 25 g of an antioxidant prepared by the following method:

[0045] 0.1 mol 4,4'-diaminodiphenylmethane is dissolved in 200 ml tetrahydrofuran, 0.48 mol triethylamine is added dropwise at 0-5°C, and under nitrogen protection, 0.4 mol 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18wt%) is added dropwise for 30 minutes. After the addition is completed, the temperature is raised to 55°C and reacted for 22 hours. The antioxidant is obtained through post-treatment.

[0046] Comparative Example 5

[0047] The preparation method of the anti-ultraviolet and anti-aging polypropylene synthetic paper is basically the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced with 25 g of an antioxidant prepared by the following method:

[0048] 0.1 mol 4,4'-diaminodiphenyl sulfone was dissolved in 200 ml tetrahydrofuran, 0.48 mol triethylamine was added dropwise at 0-5°C, and 0.4 mol 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18 wt%) was added dropwise under nitrogen protection for 30 minutes. After the addition was completed, the temperature was raised to 55°C and reacted for 22 hours. The antioxidant was obtained through post-treatment.

[0049] Comparative Example 6

[0050] The preparation method of the anti-ultraviolet and anti-aging polypropylene synthetic paper is basically the same as that of Example 5, except that the antioxidant (prepared in Example 2) is replaced with 25 g of an antioxidant prepared by the following method:

[0051] 0.1 mol of p-phenylenediamine was dissolved in 200 ml of tetrahydrofuran, and 0.48 mol of triethylamine was added dropwise at 0-5° C., and 0.4 mol of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride tetrahydrofuran solution (concentration 18 wt%) was added dropwise under nitrogen protection for 30 minutes. After the addition was completed, the temperature was raised to 55° C. and reacted for 22 hours. The antioxidant was obtained through post-treatment.

[0052] The post-treatment operation process of Comparative Examples 4-6 is the same as that of Example 2.

[0053] Comparative Example 7

[0054] A polypropylene synthetic paper with UV resistance and anti-aging properties, wherein the raw materials and proportions of the outer layer, the middle layer and the inner layer are the raw materials and proportions of Example 2 of the Chinese invention patent with publication number CN104943308A.

[0055] The UV-resistant and anti-aging polypropylene synthetic papers of Examples 4-6 and Comparative Examples 1-7 were prepared by the following process:

[0056] S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively;

[0057] S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming;

[0058] Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.

[0059] The brand of titanium dioxide used in the examples and comparative examples of the present application is DuPont R-706, the brand of calcium carbonate is KJ-106, and the polypropylene is CJS-700 homopolymer polypropylene produced by Sinopec.

[0060] The UV-resistant and anti-aging polypropylene synthetic papers prepared in Examples 4-6 and Comparative Examples 1-7 were subjected to UV aging tests, and the test method was carried out according to the method of GB / T 16422.3-2014 "Plastic Laboratory Light Source Exposure Test Method".

[0061] The anti-ultraviolet and anti-aging polypropylene synthetic papers prepared in Examples 4-6 of the present application and Comparative Examples 1-7 and the aged polypropylene synthetic papers were subjected to tensile strength tests according to the method of GB13022-91. The test results are shown in Table 1.

[0062] Table 1

[0063]

[0064] It can be seen from the data of Examples 4, 5 and 6 in Table 1 that the UV-resistant and anti-aging polypropylene synthetic paper prepared by the present invention has excellent transverse and longitudinal mechanical properties after aging, with a transverse tensile strength higher than 110 MPa and a longitudinal tensile strength higher than 65 MPa.

[0065] Comparative Examples 1, 2, and 3 are different from Example 5, and the difference is that the antioxidant (prepared in Example 2) is replaced by 4,4'-diaminodiphenylamine, 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride and 4,4'-diaminodiphenylamine. It can be seen from the data in Table 1 that after aging, the polypropylene synthetic paper prepared using the two antioxidants and the mixed antioxidants has a transverse tensile strength of less than 100 MPa and a longitudinal tensile strength of less than 52 MPa.

[0066] Comparative Examples 4-6 are different from Example 5, and the difference is that the antioxidant (prepared in Example 2) is replaced by 4,4'-diaminodiphenylmethane-modified 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, 4,4'-diaminodiphenyl sulfone-modified 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and p-phenylenediamine-modified 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride. It can be seen from the data in Table 1 that after aging, the polypropylene synthetic paper prepared using the antioxidants of Comparative Examples 4-6 has a transverse tensile strength of less than 103 MPa and a longitudinal tensile strength of less than 57 MPa.

[0067] Comparative Example 7 is a synthetic paper prepared using the raw materials and proportions in Example 2 of the Chinese invention patent publication number CN104943308A, and its longitudinal tensile strength after aging is less than 50 MPa.

[0068] In summary, it can be seen from the data of the comparative examples and embodiments in Table 1 that the anti-ultraviolet and anti-aging polypropylene synthetic paper prepared by the present invention has excellent transverse and longitudinal mechanical properties, and still maintains relatively good mechanical properties after aging. The reason why the polypropylene synthetic paper prepared by the present application has excellent antioxidant and anti-aging effects is that the antioxidant prepared by the present application undergoes an esterification reaction between 4,4'-diaminodiphenylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, and 4,4'-diaminodiphenylamine is grafted onto 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride, thereby increasing the molecular weight of the antioxidant (3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N-[4-({4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionylamino]phenyl}amino)phenyl]propionamide), improving the antioxidant's resistance to extraction and migration, and reducing the loss of the antioxidant. On the other hand, by grafting modification of 4,4'-diaminodiphenylamine, the conjugation effect of δ-π (N-benzene ring) is increased, and the hydrogen on the secondary amine is more likely to fall off to form free radicals, thereby increasing the activity of the antioxidant monomer. The shed hydrogen will quickly react with the free radicals and peroxy radicals on the carbon chain of polypropylene, causing it to lose its activity, thereby inhibiting the chain reaction process and thereby improving the anti-aging ability. The use of 4,4'-diaminodiphenylmethane or 4,4'-diaminodiphenyl sulfone grafting modification provides a higher molecular weight hindered phenol antioxidant with two hindered phenol units, which only improves the migration resistance of the antioxidant, but does not increase the activity of the antioxidant monomer to form free radicals. Therefore, the scheme of the present application has more excellent anti-aging performance.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. However, any equivalent changes, modifications and evolutions made by ordinary technicians in the field without departing from the scope of the technical solution of the present invention by using the technical content disclosed above are all equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

Claims

1. A polypropylene synthetic paper with UV resistance and anti-aging properties, comprising an outer layer, an intermediate layer and an inner layer, It is characterized in that The outer layer comprises the following raw materials in parts by weight: 30-40 parts of polypropylene, 1-2 parts of titanium dioxide, 2-3 parts of antioxidant, and 1-4 parts of calcium carbonate; The middle layer comprises the following raw materials in parts by weight: 40-50 parts of polypropylene, 1-2 parts of titanium dioxide, and 2-3 parts of antistatic agent; The raw materials and the number of portions of the inner surface layer are the same as those of the outer surface layer; The antioxidant is 3-(3,5-di-tert-butyl-4-hydroxyphenyl)-N-[4-({4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionylamino]phenyl}amino)phenyl]propionamide, which is prepared by acylation reaction of 4,4'-diaminodiphenylamine and 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride; The antioxidant is prepared by the following method: Dissolve 4,4'-diaminodiphenylamine in tetrahydrofuran, add triethylamine dropwise at 0-5°C, add a tetrahydrofuran solution of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride dropwise under nitrogen protection, raise the temperature to 50-60°C for reaction for 18-24h, and then post-treat to obtain the antioxidant; The molar ratio of 4,4'-diaminodiphenylamine to 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride is 1:(3-5); The molar ratio of 3,5-bis(tert-butyl)-4-hydroxyphenylpropionyl chloride to triethylamine is 1:(1-1.2).

2. The anti-ultraviolet and anti-aging polypropylene synthetic paper according to claim 1, It is characterized in that The antistatic agent is one of AS11N antistatic agent and Armostat 400 antistatic agent.

3. A method for preparing the UV-resistant and anti-aging polypropylene synthetic paper according to any one of claims 1 to 2, It is characterized in that The following steps are involved: S1: Extruding the outer layer raw material, the middle layer raw material and the inner layer raw material through an extruder respectively; S2: extruding each layer of raw materials extruded by the extruder through a T-type die, and then longitudinally stretching and transversely stretching, followed by cooling, corona treatment, and trimming; Among them, the extrusion temperature of the outer layer raw material and the inner layer raw material is 230°C, and the extrusion temperature of the middle layer raw material is 250°C; the preheating section temperature of longitudinal stretching is 130°C, the stretching section temperature is 142°C, the shaping section temperature is 145°C, the longitudinal stretching ratio is 4.9, the preheating section temperature of transverse stretching is 167°C, the stretching section temperature is 155°C, the shaping section temperature is 171°C, the transverse stretching ratio is 9 times, and the corona is 34.