A TOPCon battery and its preparation process
By adding a conductive passivation layer and burning through the insulating passivation layer to the N-TOPCon solar cell, problems such as bubbling during the traditional passivation process are solved, the stability and efficiency of the cell are improved, and higher photovoltaic performance is achieved. conversion efficiency.
Patent Information
- Application Number
- CN202410908386.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Traditional N-TOPCon solar cells are prone to blistering, pinhole films and other phenomena during the backside passivation process, resulting in incomplete passivation effects and affecting battery performance.
The process of adding a conductive passivation layer is adopted, which includes sequentially setting a back field layer, a conductive passivation layer and an insulating passivation layer on a single crystal substrate, and burning through the insulating passivation layer to contact the conductive layer without contacting the conductive layer. The back field layer contacts to form an N-N+-N++ gradient structure to enhance the field passivation effect of the interface layer.
It improves the passivation reliability and performance stability of the battery, enhances the interface carrier tunneling effect, and reduces the backside recombination rate, thus improving the open circuit voltage and photoelectric conversion efficiency of the battery.
Smart Images

Figure CN118448478B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells, and in particular relates to a TOPCon cell and a preparation process thereof. Background Art
[0002] At present, n-type tunneling oxide passivation contact (N-TOPCon) solar cells are one of the crystalline silicon solar cells with the highest photoelectric conversion efficiency on the market. Its theoretical limit photoelectric conversion efficiency is 28.7%, which is close to the limit photoelectric conversion efficiency of monocrystalline silicon solar cells (29.43%). From the perspective of industrial development, N-TOPCon cell technology has become the focus of market attention due to its unique cell structure and high photoelectric conversion efficiency. The main feature of tunneling oxide passivation is to first use a chemical method to prepare an ultra-thin silicon oxide layer on the back of the n-type silicon wafer, and then deposit a doped polysilicon layer. The two together form a passivation contact structure as the back passivation layer of the cell.
[0003] When the traditional method is used to passivate the back of the battery, the SiOx / poly-Si structure on the back of the battery will cause bubbles, pinhole films and other phenomena, resulting in the inability to achieve a comprehensive passivation effect using a single SiOx / poly-Si structure.
[0004] Therefore, in view of the above technical problems, it is necessary to provide a TOPCon battery and a preparation process thereof.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] The object of the present invention is to provide a TOPCon battery and a preparation process thereof, which can increase a conductive passivation layer to increase the passivation reliability and improve the stability of product performance.
[0007] In order to achieve the above object, a specific embodiment of the present invention provides a TOPCon cell, including a single crystal substrate;
[0008] A back field layer, a conductive passivation layer, an insulating passivation layer and an electrode are sequentially arranged on one side surface of the single crystal substrate;
[0009] The back field layer includes a tunneling oxide layer and a polysilicon layer sequentially arranged in a direction away from the single crystal substrate, and the conductive passivation layer includes a tunneling layer and a conductive layer sequentially arranged in a direction away from the single crystal substrate;
[0010] One end of the electrode burns through the insulating passivation layer and contacts the conductive passivation layer, but does not contact the back field layer;
[0011] The thickness of the polysilicon layer is 5-30 nm, and the thickness of the conductive layer is 30-50 nm.
[0012] In one or more embodiments of the present invention, one end of the electrode is burned through the insulating passivation layer and remains in the conductive layer.
[0013] In one or more embodiments of the present invention, one end of the electrode burns through the insulating passivation layer and completely penetrates the conductive layer to contact the surface of the tunnel layer on the side facing away from the single crystal substrate.
[0014] In one or more embodiments of the present invention, the tunneling layer is any one or more combinations of a titanium oxide film, a silicon oxide film or an aluminum oxide film.
[0015] In one or more embodiments of the present invention, the conductive layer is made of any one or more combinations of TCO glass, ITO conductive glass, AZO conductive glass, amorphous silicon or highly doped polysilicon.
[0016] In one or more embodiments of the present invention, the mass ratio of the doping element content to the silicon element content in the high-concentration doped polysilicon is (0.6-1):1.
[0017] In one or more embodiments of the present invention, the material of the polysilicon layer is any one or more combinations of amorphous silicon, intrinsic polysilicon or low-concentration doped polysilicon.
[0018] In one or more embodiments of the present invention, the mass ratio of the doping element content to the silicon element content in the low-concentration doped polysilicon is (0.3-0.5):1.
[0019] In one or more embodiments of the present invention, the insulating passivation layer includes a first insulating layer and a second insulating layer sequentially arranged in a direction away from the single crystal substrate;
[0020] The materials of the first insulating layer and the second insulating layer are any one or more combinations of silicon oxide, silicon nitride, silicon oxynitride or aluminum oxide.
[0021] In one or more embodiments of the present invention, a process for preparing a TOPCon battery comprises the following steps:
[0022] S1. preparing a doping layer on the front side of a single crystal substrate;
[0023] S2, forming a tunneling oxide layer on the back side of the single crystal substrate;
[0024] S3, depositing a low-concentration doped polysilicon layer / intrinsic polysilicon layer on the surface of the tunnel oxide layer;
[0025] S4, forming a tunneling layer in the entire surface area of the low-concentration doped polysilicon layer / intrinsic polysilicon layer;
[0026] S5, preparing a conductive layer on the surface of the tunneling layer;
[0027] S6, preparing an insulating passivation layer on the surface of the conductive layer;
[0028] S7. Form a front electrode on the surface of the doped layer by screen printing, and form a back electrode on the surface of the high-concentration doped polysilicon layer by screen printing, and then perform high-temperature sintering to ensure that one end of the back electrode remains in the high-concentration doped polysilicon layer.
[0029] Compared with the prior art, the TOPCon battery of the present invention adopts an additional conductive passivation layer to increase the passivation reliability and improve the stability of product performance;
[0030] The N-N+-N++ gradient structure is formed from the single crystal substrate to the upper conductive layer, which can further enhance the field passivation effect of the interface layer, and at the same time is conducive to enhancing the interface carrier tunneling and reducing the back recombination rate, thereby improving the open circuit voltage and conversion efficiency of the battery;
[0031] The electrode of the TOPCon battery structure burns through the insulating layer and contacts the conductive layer instead of directly contacting the rear surface field area of the back polysilicon layer. This not only increases the passivation effect of the battery cell, but also effectively avoids the failure of the tunneling effect caused by the electrode silver paste burning through the polysilicon layer and damaging the tunneling oxide layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 A schematic diagram of the structure of a TOPCon battery in one embodiment of the present invention Figure 1 ;
[0034] Figure 2 A schematic diagram of the structure of a TOPCon battery in one embodiment of the present invention Figure 2 ;
[0035] Figure 3 The figure is a flow chart of a preparation process of a TOPCon battery in one embodiment of the present invention.
[0036] Description of main reference numerals:
[0037] 1. Single crystal substrate; 2. Tunneling oxide layer; 3. Polysilicon layer; 4. Tunneling layer; 5. Conductive layer; 6. First insulating layer; 7. Second insulating layer; 8. Electrode. DETAILED DESCRIPTION
[0038] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0039] like Figure 1-Figure 2 As shown, a TOPCon cell in one embodiment of the present invention comprises a single crystal substrate 1, which is an N-type silicon substrate. A back field layer, a conductive passivation layer, an insulating passivation layer and an electrode 8 are sequentially arranged on one side surface of the single crystal substrate 1.
[0040] The back field layer includes a tunnel oxide layer 2 and a polysilicon layer 3 sequentially arranged in a direction away from the single crystal substrate 1. In this embodiment, the material of the tunnel oxide layer 2 can be silicon oxide but is not limited to silicon oxide; the thickness of the tunnel oxide layer 2 is 1-5 nm.
[0041] The material of the polysilicon layer 3 is any one or more combinations of amorphous silicon, intrinsic polysilicon or low-concentration doped polysilicon; the thickness of the polysilicon layer 3 is 5-30 nm.
[0042] Preferably, in the present embodiment, the material of the polysilicon layer 3 is preferably intrinsic polysilicon or low-concentration doped polysilicon. The advantage of using intrinsic polysilicon is that the diffusion doping process can be omitted, and the doping elements can be directly grown in situ, thereby reducing the number of processes and cutting costs. If low-concentration doped polysilicon is used, the content of the doping elements in the low-concentration doped polysilicon can be higher than the content of the doping elements in the single crystal substrate 1, so that a surface field passivation effect can be established between the two, thereby accelerating the selective absorption of electrons or holes in photogenerated carriers.
[0043] The conductive passivation layer includes a tunneling layer 4 and a conductive layer 5 which are sequentially arranged in a direction away from the single crystal substrate 1 .
[0044] The tunneling layer 4 is any one or more combinations of titanium oxide film, silicon oxide film or aluminum oxide film; the thickness of the tunneling layer 4 is 1-2 nm.
[0045] Preferably, in the present embodiment, the tunneling layer 4 is preferably a silicon oxide film, which can be formed by chemical vapor deposition of silicon oxide. Compared with intrinsic amorphous silicon, silicon oxide has a denser crystal structure and can provide a good interface barrier layer for atomic doping of intrinsic amorphous silicon, thereby blocking the diffusion movement of some doping elements and facilitating the formation of a gradient doping structure.
[0046] The conductive layer 5 is made of any one or more combinations of TCO glass, ITO conductive glass, AZO conductive glass, amorphous silicon or highly doped polysilicon; the thickness of the conductive layer 5 is 30-50 nm.
[0047] Preferably, in this embodiment, the material of the conductive layer 5 is preferably high-concentration doped polysilicon, and the content of doping elements in the high-concentration doped polysilicon should be higher than the content of doping elements in the low-concentration doped polysilicon to ensure conductivity.
[0048] Among them, the mass ratio of the doping element content to the silicon element content in the high-concentration doped polysilicon can be (0.6-1):1; the mass ratio of the doping element content to the silicon element content in the low-concentration doped polysilicon is (0.3-0.5):1.
[0049] Combined with actual production, an additional conductive passivation layer is adopted to increase the passivation reliability and improve the stability of product performance. In this structure, the bottom layer is an intrinsic polysilicon layer or a low-concentration doped polysilicon layer, and the upper layer is a high-concentration doped polysilicon layer. During the high-temperature annealing process in the post-process, the doping elements in the upper high-concentration doped polysilicon layer enter the underlying intrinsic polysilicon layer or the low-concentration doped polysilicon layer to achieve doping of the layer. Finally, an N-N+-N++ gradient structure is formed from the N-type silicon substrate to the high-concentration doped polysilicon layer, which can further enhance the field passivation effect of the interface layer, and at the same time is conducive to enhancing the interface carrier tunneling and reducing the back recombination rate, thereby improving the open circuit voltage and conversion efficiency of the battery, and achieving a gain effect on the efficiency of the TOPCon battery.
[0050] One end of the electrode 8 burns through the insulating passivation layer and contacts the conductive passivation layer, but does not contact the back field layer. Specifically, one end of the electrode 8 burns through the insulating passivation layer and remains in the conductive layer 5. The existing electrode 8 needs to burn through the conductive passivation layer to contact the back layer, which is easy to damage the tunneling oxide layer 2 and cause the tunneling effect to fail. By burning one end of the electrode 8 through the insulating passivation layer and leaving it in the newly added conductive layer 5, it is ensured that the electrode 8 does not directly contact the back field layer area, which can not only increase the passivation effect of the battery cell, but also effectively avoid the electrode silver paste burning through the polysilicon layer 3 and damaging the tunneling oxide layer 2, causing the tunneling effect to fail.
[0051] Furthermore, one end of the electrode 8 burns through the insulating passivation layer and completely penetrates the conductive layer 5 to contact the surface of the tunnel layer 4 facing away from the single crystal substrate 1. The tunnel layer 4 can prevent further sintering corrosion of the electrode 8, so that it can only reach the tunnel layer 4 and cannot go further. This is the optimal depth of electrode burn-through, which can maximize the contact area between the electrode 8 and the conductive layer 5, thereby reducing resistance and improving the efficiency of the TOPCon cell.
[0052] The insulating passivation layer comprises a first insulating layer 6 and a second insulating layer 7 which are arranged in sequence along a direction away from the single crystal substrate 1 .
[0053] The materials of the first insulating layer 6 and the second insulating layer 7 are any one or more combinations of silicon oxide, silicon nitride, silicon oxynitride or aluminum oxide.
[0054] Preferably, in this embodiment, the material of the first insulating layer 6 is preferably aluminum oxide, and the material of the second insulating layer 7 is preferably silicon nitride. The aluminum oxide layer and the silicon nitride layer can further enhance the passivation effect.
[0055] like Figure 3 As shown, a preparation process of a TOPCon battery includes the following steps:
[0056] S1, preparing a doping layer on the front side of the single crystal substrate 1: performing boron diffusion on the single crystal substrate 1 to prepare a doping layer on the front side of the single crystal substrate 1;
[0057] S2, forming a tunneling oxide layer 2 on the back side of the single crystal substrate 1: introducing a carrier gas containing oxygen into the chemical deposition chamber, and obtaining a tunneling silicon oxide layer 2 by thermal oxidation reaction between oxygen in the carrier gas and silicon atoms on the back side of the crystalline silicon;
[0058] S3, forming an intrinsic polysilicon layer by deposition on the surface of the tunnel oxide layer 2: introducing a silicon source gas and a mixture of a carrier gas and a silicon source gas into a chemical deposition chamber, and obtaining an intrinsic polysilicon layer by in-situ deposition of the silicon source gas on the surface of the tunnel oxide layer 2 under high temperature conditions;
[0059] S4, forming a tunneling layer 4 in the entire surface area of the low-concentration doped polysilicon layer / intrinsic polysilicon layer: introducing a carrier gas containing oxygen into the chemical deposition chamber, and the oxygen in the carrier gas undergoes an oxidation reaction with the intrinsic polysilicon to obtain the tunneling layer 4;
[0060] S5, preparing a conductive passivation layer on the surface of the tunneling layer: introducing a silicon source gas and a mixture of a carrier gas and a silicon source gas into a chemical deposition chamber, and depositing the silicon source gas in situ on the surface of the tunneling layer 4 under high temperature conditions to obtain a conductive layer;
[0061] S51. Introduce a doping element gas source and oxygen into the chemical deposition chamber to diffuse the doping element toward the single crystal substrate 1, and then diffuse into the conductive layer 5, the tunneling layer 4 and the polysilicon layer 3 in sequence, so that the conductive layer 5 becomes a high-concentration doped polysilicon layer, and the polysilicon layer 3 becomes a low-concentration doped polysilicon layer.
[0062] S6. preparing an insulating passivation layer on the surface of the conductive layer: depositing an aluminum oxide layer and a silicon nitride layer on the surface of the conductive layer in sequence;
[0063] S7, forming a front electrode on the surface of the doped layer by screen printing, forming a back electrode on the surface of the high-concentration doped polysilicon layer by screen printing, and then performing high-temperature sintering, and ensuring that one end of the back electrode remains in the high-concentration doped polysilicon layer;
[0064] S71 . During the high-temperature sintering process, the tunneling layer 4 will prevent the electrode 8 from further sintering and corrosion. At this time, it is only necessary to ensure that the electrode 8 burns through the conductive layer 5 and contacts the tunneling layer 4 .
[0065] The following is an explanation of the TOPCon battery preparation process in combination with the experimental process:
[0066] Experimental process:
[0067] Experimental group (double-layer passivation): all processes were kept at a constant temperature of 440°C;
[0068] Laughing gas was introduced into the chemical deposition chamber for 98 seconds at a pressure of 1800 mbar to form a first layer of silicon oxide;
[0069] Nitrogen was introduced for 29 seconds to flush out the residual nitrous oxide;
[0070] Vacuum for 15 seconds;
[0071] Nitrogen, hydrogen and phosphine are introduced for 200 seconds to form a phosphorus-doped polysilicon layer. At this time, the pressure is increased to 3300 mbar. The phosphine is removed and the pressure is continued for another 25 seconds to form a low-concentration phosphorus-doped polysilicon layer. The pressure in this process is 1500 mbar.
[0072] Laughing gas was introduced into the chemical deposition chamber again for 35 seconds at a pressure of 2200 mbar to form a second layer of silicon oxide;
[0073] Pass nitrogen gas for 20 seconds to flush out the residual laughing gas;
[0074] Vacuum for 15 seconds;
[0075] Nitrogen, hydrogen and phosphine were introduced for 200 seconds, and then the amount of phosphine was increased by 13.33% for 320 seconds. The process pressure was kept at 3300 mbar to form a high-concentration doped polysilicon layer.
[0076] After nitrogen is introduced for 20 seconds, vacuum is applied for 15 seconds;
[0077] During the masking process, silane and nitrous oxide were introduced for 70 seconds, and the pressure was maintained at 1750 mbar to form an insulating passivation protective layer;
[0078] Control group (single layer passivation):
[0079] Nitrogen was introduced into the chemical deposition chamber for 550 seconds at a temperature of 415°C to flush impurities on the surface of the silicon wafer.
[0080] Add laughing gas at 415°C for 185 seconds.
[0081] Nitrogen, hydrogen and phosphine were introduced for 195 seconds to form a phosphorus-doped polysilicon layer. Then, the hydrogen flow rate was reduced by 15.72% and the phosphine flow rate was increased by 21.51% for 185 seconds to form a phosphorus-doped polysilicon layer.
[0082] During the masking process, silane and nitrous oxide were introduced for 120 seconds, and the pressure was maintained at 1750 bar to form an insulating passivation protective layer.
[0083] Experimental results: After the test, it was found that the efficiency of the double-layer passivation layer and the single-layer passivation layer was basically the same, 25.301 and 25.317 respectively; but the airflow print was significantly reduced, from 28.41% to 3.15%. The experimental group is the newly invented process, and the comparison group is the original process. The original process makes the metal electrode directly contact with the back field layer on the basis of forming a tunneling oxide layer, which is prone to bubbling, burning through and other phenomena. The existing process adds a conductive passivation layer to prevent the metal electrode from directly contacting the back field layer, effectively avoiding the electrode silver paste from burning through the phosphorus-doped polysilicon layer and damaging the tunneling layer, resulting in the failure of the tunneling effect.
[0084] Compared with the prior art, the TOPCon battery of the present invention adopts an additional conductive passivation layer to increase the passivation reliability and improve the stability of product performance;
[0085] The N-N+-N++ gradient structure is formed from the single crystal substrate to the upper conductive layer, which can further enhance the field passivation effect of the interface layer, and at the same time is conducive to enhancing the interface carrier tunneling and reducing the back recombination rate, thereby improving the open circuit voltage and conversion efficiency of the battery;
[0086] The electrode of the TOPCon battery structure burns through the insulating layer and contacts the conductive layer instead of directly contacting the rear surface field area of the back polysilicon layer. This not only increases the passivation effect of the battery cell, but also effectively avoids the failure of the tunneling effect caused by the electrode silver paste burning through the polysilicon layer and damaging the tunneling oxide layer.
[0087] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0088] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A TOPCon battery, characterized in that: include: A single crystal substrate, wherein a back field layer, a conductive passivation layer, an insulating passivation layer and an electrode are sequentially arranged on one side surface of the single crystal substrate; The back field layer includes a tunneling oxide layer and a polysilicon layer sequentially arranged in a direction away from the single crystal substrate, and the conductive passivation layer includes a tunneling layer and a conductive layer sequentially arranged in a direction away from the single crystal substrate; One end of the electrode burns through the insulating passivation layer and contacts the conductive passivation layer, but does not contact the back field layer; The thickness of the polysilicon layer is 5-30nm, and the thickness of the conductive layer is 30-50nm; One end of the electrode burns through the insulating passivation layer and completely penetrates the conductive layer to contact the surface of the tunneling layer on a side away from the single crystal substrate; The conductive layer is made of any one or more combinations of TCO glass, ITO conductive glass, AZO conductive glass, amorphous silicon or highly doped polysilicon; The mass ratio of the doping element content to the silicon element content in the high-concentration doped polysilicon is (0.6-1):1; The material of the polysilicon layer is any one or more combinations of amorphous silicon, intrinsic polysilicon or low-concentration doped polysilicon; The mass ratio of the doping element content to the silicon element content in the low-concentration doped polysilicon is (0.3-0.5):
1.
2. A TOPCon battery according to claim 1, characterized in that: One end of the electrode is burned through the insulating passivation layer and remains in the conductive layer.
3. A TOPCon battery according to claim 1, characterized in that: The tunneling layer is any one or more combinations of a titanium oxide film, a silicon oxide film or an aluminum oxide film.
4. A TOPCon battery according to claim 1, characterized in that: The insulating passivation layer comprises a first insulating layer and a second insulating layer which are sequentially arranged in a direction away from the single crystal substrate; The materials of the first insulating layer and the second insulating layer are any one or more combinations of silicon oxide, silicon nitride, silicon oxynitride or aluminum oxide.
5. A process for preparing a TOPCon battery, for preparing a TOPCon battery as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: S1, preparing a doping layer on the front side of the single crystal substrate; S2, forming a tunneling oxide layer on the back side of the single crystal substrate; S3, depositing a low-concentration doped polysilicon layer / intrinsic polysilicon layer on the surface of the tunnel oxide layer; S4, forming a tunneling layer in the entire surface area of the low-concentration doped polysilicon layer / intrinsic polysilicon layer; S5, preparing a conductive layer on the surface of the tunneling layer; S6, preparing an insulating passivation layer on the surface of the conductive layer; S7. Form a front electrode on the surface of the doped layer by screen printing, and form a back electrode on the surface of the high-concentration doped polysilicon layer by screen printing, and then perform high-temperature sintering to ensure that one end of the back electrode remains in the high-concentration doped polysilicon layer.