Device and production process for preparing boron nitride nanotubes based on plasma method
By combining high-energy ball milling and powder screening, the problems of low yield and high cost of boron nitride nanotube preparation are solved, and efficient and low-cost nanotube preparation is achieved, with morphological control capabilities and suitable for commercial production. .
Patent Information
- Application Number
- CN202410931747.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-12
AI Technical Summary
The existing preparation methods for boron nitride nanotubes (BNNTs) have problems such as low yield, high cost, many product impurities and difficult morphology control, especially the efficiency of ball mill annealing method and high temperature thermal plasma method in large-scale production. and insufficient economicality.
Using a plasma method-based device and process, the particle size and distribution of precursors are regulated through high-energy ball milling and powder screening strategies, and the conversion rate and energy consumption efficiency of chemical reactions are improved. Combined with the induction plasma module to generate high temperature flame feathers, achieving high BNNTs Production and high purity preparation.
It significantly improves the yield and purity of BNNTs, reduces energy consumption and production costs, realizes control of morphological characteristics, is suitable for semi-continuous production, and promotes the commercial application of nanotubes.
Smart Images

Figure CN118458708B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new materials and preparation methods thereof, in particular to a device and a production process for preparing boron nitride nanotubes based on a plasma method. Background Art
[0002] Boron nitride nanotubes have unique physical and chemical properties, including excellent thermal conductivity, good mechanical properties and outstanding thermal stability. In recent years, people have done a lot of theoretical research and experimental demonstration on its application potential in different fields. Generally, different application scenarios have different requirements for the quality of BNNTs (boron nitride nanotubes). Since the properties of BNNTs are closely related to their microstructure (including length, diameter, number of tube walls, crystallinity, etc.) and impurity content, in order to further explore its commercial value, how to establish a set of BNNTs that can be prepared with high yield, high purity and controllable morphology is the core problem that needs to be solved at present. According to the reaction temperature, the mainstream preparation methods of BNNTs can be divided into two categories: (1) low-temperature reaction method (including ball milling annealing method, chemical vapor deposition (CVD) and physical vapor deposition (PVD)), (2) high-temperature reaction method (including laser ablation, arc discharge method and thermal plasma method). In low-temperature reactions, the ball milling annealing method is a high-yield and relatively low-cost synthetic route, which generally includes two independent steps, namely high-energy mechanical ball milling and thermal annealing. High-energy ball milling can not only reduce the particle size, but more importantly, the process can change the molecular structure of solid boron source materials (such as elemental boron, boron nitride and boron oxide) through chemical reactions at room temperature. The prepared precursor can be generated after thermal annealing to obtain BNNTs. In high-temperature reactions, although laser ablation technology can produce high-crystallinity BNNTs, its production efficiency is limited (the output per hour is only in the order of milligrams). In comparison, in the reaction system based on the high-temperature thermal plasma method, the plasma generated by two concentric electrodes can provide a large amount of thermal energy in a larger volume, thereby constructing a larger space suitable for the growth of BNNTs (the inner diameter of a typical reactor is 15 cm, and the length covered by the effective growth temperature is greater than 30 cm). Therefore, ball milling annealing and thermal plasma methods have developed into effective means for large-scale production of BNNTs.
[0003] Although the ball milling annealing method and the thermal plasma method have met the production needs to a certain extent, the above two methods still have many shortcomings. The main problems of the ball milling annealing method are as follows: (1) The BNNTs prepared by this method usually have a bamboo structure (the content of cylindrical BNNTs in the product is low); (2) This method cannot take into account both yield and purity (when the catalyst dosage is low, the catalytic efficiency is not ideal; when the catalyst dosage is high, the content in the product increases rapidly). The main problems of the high-temperature thermal plasma method are as follows: (1) The reaction efficiency will be reduced due to the instability of the plasma flame plume (the reasons for this phenomenon include the interference of the material with the plasma gas flow characteristics, pressure fluctuations under positive or negative pressure reaction conditions, etc.); (2) The production cost is high. During the reaction process, the amount of material used is large, such as the total gas flow rate of the reaction gas and the carrier gas is generally greater than 100 standard liters per minute; if a mixed plasma gas is used, it will also increase the additional equipment operation and maintenance costs and system complexity; the equipment energy consumption is high, and the power required to maintain the plasma flame plume is generally greater than 30 kilowatts; the equipment cost is high and the initial investment is large. Summary of the invention
[0004] In order to overcome the disadvantages of the methods for producing BNNTs by low-temperature reaction and high-temperature reaction in the prior art due to technical limitations as described in the background technology, the present invention provides a device and production process for preparing boron nitride nanotubes based on plasma method, which can effectively control the particle size and distribution of precursor powder through high-energy ball milling and powder screening strategies under the joint action of relevant mechanisms, thereby improving the chemical reaction conversion rate and energy consumption efficiency of raw materials, and effectively controlling the microscopic morphology and uniformity of BNNTs products while improving the purity of BNNTs products by reducing the particle size distribution of precursor ultrafine powders, and improving the energy utilization efficiency of thermal plasma reactors by lowering the boiling point of precursor ultrafine powders, effectively improving the utilization rate of energy and materials, and realizing semi-continuous production, which provides strong technical support for promoting the relevant research and application of BNNTs.
[0005] The technical solution adopted by the present invention to solve the technical problem is:
[0006] The device for preparing boron nitride nanotubes based on plasma method is characterized in that it includes a precursor pretreatment module, a feeding module, an induction plasma module, a reaction chamber module, a connection module, a collection and filtration module, a pressure control module, a cooling system centralized control module, an electric and gas centralized control module, a gas supply module and a rack and platform module; the precursor pretreatment module, the feeding module, the induction plasma module, the reaction chamber module, the connection module, the collection and filtration module, the pressure control module, the cooling system centralized control module, the electric and gas centralized control module, and the gas supply module are installed on the rack and platform module, and the electric and gas centralized control module controls the power output end and the precursor pretreatment module, the feeding module, the induction plasma module, the reaction chamber module, the connection module, the collection and filtration module, the pressure control module, the cooling system centralized control module, and the gas supply module. The control signal input end of the gas supply module is electrically connected respectively; the gas output end of the gas supply module and the precursor pretreatment module, the feeding module , the gas input ends of the induction plasma module, the reaction chamber module, the connection module, and the collection and filtration module are respectively connected through pipelines; the signal input end of the cooling system centralized control module is electrically connected to the signal output ends of the induction plasma module, the reaction chamber module, and the connection module; the signal input end of the pressure control module is electrically connected to the pressure signal output ends of the pressure sensor installed in the feeding module, the reaction chamber module, the connection module, and the collection and filtration module; the precursor pretreatment module is a high-energy ball milling device, the discharge pipe of the high-energy ball mill is connected to the feed pipe of the powder raw material storage device of the feeding module, the discharge pipe of the second-stage cyclone separator of the powder raw material storage device is connected to the ultrafine powder feed port of the reaction chamber module, the induction plasma nozzle of the induction plasma module is connected to the premixing cavity of the reaction chamber module, the outlet connecting component of the reaction chamber module is connected to the inlet connecting port of the connection module, and the outlet connecting port of the connection module is connected to the inlet connecting port of the collection and filtration module.
[0007] Furthermore, the feeding module includes a powder raw material storage device, a first-stage cyclone separator, a powder feeding switch, a compressed gas supply control device, and a second-stage cyclone separator. A screw feeder is installed in the powder raw material storage device. The discharge pipe of the screw feeder is connected to the upper feed pipe of the first-stage cyclone separator, the lower return pipe at the lower end of the first-stage cyclone separator is connected to the right return pipe at the right end of the powder raw material storage device, the discharge pipe of the first-stage cyclone separator is connected to the lower feed pipe of the powder feeding switch, the upper discharge pipe of the powder feeding switch is connected in parallel with the right exhaust pipe of the compressed gas supply control device and the upper feed pipe on the left side of the second-stage cyclone separator, the lower return pipe at the lower end of the second-stage cyclone separator is connected to the upper return pipe on the right side of the upper end of the first-stage cyclone separator, and the left air inlet pipe of the compressed gas supply control device is connected to one of the gas output ends of the gas output end of the air supply module.
[0008] Furthermore, the induction plasma module includes an induction plasma control cabinet, an ignition cavity, a matrix tube combination, an induction coil, a gas inlet A, a gas inlet B, an induction plasma nozzle, a coolant inlet, and a coolant outlet. The signal output end of the induction plasma control cabinet is electrically connected to the induction coil, the electric valves of the gas inlet A and the gas inlet B, and the coolant inlet and the coolant outlet. The outer ends of the gas inlet A, the gas inlet B, and the coolant inlet are respectively connected to the gas output end and the other three gas output ends of the gas supply module. The matrix tube combination is installed at the inner end of the ignition cavity, and the induction coil is installed at the outer end of the ignition cavity.
[0009] Furthermore, the reaction chamber module includes a premixing cavity, an ultrafine powder feed port, a powder distribution pipe, a coolant inlet, a coolant outlet, an inlet section reaction cavity, a connecting section reaction cavity, an outlet section reaction cavity, and an outlet connecting component. The lower end of the premixing cavity and the upper end of the inlet section reaction cavity are installed together via the inlet connecting component. The upper end of the connecting section reaction cavity is connected to the lower end of the inlet section reaction cavity, the lower end of the connecting section reaction cavity is connected to the upper end of the outlet section reaction cavity, the upper end of the outlet connecting component is installed at the lower end of the outlet section reaction cavity, the left side of the ultrafine powder feed port is installed at the right end of the powder distribution pipe, the powder distribution pipe is installed at the upper end of the premixing cavity, the coolant outlet and the coolant inlet are respectively installed on the left and right sides of the premixing cavity, and the inlet section insulation layer is installed on the left outer side of the inlet section reaction cavity. , and an inlet section thermocouple is installed outside the right end, an inlet section coolant inlet and an inlet section coolant outlet are respectively installed at the lower right end and the upper left end of the inlet section reaction cavity, a connecting section coolant inlet and a connecting section coolant outlet are respectively installed at the lower right end and the upper left end of the connecting section reaction cavity, a connecting section thermocouple is installed at the upper right end of the connecting section reaction cavity, an outlet section coolant inlet and an outlet section coolant outlet are respectively installed at the lower right end and the upper left end of the outlet section reaction cavity, an outlet section thermocouple is installed at the upper right end of the outlet section reaction cavity, an outlet section insulation layer is installed outside the outlet section reaction cavity, the gas output ends of the three coolant inlet gas supply modules are connected to the fifth, sixth and seventh gas output ends, and the three thermocouples are electrically connected to the three temperature collection ports of the electric and gas centralized control module.
[0010] Furthermore, the connection module includes an inlet connection plate, an observation window, a pressure gauge, a thermometer, a pressure transmitter, a safety valve, an outlet connection plate, and a pipeline. The inlet connection plate is installed at the upper end of the pipeline, the observation window is installed at the upper left end of the pipeline, the pressure gauge and the thermometer are respectively installed at the front and right sides of the upper end of the pipeline, the pressure transmitter is installed in the middle of the upper end of the pipeline, the safety valve is installed at the front side of the rear end of the pipeline, the outlet connection plate is installed at the lower right end of the pipeline, the middle and upper parts of the lower left end of the pipeline are respectively installed with a front coolant inlet and a front coolant outlet, and the lower part and the middle of the upper right end of the pipeline are respectively installed with a rear end coolant inlet and a rear end coolant outlet; the gas output ends of the two coolant inlet air supply modules are respectively connected to the eighth and ninth gas output ends.
[0011] Furthermore, the collection and filtration module includes an inlet connecting plate, a filter tank, a filter cartridge, an outlet connecting plate, a filter bag tank connecting pipe, a filter bag tank, a filter bag, a filter bag tank connecting pipe, an air tank, a regulating valve a, a regulating valve b, and an exhaust gas discharge port. The right end of the inlet connecting plate is installed at the left end of the filter tank, the filter cartridge is installed in the filter tank, and operation ports are respectively provided at both ends of the front side of the filter tank. The filter tank has a window and a sampling port at the lower end of the filter cartridge, and the lower end of the outlet connecting plate is installed at the upper end of the filter tank. Both sides of the filter bag tank connecting pipe are respectively installed with the upper end of the outlet connecting plate and the middle of the left end of the filter bag tank. The filter bag is installed in the filter bag tank, and an ash removal tray is provided at the lower front end opening of the filter bag tank. A filter bag tank window is provided on the front side of the filter bag tank at the lower end of the filter bag. The filter bag tank connecting pipe is installed in series with the upper left end of the air tank through the air inlet and exhaust port of the regulating valve a, and the lower right end of the air tank is installed in series with the left end of the exhaust gas discharge port of the air tank through the air inlet and exhaust port of the regulating valve b.
[0012] The production process of the device for preparing boron nitride nanotubes based on the plasma method is characterized in that it includes the following processes: S1: the precursor pretreatment module processes the solid raw material particles, and the particle size thereof is reduced, and enters the feeding module; S2: the feeding module obtains ultrafine powder with a narrow particle size distribution by screening the raw material, and uses it as a precursor for preparing BNNTs; S3: the induction plasma module generates a plasma flame plume to provide a high-temperature heat source for the synthesis reaction; S4: under the action of high temperature, the ultrafine powder of the BNNTs precursor is vaporized in the reaction chamber module, and combined with the gaseous nitrogen source, and after cooling, BNNTs are generated and enter the connection module; S5: the product obtained in step S4 is cooled in the connection module and collected in the collection and filtration module.
[0013] Furthermore, the function of the pressure control module is to monitor and regulate the pressure in the feed module, reaction chamber module, connection module and collection and filtration module, thereby affecting the dispersion level of the material, the synthesis reaction conditions and the collection efficiency of the product.
[0014] Furthermore, in the step S1, the solid raw material particles are pure amorphous elemental boron powder or a multi-component mixture thereof with a catalyst compound.
[0015] Furthermore, in step S2, the volume of the powder charged at one time accounts for 50-75% of the storage volume in the raw material storage device, and the feeding speed of the screw feeder is controlled at 10-30 ml / min; the number of first-stage cyclone separators can be adjusted according to actual conditions, and the total number of cyclone separators involved in the system is not less than 2; the compressed gas is a mixed gas of one or more of argon, nitrogen, and ammonia, and the flow rate is 10-30 liters / min.
[0016] Compared with the prior art, the present invention has the following beneficial effects: (1) The present invention can rapidly gasify the boron-containing raw material and efficiently mix it with the nitrogen source, thereby significantly increasing the output per unit time. On the other hand, it can significantly increase the chemical reaction activity of the precursor, thereby optimizing the conversion rate of the raw material; (2) The narrower particle size distribution is conducive to the preparation of BNNTs products with similar morphological characteristics. When smaller-sized particles are used as precursors, their boiling point is significantly reduced, which is more conducive to their rapid gasification and full mixing with the nitrogen source under the action of high-temperature thermal plasma, thereby effectively reducing the impurity content in the product and improving the energy utilization efficiency of the high-temperature process at the same time, which is more in line with the concept of green production; (3) The production system involves multiple adjustable variables, which facilitates the effective regulation of the structural characteristics of the BNNTs product; (4) The synthetic process involved in the production is suitable for semi-continuous production. During the process, all solid substances are transported in each module by a screw extruder and a carrier gas. In addition, after the high-temperature plasma reactor component is expanded, it has the ability to realize semi-continuous large-scale production of BNNTs. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The figure is a schematic diagram of the overall modularization of the device for preparing boron nitride nanotubes by a high-temperature thermal plasma method based on a highly active ultrafine powder precursor according to the present invention.
[0018] Figure 2 Schematic diagram of the layout of the components of the feed module.
[0019] Figure 3 Schematic diagram of the layout of the components of the inductive plasma module.
[0020] Figure 4 Schematic diagram of the layout of the components of the reaction chamber module.
[0021] Figure 5 This is a schematic diagram of the layout of the components of the connection module.
[0022] Figure 6 This is a schematic diagram of the layout of the components of the collection and filtration module.
[0023] Figure 7 This is a SEM image of the raw material amorphous elemental boron powder before high-energy ball milling in Example 1 of the present invention (scale: 2 microns).
[0024] Figure 8 This is a SEM image of the raw material amorphous elemental boron powder after high-energy ball milling in Example 1 of the present invention (scale: 2 microns).
[0025] Fig. 9 This is a particle size distribution diagram of the powder after particle size screening in Example 1 of the present invention.
[0026] Fig.10 This is the XPS graph of the precursor ultrafine powder in Example 1 of the present invention.
[0027] Fig.11 This is a SEM image of the BNNTs prepared in Example 1 of the present invention (scale: 30 μm).
[0028] Fig.12 This is a TEM image of BNNTs prepared in Example 1 of the present invention.
[0029] Fig.13 This is the XPS graph of the precursor ultrafine powder in Example 2 of the present invention.
[0030] Fig.14 TEM image of BNNTs prepared in Example 3 of the present invention 。 DETAILED DESCRIPTION
[0031] Figure 1 , 2, 3, 4, 5, and 6, a device for preparing boron nitride nanotubes based on a plasma method comprises a precursor pretreatment module 1, a feed module 2, an induction plasma module 3, a reaction chamber module 4, a connection module 5, a collection and filtration module 6, a pressure control module 7, a cooling system centralized control module 8, an electric and gas centralized control module 9, a gas supply module 10, and a rack and platform module 11; the precursor pretreatment module 1, the feed module 2, the induction plasma module 3, the reaction chamber module 4, the connection module 5, the collection and filtration module 6, the pressure control module 7, the cooling system centralized control module 8, the electric and gas centralized control module 9, the gas supply module 10, and the rack and platform module 11. The cooling system centralized control module 8, the electricity and gas centralized control module 9, and the gas supply module 10 are installed on the rack and platform module 11, and the electricity and gas centralized control module 9 controls the power output end and the precursor pretreatment module 1, the feeding module 2, the induction plasma module 3, the reaction chamber module 4, the connection module 5, the collection and filtration module 6, the pressure control module 7, the cooling system centralized control module 8, and the signal input end of the gas supply module 10 are respectively connected via wires; the gas output end of the gas supply module and the precursor pretreatment module 1, the feeding module 2, the induction plasma module 3, The gas input ends of the reaction chamber module 4, the connection module 5, and the collection and filtration module 6 are connected via pipelines respectively; the signal input end of the cooling system centralized control module 8 and the signal output ends of the induction plasma module 3, the reaction chamber module 4, and the connection module 5 are connected via wires respectively; the signal input end of the pressure control module and the pressure signal output end of the pressure sensor installed in the feeding module, the reaction chamber module, the connection module, and the collection and filtration module are connected via wires respectively; the precursor pretreatment module 1 is a high-energy ball milling device, and the discharge pipe of the high-energy ball mill and the powder of the feeding module 2 The left side of the feed pipe of the final raw material storage device 21 is connected via a pipeline, the right side of the discharge pipe of the second-stage cyclone separator 25 of the feed module 2 and the right side of the ultrafine powder feed port 42 of the reaction chamber module 4 are connected via a pipeline, the lower side of the induction plasma nozzle 37 of the induction plasma module 3 and the upper side of the premixing cavity 41 of the reaction chamber module 4 are connected via a pipeline, the outlet connecting component 422 of the reaction chamber module 4 and the upper side of the inlet connecting plate 51 of the connecting module 5 are connected via a pipeline, and the outlet connecting plate 511 of the connecting module 5 and the inlet connecting plate A61 of the collecting and filtering module 6 are connected via a pipeline.
[0032] Figure 1 , 2, 3, 4, 5, and 6, the feeding module 2 includes a powder raw material storage device 21, a first-stage cyclone separator 22, a powder feeding switch 23, a compressed gas supply control device 24, and a second-stage cyclone separator 25. A screw feeder is installed in the powder raw material storage device 21, and the discharge pipe of the screw feeder and the upper feed pipe of the first-stage cyclone separator 22 are connected via a pipeline. The lower return pipe at the lower end of the first-stage cyclone separator 22 and the right return pipe at the right end of the powder raw material storage device 21 are connected via a pipeline. The discharge pipe of the device 22 and the lower feed pipe of the powder feed switch 23 are connected via a pipeline, the upper discharge pipe of the powder feed switch 23 and the right exhaust pipe of the compressed gas supply control device 24 and the upper feed pipe on the left side of the second-stage cyclone separator 25 are connected in parallel via pipelines, the lower return pipe at the lower end of the second-stage cyclone separator 25 and the upper return pipe on the right side of the upper end of the first-stage cyclone separator 22 are connected via pipelines, and the left air inlet pipe of the compressed gas supply control device 24 and one of the gas output ends of the gas supply module are connected via pipelines. The induction plasma module 3 includes an induction plasma control cabinet 31, an ignition cavity 32, a rectangular tube assembly 33, an induction coil 34, a gas inlet A35 (carrier gas, auxiliary gas), a gas inlet B36 (cooling gas), an induction plasma nozzle 37, a coolant inlet 38, and a coolant outlet 39. The signal output end of the induction plasma control cabinet 31 and the electric valves of the induction coil 34, the gas inlet A35 and the gas inlet B36, and the electric valve signal input ends of the coolant inlet 38 and the coolant outlet 39 are respectively connected through wires, and the outer ends of the gas inlet A35, the gas inlet B36, and the coolant inlet 38 are respectively connected to the gas output end and the other three gas output ends of the gas supply module through pipelines. The rectangular tube assembly 33 is installed at the inner end of the ignition cavity 32, and the induction coil 34 is installed at the outer end of the ignition cavity 32.The reaction chamber module 4 includes a premixing chamber 41, an ultrafine powder feed port 42, a powder distribution pipe 43, a coolant inlet A44, a coolant outlet A45, an inlet section reaction chamber 47, a connecting section reaction chamber 412, an outlet section reaction chamber 417, and an outlet connecting component 422. The lower end of the premixing chamber 41 and the upper end of the inlet section reaction chamber 47 are installed together via an inlet connecting component 46. The upper end of the connecting section reaction chamber 412 is connected to the lower end of the inlet section reaction chamber 47, the lower end of the connecting section reaction chamber 412 is connected to the upper end of the outlet section reaction chamber 417, the upper end of the outlet connecting component 422 is installed at the lower end of the outlet section reaction chamber 417, the left side of the ultrafine powder feed port 42 is installed at the right end of the powder distribution pipe 43, the powder distribution pipe 43 is installed at the upper end of the premixing chamber 41, the left and right sides of the premixing chamber 41 are respectively installed with a coolant outlet A45 and a coolant inlet A44, the left outer side of the inlet section reaction chamber 47 is installed with an inlet section The insulation layer 48 is provided, and an inlet section thermocouple 49 is installed outside the right end. The inlet section reaction cavity 47 is provided with an inlet section coolant inlet 410 and an inlet section coolant outlet 411 at the lower right end and the upper left end, respectively. The connecting section reaction cavity 412 is provided with a connecting section coolant inlet 415 and a connecting section coolant outlet 416 at the lower right end and the upper left end, respectively. A connecting section thermocouple 414 is installed at the upper right end of the connecting section reaction cavity 412. An outlet section coolant inlet 420 and an outlet section coolant outlet 421 are installed at the lower right end and the upper left end of the outlet section reaction cavity 417, respectively. An outlet section thermocouple 419 is installed at the upper right end of the outlet section reaction cavity 417. An outlet section insulation layer 418 is provided outside the outlet section reaction cavity 417. The three coolant inlets and the fifth, sixth and seventh gas output ends of the gas output end of the gas supply module are connected via pipelines, respectively. The three thermocouples and the three temperature collection ports of the electric and gas centralized control module 9 are connected via wires, respectively. The connection module 5 includes an inlet connection plate 51, an observation window 52, a pressure gauge 53, a thermometer 54, a pressure transmitter 55 (pressure sensor), a safety valve 56, an outlet connection plate 511, and a pipeline. The inlet connection plate 51 is installed at the upper end of the pipeline, the observation window 52 is installed at the upper left end of the pipeline, the pressure gauge 53 and the thermometer 54 are installed at the front and right sides of the upper end of the pipeline respectively, the pressure transmitter 55 is installed at the middle of the upper end of the pipeline, the safety valve 56 is installed at the front side of the rear end of the pipeline, the outlet connection plate 511 is installed at the lower right end of the pipeline, the middle and upper parts of the lower left end of the pipeline are respectively installed with a front coolant inlet 57 and a front coolant outlet 58, and the lower right end and the middle of the upper side of the pipeline are respectively installed with a rear coolant inlet 59 and a rear coolant outlet 510; the eighth and ninth gas output ends of the two coolant inlet air supply modules are respectively connected through pipelines.The collection and filtration module includes an inlet connecting plate A61, a filter tank 62, a filter cartridge 65, an outlet connecting plate A66, a filter bag tank connecting pipe 67, a filter bag tank 68, a filter bag 610, a filter bag tank connecting pipe A612, an air storage tank 614, a regulating valve a613, a regulating valve b615, and an exhaust gas discharge port 616. The right end of the inlet connecting plate A61 is installed on the left end of the filter tank 62, the filter cartridge 65 is installed in the filter tank 62, and the two ends of the front side of the filter tank 62 are respectively provided with operation ports 64. The filter tank 62 has a viewing window and a sampling port 63 at the lower end of the filter cartridge 65. The lower end of the outlet connecting plate A66 is installed on the filter tank 62 upper end, both sides of the filter bag tank connecting pipe 67 are respectively installed with the upper end of the outlet connecting plate A66 and the middle of the left end of the filter bag tank 68, the filter bag 610 is installed in the filter bag tank 68, and the filter bag tank 68 has an ash tray 611 at the lower front end opening, and the filter bag 610 has a filter bag tank window 69 on the front side of the filter bag tank 68 at the lower end position of the filter bag 610, and the filter bag tank connecting pipe A612 is installed with the upper left end of the gas tank 614 in series through the air inlet and exhaust port of the regulating valve a613, and the lower right end of the gas tank 614 is installed with the left end of the exhaust outlet 616 of the gas tank 614 in series through the air inlet and exhaust port of the regulating valve b615.
[0033] Figure 1 , 2 , 3, 4, 5, and 6, the production process of the device for preparing boron nitride nanotubes based on the plasma method includes the following steps: Step 1: After high-energy ball milling (precursor pretreatment module 1), the particle size of the solid raw material particles is reduced. Step 2: After the raw material obtained in step 1 is subjected to particle size screening treatment by the feed module 2, an ultrafine powder with a narrow particle size distribution is obtained, which is used as a precursor for preparing BNNTs. Step 3: The induction plasma module 3 generates a plasma flame plume to provide a high-temperature heat source for the synthesis reaction. Step 4: Under the action of high temperature, the precursor ultrafine powder is vaporized in the reaction chamber module 4, combined with the gaseous nitrogen source, and cooled to generate BNNTs. Step 5: After the product of step 3 is further cooled by the connection module 5, it is subsequently collected in the collection and filtration module 6. The function of the pressure control module 7 is to monitor and / or regulate the pressure inside the feed module 2, the reaction chamber module 4, the connection module 5 and the collection and filtration module 6, thereby affecting the dispersion level of the material, the synthesis reaction conditions and the collection efficiency of the product; the cooling system centralized control module 8 is used to monitor and / or adjust the flow rate of different types of coolants in the induction plasma module 3, the reaction chamber module 4, and the connection module 5, which is used to protect the reliability of structural components during high-temperature reactions, adjust the quenching rate of boron-nitrogen intermediate compounds, and further cool the product BNNTs for unified collection; the electricity and gas centralized control module 9 and the gas supply module 10 are used to supply power and gas to the entire reaction system.
[0034] Figure 1 , 2As shown in Figures 3, 4, 5, and 6, in step 1, the boron source solid powder raw material is pretreated by high-energy ball milling, which includes the following steps: (1) preparing a solid powder raw material (i.e., high-purity amorphous elemental boron powder or a multi-component mixture thereof with a catalyst compound); (2) placing ball mill beads, powder, and liquid grinding aid into a ball mill jar, constructing an atmosphere combination required for the ball milling process in the jar and adjusting the initial pressure in the jar (i.e., filling the jar with nitrogen-containing gas or a mixture thereof with an inert gas); (3) regulating the ball milling speed and running time to crush the raw material powder particles; in an inert gas atmosphere, opening the ball mill jar, taking out the powder mixture and drying it. In terms of parameter setting of the above process, the initial particle size of the elemental boron powder raw material is 3-50 microns (commercial size); the catalyst includes but is not limited to a mixture of one or more substances, specifically including metal nanoparticles (including but not limited to nano-scale powders of iron, chromium, and nickel, with a particle size between 50 and 200 nanometers), metal salts (including but not limited to iron nitrate, cobalt nitrate, and chromium nitrate), oxides (including but not limited to lithium oxide, cobalt oxide, yttrium oxide, ferrous oxide, iron oxide, magnesium oxide, and aluminum oxide); the ratio (mass ratio) of the elemental boron powder / catalyst mixture is controlled between 100 parts / 0 parts and 100 parts / 25 parts; the materials of the ball mill and the ball mill include but are not limited to stainless steel, carbon steel, etc. Tungsten, zirconium oxide; ball milling beads contain a compound of three different sizes (diameters are 25.4, 15, and 5 mm), the quantity ratio of the first two is 1:3, and the mass ratio of ball milling beads to the mixed powder is controlled at 40:1-120:1; the liquid grinding aid includes but is not limited to methanol, ethanol, and isopropanol, and the mass ratio of the grinding aid to the mixed powder is controlled at 1:1-3:1; the ball milling atmosphere is composed of one or more mixtures of argon, nitrogen and ammonia, and its initial pressure is maintained at 1-4 standard atmospheres; the ball milling speed and time are controlled at 300-600 rpm and 90-160 hours respectively; the temperature of the drying process does not exceed 35°C and the time is 24-36 hours.
[0035] Figure 1 , 2 , 3, 4, 5, and 6, in step 2, the ball-milled particles are specifically screened by a multi-stage cyclone separator ( Figure 2Schematic diagram of the layout of the components of the feeding module), including the following steps: (1) placing the dried powder from the above step 1 in a powder raw material storage device 21, and transmitting it to the upper inlet of the first-stage cyclone separator 22 through a screw feeder, and the powder agglomerate particles with larger particle sizes return to the powder raw material storage device 21 through the lower ash discharge port, and the powder agglomerate particles with smaller particle sizes leave through the upper exhaust port; (2) turning on the powder feeding switch 23, the powder agglomerate particles with smaller particle sizes are crushed and evenly dispersed in the gas medium under the high-speed airflow generated by the compressed gas supply control device 24, and enter the second-stage cyclone separator 25, wherein the powder agglomerate particles with larger particle sizes after dispersion return to the upper return inlet of the first-stage cyclone separator 22 through the lower ash discharge port, and the ultrafine powder particles with smaller particle sizes after dispersion leave the feeding module through the upper exhaust port. In terms of parameter setting of the above process, the volume of the dried powder charged at one time accounts for 50-75% of the storage volume in the raw material storage device 21; the feeding speed of the screw feeder is controlled at 10-30 ml / min; the number of first-stage cyclone separators can be adjusted according to actual conditions, and the total number of cyclone separators involved in the system is not less than 2; the compressed gas is a mixed gas of one or more of argon, nitrogen, and ammonia, and the flow rate is 10-30 liters / min.
[0036] Figure 1 , 2 , 3, 4, 5, 6, in step 3, the specific generation and regulation of high temperature plasma ( Figure 3Schematic diagram of the layout of the components of the induction plasma module), including the following steps: (1) plasma is generated inside the ignition chamber 32 through the induction plasma control cabinet 31 and its power is regulated; (2) the matrix tube assembly 33 is placed in the induction coil 34 for guiding the flow, and the carrier gas (according to actual conditions, the precursor can be introduced through the carrier gas) and the auxiliary gas are introduced from the gas inlet A35, and the cooling gas is introduced from the gas inlet B36. The plasma flame plume leaves the induction plasma module from the induction plasma nozzle 37, and the cooling medium enters from the coolant inlet 38 and flows out from the coolant outlet 39, adopting a circulating cooling scheme. In terms of parameter setting of the above scheme, the rectangular tube combination adopts concentric quartz tubes; the carrier gas uses a mixed gas of one or more of argon, nitrogen, and ammonia (it can be used or not to introduce the precursor ultrafine powder according to actual needs; if the precursor ultrafine powder is introduced at the same time, the solid matter flow rate is 1-10 g / min), and the total gas flow rate is controlled within the range of 1-20 liters / min; the auxiliary gas uses a mixture of one or more of argon, nitrogen, and ammonia, and the flow rate is controlled within the range of 25-50 liters / min, which is used to maintain the plasma flame plume and introduce the precursor ultrafine powder into the end of the tube; the cooling gas uses argon or nitrogen or a mixture of the two, and the gas flow rate is controlled within the range of 50-250 liters / min, which is used to isolate the plasma gas from the inner wall of the rectangular tube; the cooling medium uses compressed air or deionized water, which is used to regulate the working temperature of the induction coil 34.
[0037] Figure 1 , 2 , 3, 4, 5, and 6, in step 4, the specific high temperature plasma method for preparing BNNTs ( Figure 4Schematic diagram of the layout of the components of the reaction chamber module), including the following steps: (1) introducing the precursor ultrafine powder from the ultrafine powder feed port 42 on the side of the premixing chamber 41, and evenly releasing it from the powder distribution pipe 43 with small holes. The precursor ultrafine powder is rapidly vaporized under the action of the high-temperature flame plume (nitrogen-containing plasma gas) at the induction plasma nozzle 37, and evenly mixed with the nitrogen source inside the premixing chamber 41 to form a high-temperature boron-nitrogen intermediate compound; (2) the premixing chamber 41 is protected by a cooling medium, and the cooling medium enters from the coolant inlet A44 and flows out from the coolant outlet A45; (3) the high-temperature boron-nitrogen intermediate compound enters a series of reaction chambers (inlet A45) in series through the inlet connecting component 46. The reaction chamber module is quenched by a plurality of inlet section reaction chambers (inlet section reaction chamber 47, connecting section reaction chamber 412 and outlet section reaction chamber 417), each reaction chamber comprises an independent insulation layer (inlet section insulation layer 48, connecting section insulation layer 413 and outlet section insulation layer 418), a temperature measuring thermocouple (inlet section thermocouple 49, connecting section thermocouple 414 and outlet section thermocouple 419), a coolant inlet (inlet section coolant inlet 410, connecting section coolant inlet 415 and outlet section coolant inlet 420) and an outlet (inlet section coolant outlet 411, connecting section coolant outlet 416 and outlet section coolant outlet 421), and most of the quenched products leave the reaction chamber module through the outlet connecting component 422. In terms of parameter settings of the above scheme, the interior of the premixing chamber is cylindrical, 75-200 mm high, 25-100 mm in diameter, the direction of the ultrafine powder feed port 42 is tangent to the cylinder, and the angle with the top surface is controlled within the range of 30-60°, the flow rate of the solid precursor ultrafine powder introduced is 1-10 g / min, the carrier gas uses a mixture of one or more of argon, nitrogen, and ammonia, and the total flow rate is controlled within the range of 1-20 liters / min, and the cooling medium (premixing chamber 41) uses compressed air or deionized water to adjust its working temperature. degree; the thermocouple adopts tungsten-rhenium or platinum-rhodium thermocouple, which is used to monitor the temperature outside the reaction chamber; the reaction chamber is made of graphite, and there is a filling gap between it and the water-cooled wall, which can be filled with insulation materials of different thicknesses (or no insulation material is selected), and at the same time, the required temperature field is constructed by adjusting the type of cooling medium (including but not limited to compressed air or deionized water) and flow rate to adjust the quenching rate of the boron-nitrogen intermediate compound; the reaction chamber can include multiple connecting sections (1-3) for constructing the required temperature field to adjust the quenching rate of the boron-nitrogen intermediate compound.
[0038] Figure 1 , 2 , 3, 4, 5, 6, in step 5, the further cooling and transfer of the specific product ( Figure 5Schematic diagram of the layout of the components of the connection module), including the following steps: (1) the product prepared in the above step 4 enters the connection module from the inlet connection plate 51, and the working state of the plasma flame plume and the distribution of the product in the reaction chamber module can be observed through the observation window. The gas pressure inside the system is evaluated by the pressure level measured at the pressure gauge 53, and the pressure of the reaction system is controlled in conjunction with the pressure transmitter 55. A safety valve 56 is provided to ensure that the system pressure does not exceed the normal pressure range during the reaction process; (2) based on the temperature value obtained at the thermometer 54, the type and flow rate of the cooling medium used in the front section and the rear section (two independent front section coolant inlets 57, front section coolant outlets 58, rear section coolant inlets 59, and rear section coolant outlets 510) are adjusted to control the temperature of the product at the outlet connection plate 511. In terms of parameter setting of the above scheme, the normal pressure value range is 85%-115% of the set pressure level (within the range of 1-12 standard atmospheric pressure); the safety valve connection flange is DN125, which is convenient for checking the upper and lower pipes after removal; the thermocouple adopts platinum-rhodium thermocouple; by adjusting the type of cooling medium (compressed air or deionized water) and flow rate, the product can be quickly cooled to a low temperature to keep the outlet temperature of the connection module below 85°C.
[0039] Figure 1 , 2 , 3, 4, 5, 6, in step 5, the specific product collection ( Figure 6In the schematic diagram of the layout of the components of the collection and filtration module, the product enters the filter tank 62 through the inlet connecting plate A61. During the reaction, the collection of the product can be monitored through the window and the sampling port 63, and necessary adjustments can be made through the operation port 64. Large particle products cannot pass through the filter cartridge 65 (after the reaction is completed, the window and the sampling port 63 can be opened to further collect the product). Small particle products pass through the filter screen of the filter cartridge 65 and then pass through the outlet connecting plate A66 and the filter bag tank connecting pipe 67 before entering the filter bag tank 68. A filter bag tank viewing window 69 is provided on the outer wall of the filter bag tank 68; large particle products cannot pass through the filter bag 610, and after the reaction is completed, they are collected in the ash tray 611 due to gravity factors; small particle products can pass through the filter bag and enter the gas storage tank 614 along the filter bag tank connecting pipe A612. Independent regulating valves (regulating valve a613 and regulating valve b615) are respectively provided at the inlet and outlet of the gas storage tank as auxiliary means of regulating the internal pressure level of the system; product powder that cannot be collected is discharged and purified from the exhaust gas outlet 616 under the action of airflow. In terms of parameter setting of the above scheme, the flange interface size at the sampling port 63 is DN350, which is convenient for placing or removing containers, and a window is installed on the flange cover; the flange interface size at the operation port 64 is DN125, and a window (for observation) or gloves (for operation) can be selected; the filter cartridge 65 and the filter bag 610 are both equipped with differential pressure transmitters, and if blockage occurs, no backblowing treatment is performed; the gas storage tank 614 and the regulating valve a613 and the regulating valve b615 are used to assist in regulating the system pressure to reduce abnormal or unstable working conditions of the plasma flame plume caused by pressure fluctuations.
[0040] Figure 1 , 2, 3, 4, 5, and 6, the production process of the device for preparing boron nitride nanotubes based on the plasma method, Example 1 includes the following steps: (1) granulating the boron source solid powder raw material by high-energy ball milling process: weighing 4 grams of high-purity amorphous elemental boron powder (99.9%, ~5 μm); stainless steel ball milling beads (including three different sizes, with diameters of 25.4 mm (2 beads), 15 mm (6 beads) and 5 mm (about 210 beads), with a total mass of 320 grams; The mass ratio of grinding beads to solid powder is 80:1), elemental boron powder and 8 ml of ethanol are placed in a stainless steel ball mill; the mixed gas is filled in the tank and the initial pressure in the tank is adjusted (the partial pressures of ammonia and argon are 2.5 and 1 atmospheres, respectively; a total of 3.5 atmospheres); the ball mill speed (600 rpm) and ball milling time (120 hours) are set to complete the ball milling premixing and crushing process; in a glove box (argon atmosphere), the mixed material is taken out and dried (25°C, 24 hours). (2) Screening the dried powder by a secondary cyclone separator: The dried powder (about 100 g in total after repeated step (1)) is placed in a powder raw material storage device 21 and transferred to the upper inlet of the first-stage cyclone separator 22 by a screw feeder (feeding speed: 15 ml / min). The powder agglomerates with larger particle sizes return to the powder raw material storage device 21 through the lower ash discharge port, and the powder agglomerates with smaller particle sizes leave through the upper exhaust port. The powder feeding switch 23 is turned on. The agglomerates with smaller particle sizes are dispersed into fine powder by the high-speed airflow (nitrogen with a flow rate of 20 L / min) generated by the compressed gas supply control device 24. The agglomerates with larger particle sizes that cannot be effectively dispersed return to the upper return inlet of the first-stage cyclone separator 22 through the lower ash discharge port. The ultrafine powder with smaller particle sizes that is effectively dispersed leaves the feeding module through the upper exhaust port. (3) Generation and regulation of high-temperature plasma: Plasma is generated and regulated inside the ignition chamber 32 through the induction plasma control cabinet 31; the gas composition and flow rate are adjusted as follows: nitrogen is used as the carrier gas (excluding solid ultrafine powder raw materials), auxiliary gas and cooling gas, and the flow rates are 3, 27 and 60 liters / minute (a total of 90 liters / minute). Compressed air is used as the cooling medium to control the temperature of the ignition chamber 32, and its flow rate is 3 liters / minute.(4) Preparation of BNNTs by high-temperature plasma method: Solid precursor raw materials (feed rate: 1.5 g / min; nitrogen is used as carrier gas with a flow rate of 1.5 liters / min) are introduced from the ultrafine powder feed port 42 on the side of a cylindrical premixing chamber 41 (50 mm in diameter and 120 mm in height), and are guided into the premixing chamber 41 by a powder distribution pipe 43 with small holes; the precursor ultrafine powder is rapidly vaporized under the action of the high-temperature flame plume (nitrogen-containing plasma gas) at the induction plasma nozzle 37, and is uniformly mixed with the nitrogen source inside the premixing chamber 41 to form a high-temperature boron-nitrogen intermediate mixture; the premixing chamber 41 is temperature-controlled and protected by a cooling medium (compressed air, flow rate: 1.5 liters / min); the high-temperature boron-nitrogen intermediate mixture enters a series of A series of reaction chambers (the number of inlet section, connecting section and outlet section chambers is 1) are quenched; each reaction chamber comprises an independent insulation layer (the inlet section insulation layer 48, the connecting section insulation layer 413 and the outlet section insulation layer 418 are all made of graphite) and a temperature measuring thermocouple (the inlet section thermocouple 49 and the connecting section thermocouple 414 are tungsten-rhenium thermocouples, and the outlet section thermocouple 419 is platinum-rhodium thermocouple); the type and flow rate of the cooling medium are adjusted to thereby control the quenching rate of the boron-nitrogen intermediate mixture in the reaction chamber (the inlet section and the connecting section use compressed air as the cooling medium with a flow rate of 1.5 liters / minute; the outlet section uses deionized water as the cooling medium with a flow rate of 5 liters / minute), and most of the quenched products leave the reaction chamber module through the outlet connecting component 422. (5) Further cooling and transfer of the product: The quenched product enters the connection module from the inlet connection plate 51; the working state of the plasma flame plume and the accumulation of the product in the reaction chamber module can be observed through the observation window; the overall pressure of the system (7.5 atmospheres) is regulated by the pressure transmitter 55, and deionized water is used as a cooling medium to cool the connection module to maintain the outlet temperature below 85°C (the circulation flow rate of the deionized water can be adjusted according to the temperature value measured by the platinum-rhodium thermocouple at the thermometer 54). (6) Collection of products: Products enter the filter tank 62 through the inlet connecting plate A61; during the reaction, the window and the sampling port 63 can be used to determine whether the channel is blocked, and necessary adjustments can be made through the operation port 64; during the reaction, the pressure level inside the system is further stabilized through the regulating valve a613 and the regulating valve b615 (to reduce the instability of the working state of the plasma flame plume and additional airflow disturbance caused by pressure changes); products and waste that cannot be collected are discharged and purified from the exhaust gas discharge port 616 under the action of the airflow; after the reaction is completed, the product agglomerates with decreasing sizes can be collected in the filter cartridge 65 and the ash tray 611. It should be noted that when operating the device, the internal pressure of the plasma flame plume and the reaction system must be stabilized before the precursor ultrafine powder can be introduced into the premixing chamber 41. Figure 7This is a SEM image of the raw material amorphous elemental boron powder particles in this example, indicating that the particle size of the particles before ball milling is about 3-5 microns; Figure 8 is a SEM image of the powder after ball milling, showing that the powder is an agglomerate of small-sized particles (submicron level); Fig. 9 This is the particle size distribution diagram of the ultrafine powder after particle size screening treatment. D10 (D10 represents 10% of all particles), D50 (D50 represents 50% of all particles) and D90 (D90 represents 90% of all particles) are 0.172, 0.235 and 0.353 microns respectively, indicating that after pretreatment, the powder particle size is significantly reduced and the particle size distribution is narrow. Fig.10 The XPS graph of the precursor ultrafine powder in this embodiment shows that BN chemical bonds exist in the powder material after ball milling (which is conducive to the synthesis of BNNTs), indicating that the ball milling process can effectively improve the chemical reaction activity of the raw materials; Fig.10 In the equation, eV stands for electron volt, BN stands for boron-nitrogen chemical bond, BB stands for boron-boron chemical bond, B1S stands for the 1S orbital of boron, NH3 stands for ammonia, and at% stands for atomic percentage. Fig.11 and Fig.12 They are SEM and TEM images of the BNNTs prepared in Example 1 of the present invention, respectively, indicating that the high-temperature thermal plasma method based on pre-treated precursor ultrafine powder can prepare BNNTs with a diameter of about 10-20 nm; after weighing on a balance, the single batch conversion rate is about 53%. Fig.13 In the equation, eV stands for electron volt, BN stands for boron-nitrogen chemical bond, BB stands for boron-boron chemical bond, B1S is the 1S orbital of boron, N2 stands for nitrogen, and at% stands for atomic percentage.
[0041] Figure 1 , 2, 3, 4, 5, and 6, the production process of the device for preparing boron nitride nanotubes based on the plasma method, Example 2 includes the following steps: (1) granulating the boron source solid powder raw material by high-energy ball milling process: weigh 4 grams of high-purity amorphous elemental boron powder (99.9%, ~5 μm); put stainless steel ball mill beads (including three different sizes, with diameters of 25.4 mm (2 beads), 15 mm (6 beads) and 5 mm (about 210 beads), with a total mass of 320 grams; the mass ratio of ball mill beads to solid powder is 80:1), elemental boron powder, 0.4 grams of iron nitrate (used as a catalyst) and 12 milliliters of ethanol into a stainless steel ball mill; fill the tank with mixed gas and adjust the initial pressure in the tank (nitrogen atmosphere, 3 atmospheres); set the ball mill speed (300 rpm) and time (150 hours) to complete the ball milling premixing and crushing process; take out the mixture material in the glove box (argon atmosphere) and dry it (30°C, 36 hours). (2) Screening the dried powder by a secondary cyclone separator: The dried powder (about 115 g in total after repeated step (1)) is placed in a powder raw material storage device 21 and transferred to the upper inlet of the first-stage cyclone separator 22 by a screw feeder (feeding speed of 20 ml / min). The powder agglomerates with larger particle sizes return to the powder raw material storage device 21 through the lower ash discharge port, and the powder agglomerates with smaller particle sizes leave from the upper exhaust port. The powder feeding switch 23 is turned on. The agglomerates with smaller particle sizes are subjected to the high-speed airflow (nitrogen with a flow rate of 25 L / min) generated by the compressed gas supply control device 24. Most of the particles are evenly dispersed into fine powder and then enter the second-stage cyclone separator 25. The agglomerates with larger particle sizes that cannot be effectively dispersed return to the upper return inlet of the first-stage cyclone separator 22 through the lower ash discharge port. The ultrafine powder with smaller particle sizes that is effectively dispersed leaves the feeding module through the upper exhaust port. (3) Generation and regulation of high-temperature plasma: Plasma is generated and regulated inside the ignition chamber 32 through the induction plasma control cabinet 31; the gas composition and flow rate are adjusted as follows: nitrogen is used as the carrier gas (excluding solid ultrafine powder raw materials), auxiliary gas and cooling gas, and the flow rates are 5, 25 and 70 liters / minute respectively (a total of 100 liters / minute); compressed air is used as the cooling medium to control the temperature of the ignition chamber 32, and its flow rate is 3.5 liters / minute.(4) Preparation of BNNTs by high-temperature plasma method: Solid precursor raw materials (feed rate: 2 g / min; nitrogen is used as carrier gas with a flow rate of 2 liters / min) are introduced from the ultrafine powder feed port 42 on the side of a cylindrical premixing chamber 41 (50 mm in diameter and 120 mm in height), and are guided into the premixing chamber 41 by a powder distribution pipe 43 with small holes; the ultrafine precursor powder is rapidly vaporized under the action of the high-temperature flame plume (nitrogen-containing plasma gas) at the induction plasma nozzle 37, and is uniformly mixed with the nitrogen source inside the premixing chamber 41 to form a high-temperature boron-nitrogen intermediate mixture; the premixing chamber 41 is protected by a cooling medium (compressed air, flow rate: 1.5 liters / min); the high-temperature boron-nitrogen intermediate mixture enters a series of inlet connecting components 46 The reaction chambers connected in series (the number of the inlet section, the connecting section and the outlet section chambers are all 1) are quenched; each reaction chamber comprises an independent insulation layer (the inlet section insulation layer 48, the connecting section insulation layer 413 and the outlet section insulation layer 418 are all made of graphite) and a temperature measuring thermocouple (the inlet section thermocouple 49 and the connecting section thermocouple 414 use tungsten-rhenium thermocouples, and the outlet section thermocouple 419 uses platinum-rhodium thermocouple); the type and flow rate of the cooling medium are adjusted to thereby control the quenching rate of the boron-nitrogen intermediate mixture in the reaction chamber (the inlet section and the connecting section use compressed air as the cooling medium with a flow rate of 2 liters / minute; the outlet section uses deionized water as the cooling medium with a flow rate of 5 liters / minute), and most of the quenched products leave the reaction chamber module through the outlet connecting component 422. (5) Further cooling and transfer of the product: The quenched product enters the connection module from the inlet connection plate 51; the working state of the plasma flame plume and the accumulation of the product generated in the reaction chamber module can be observed through the observation window; the system pressure (1 atmosphere) is regulated by the pressure transmitter 55, and deionized water is used as the cooling medium to cool the connection module to maintain the outlet temperature below 85°C (the circulation flow rate of the deionized water can be adjusted according to the temperature value measured by the platinum-rhodium thermocouple at the thermometer 54). (6) Collection of products: Products enter the filter tank 62 through the inlet connecting plate A61; during the reaction, the window and the sampling port 63 can be used to determine whether the channel is blocked, and necessary adjustments can be made through the operation port 64; during the reaction, the regulating valve a613 and the regulating valve b615 can be used to assist in regulating the pressure level inside the system (to reduce the instability of the working state of the plasma flame plume and additional air flow disturbance caused by pressure changes); products and waste that cannot be collected are discharged and purified from the exhaust gas discharge port 616 under the action of the airflow; after the reaction is completed, the product agglomerates with decreasing sizes can be collected in the filter cartridge 65 and the ash tray 611. It should be noted that when operating the device, the plasma flame plume and the pressure inside the reaction device must be stabilized before the precursor ultrafine powder can be introduced into the premixing chamber 41.The materials in each link of the preparation process of this example were characterized by a method similar to that of Example 1. The results showed that the structural morphology of the precursor and the product were similar to the corresponding substances obtained in Example 1. Fig.13 This is the XPS graph of the precursor ultrafine powder in this example, which shows that there is a high content of BN chemical bonds (73at%) in the powder after ball milling, which can further promote the synthesis of BNNTs; after weighing on a balance, the single batch conversion rate is about 71%, which is significantly improved compared to Example 1 (showing the efficiency after adding the catalyst during the ball milling pretreatment process).
[0042] Figure 1 , 2, 3, 4, 5, and 6, the production process of the device for preparing boron nitride nanotubes based on the plasma method, Example 3 includes the following steps: (1) granulating the boron source solid powder raw material by high-energy ball milling process: weighing 4 grams of high-purity amorphous elemental boron powder (99.9%, ~5 microns); stainless steel ball milling beads (including three different sizes, with diameters of 25.4 mm (2 beads), 15 mm (6 beads) and 5 mm (about 210 beads), with a total mass of 320 grams; the mass ratio of ball milling beads to solid powder is 8 0:1), elemental boron powder, 0.2 g of ferric nitrate, 0.25 g of chromium nitrate and 15 ml of ethanol were placed in a stainless steel ball mill; the mixed gas was filled in the tank and the initial pressure in the tank was adjusted (the mixed gas was composed of ammonia and nitrogen, and the partial pressures of the two gases were 1 and 3 atmospheres, respectively; a total of 4 atmospheres); the ball mill speed (600 rpm) and the ball milling time (90 hours) were set to complete the ball milling premixing and crushing process; in a glove box (argon atmosphere), the mixture material was taken out and dried (35°C, 48 hours). (2) Screening the dried powder by a secondary cyclone separator: The dried powder (about 130 g in total after repeated step (1)) is placed in a powder raw material storage device 21 and transferred to the upper inlet of the first-stage cyclone separator 22 by a screw feeder (feeding speed: 15 ml / min). The powder agglomerates with larger particle sizes return to the powder raw material storage device 21 through the lower ash discharge port, and the powder agglomerates with smaller particle sizes leave from the upper exhaust port. The powder feeding switch 23 is turned on. The agglomerates with smaller particle sizes are dispersed into fine powder by the high-speed airflow (nitrogen with a flow rate of 20 L / min) generated by the compressed gas supply control device 24. The agglomerates with larger particle sizes that cannot be effectively dispersed return to the upper return inlet of the first-stage cyclone separator 22 through the lower ash discharge port. The ultrafine powder with smaller particle sizes that is effectively dispersed leaves the feeding module through the upper exhaust port. (3) Generation and regulation of high-temperature plasma: Plasma is generated and regulated inside the ignition chamber 32 through the induction plasma control cabinet 31; the gas composition and flow rate are adjusted as follows: the carrier gas (containing solid ultrafine powder raw material, with a feed rate of 1.5 g / min), auxiliary gas and cooling gas are argon, nitrogen and nitrogen, respectively, with flow rates of 5, 20 and 65 liters / min (a total of 90 liters / min); compressed air is used as a cooling medium to control the temperature of the ignition chamber 32, and its flow rate is 2.5 liters / min.(4) Preparation of BNNTs by high-temperature plasma method: an ammonia / nitrogen mixture is introduced from the ultrafine powder feed port 42 on the side of a cylindrical premixing chamber 41 (diameter 50 mm, height 150 mm; compared with Examples 1 and 2, since the feeding direction of the precursor ultrafine powder (relative to the horizontal cross section of the tube body) is changed from the tangential direction (premixing chamber 41) to the normal direction (ignition chamber 32), it is necessary to extend the height of the premixing chamber 41 to promote uniform mixing) at flow rates of 0.25 and 0.75 liters per minute, respectively, and is guided into the premixing chamber 41 by a powder distribution pipe 43 with small holes to promote uniform mixing of the reactants; the precursor ultrafine powder introduced in step (3) is fully vaporized under the action of the high-temperature torch (nitrogen-containing plasma gas) at the induction plasma nozzle 37, and is uniformly mixed with the nitrogen source inside the premixing chamber 41 to form a high-temperature boron-nitrogen intermediate mixture; a cooling medium (compressed air, flow rate: 1 .5L / min) is used to control the temperature of the premixing chamber 41; the high-temperature boron-nitrogen intermediate mixture enters a series of reaction chambers in series (the number of the inlet section, the connecting section and the outlet section chambers is 1) through the inlet connecting component 46 for quenching; each reaction chamber comprises an independent insulation layer (the inlet section insulation layer 48, the connecting section insulation layer 413 and the outlet section insulation layer 418 are all made of graphite) and a temperature measuring thermocouple (the inlet section thermocouple 49 and the connecting section thermocouple 414 use tungsten-rhenium thermocouples, and the outlet section thermocouple 419 uses platinum-rhodium thermocouples); the type and flow rate of the cooling medium are adjusted to thereby control the quenching rate of the boron-nitrogen intermediate mixture in the reaction chamber (the inlet section and the connecting section use compressed air as the cooling medium with a flow rate of 2L / min; the outlet section uses deionized water as the cooling medium with a flow rate of 5L / min), and most of the quenched products leave the reaction chamber module through the outlet connecting component 422. (5) Further cooling and transfer of the product: The quenched product enters the connection module from the inlet connection plate 51; the working state of the plasma flame plume and the accumulation of the generated products in the reaction chamber module can be observed through the observation window; the pressure is regulated by the pressure transmitter 55 (2.5 atmospheres), and deionized water is used as a cooling medium to cool the connection module to keep the outlet temperature below 85°C (the circulation flow rate of the deionized water can be adjusted according to the temperature value measured by the platinum-rhodium thermocouple at the thermometer 54). (6) Collection of products: Products enter the filter tank 62 through the inlet connecting plate A61. During the reaction, the window and the sampling port 63 can be used to determine whether the channel is blocked, and necessary adjustments can be made through the operating port 64. During the reaction, the internal pressure level of the system is further stabilized by regulating valve a613 and regulating valve b615 (to reduce the instability of the working state of the plasma flame plume and additional airflow disturbances caused by pressure changes). Products and waste materials that cannot be collected are discharged and purified from the exhaust port 616 under the action of the airflow. After the reaction is completed, product agglomerates of decreasing sizes can be collected in the filter cartridge 65 and the ash tray 611, respectively.It should be noted that when the device is running, the plasma flame plume and the internal pressure of the reaction device must be stabilized before the precursor ultrafine powder can be introduced into the ignition cavity 32. The materials in each link of the preparation process of this embodiment are characterized by a method similar to that of Example 1. The results show that the morphology of the reaction precursor is similar to that of the corresponding material in Example 1; compared with Examples 1 and 2, there are wide-diameter BNNTs (boron nitride nanosheets with barbed structures) in the product. Fig.14 ), which is mainly attributed to the use of multiple catalysts in the ball milling process and the introduction of a certain proportion of ammonia during the ball milling and high-temperature plasma reaction process); after weighing on a balance, the single batch conversion rate is about 61% (including BNNTs of all morphologies).
[0043] The present invention has the following advantages. (1) The present invention combines the low-temperature ball milling process with the high-temperature thermal plasma method to prepare BNNTs; on the one hand, compared with the traditional ball milling annealing process for preparing BNNTs, the present invention adopts high-temperature thermal plasma, which can quickly gasify the boron-containing raw material and efficiently mix it with the nitrogen source, thereby significantly improving the output per unit time; on the other hand, compared with the single high-temperature thermal plasma method for preparing BNNTs, the method involved in the present invention introduces a ball milling process, which can significantly improve the chemical reaction activity of the precursor and then optimize the conversion rate of the raw material; (2) Since the present invention introduces a particle size screening process, an ultrafine powder precursor (submicron level) with a narrow particle size distribution can be prepared; on the one hand, a narrower particle size distribution is conducive to the preparation of BNNTs products with similar morphological characteristics; on the other hand, when smaller particles are used as precursors, their boiling point is significantly reduced, It is more conducive to its rapid gasification and full mixing with the nitrogen source under the action of high-temperature thermal plasma, thereby effectively reducing the impurity content in the product and improving the energy utilization efficiency of the high-temperature process, which is more in line with the concept of green production; (3) The production system involves multiple adjustable variables, including the type and ratio of raw materials (including but not limited to the catalyst used in the ball milling process, the solid boron source powder, the type and ratio of the nitrogen source atmosphere used) and process control parameters (including but not limited to the pressure during the reaction process, the flow rate of each gas during the high-temperature thermal plasma method, and the quenching rate of the product in the cavity), so as to facilitate the effective regulation of the structural characteristics of the BNNTs product; (4) The synthetic process involved in the production is suitable for semi-continuous production. During the process, all solid substances are transported in each module by a screw extruder and a carrier gas. In addition, after the high-temperature plasma reactor components are expanded, it has the ability to realize semi-continuous mass production of BNNTs.
[0044] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is limited to the details of the above exemplary embodiments, and that the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes that fall within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0045] In addition, it should be understood that although the present specification is described according to the implementation mode, the implementation mode does not only include an independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in the embodiments can also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A device for preparing boron nitride nanotubes based on a plasma method, characterized in that: It includes a precursor pretreatment module, a feed module, an induction plasma module, a reaction chamber module, a connection module, a collection and filtration module, a pressure control module, a cooling system centralized control module, an electric and gas centralized control module, a gas supply module and a rack and platform module; the precursor pretreatment module, the feed module, the induction plasma module, the reaction chamber module, the connection module, the collection and filtration module, the pressure control module, the cooling system centralized control module, the electric and gas centralized control module, and the gas supply module are installed on the rack and platform module, and the electric and gas centralized control module controls the power supply output terminal and the precursor pretreatment module, the feed module, the induction plasma module, the reaction chamber module, the connection module, The control signal input ends of the collection and filtration module, the pressure control module, the cooling system centralized control module, and the gas supply module are electrically connected respectively; the gas output end of the gas supply module and the gas input ends of the precursor pretreatment module, the feeding module, the induction plasma module, the reaction chamber module, the connection module, and the collection and filtration module are respectively connected through pipelines; the signal input end of the cooling system centralized control module and the signal output ends of the induction plasma module, the reaction chamber module, and the connection module are respectively electrically connected; the signal input end of the pressure control module and the pressure signal output end of the pressure sensor installed in the feeding module, the reaction chamber module, the connection module, and the collection and filtration module are respectively electrically connected; The precursor pretreatment module is a high-energy ball milling device, the discharge pipe of the high-energy ball mill is connected to the feed pipe of the powder raw material storage device of the feed module, the discharge pipe of the second-stage cyclone separator of the powder raw material storage device is connected to the ultrafine powder feed port of the reaction chamber module, the induction plasma nozzle of the induction plasma module is connected to the premixing cavity of the reaction chamber module, the outlet connection component of the reaction chamber module is connected to the inlet connection port of the connection module, and the outlet connection port of the connection module is connected to the inlet connection port of the collection and filtration module; the feed module includes a powder raw material storage device, a first-stage cyclone separator, a powder feed switch, a compressed gas supply control device, a second-stage cyclone separator, and a powder raw material storage device. A screw feeder is installed inside, the discharge pipe of the screw feeder is connected to the upper feed pipe of the first-stage cyclone separator, the lower return pipe at the lower end of the first-stage cyclone separator is connected to the right return pipe at the right end of the powder raw material storage device, the discharge pipe of the first-stage cyclone separator is connected to the lower feed pipe of the powder feed switch, the upper discharge pipe of the powder feed switch is connected in parallel to the right exhaust pipe of the compressed gas supply control device and the upper feed pipe on the left side of the second-stage cyclone separator, the lower return pipe at the lower end of the second-stage cyclone separator is connected to the upper return pipe on the right side of the upper end of the first-stage cyclone separator, and the left air inlet pipe of the compressed gas supply control device is connected to one of the gas output ends of the gas supply module;The induction plasma module includes an induction plasma control cabinet, an ignition cavity, a matrix tube assembly, an induction coil, a gas inlet A, a gas inlet B, an induction plasma nozzle, a coolant inlet, and a coolant outlet. The signal output end of the induction plasma control cabinet is electrically connected to the induction coil, the electric valves of the gas inlet A and the gas inlet B, and the signal input end of the electric valves of the coolant inlet and the coolant outlet. The outer ends of the gas inlet A, the gas inlet B, and the coolant inlet are respectively connected to the gas output end and the other three gas output ends of the gas supply module. The matrix tube assembly is installed at the inner end of the ignition cavity, and the induction coil is installed at the outer end of the ignition cavity. The reaction chamber module includes a premixing cavity, an ultrafine powder feed port, and a powder distribution pipe. , a coolant inlet, a coolant outlet, an inlet section reaction chamber, a connecting section reaction chamber, an outlet section reaction chamber, an outlet connecting component, the lower end of the premixing chamber and the upper end of the inlet section reaction chamber are installed together via the inlet connecting component, the upper end of the connecting section reaction chamber is connected to the lower end of the inlet section reaction chamber, the lower end of the connecting section reaction chamber is connected to the upper end of the outlet section reaction chamber, the upper end of the outlet connecting component is installed at the lower end of the outlet section reaction chamber, the left side of the ultrafine powder feed port is installed at the right end of the powder distribution pipe, the powder distribution pipe is installed at the upper end of the premixing chamber, the left and right sides of the premixing chamber are respectively installed with a coolant outlet and a coolant inlet, the left outer side of the inlet section reaction chamber is installed with an inlet section insulation layer, and the right end is installed with an inlet section thermocouple The lower right end and the upper left end of the inlet section reaction cavity are respectively provided with an inlet section coolant inlet and an inlet section coolant outlet, the lower right end and the upper left end of the connecting section reaction cavity are respectively provided with a connecting section coolant inlet and a connecting section coolant outlet, the upper right end of the connecting section reaction cavity is provided with a connecting section thermocouple, the lower right end and the upper left end of the outlet section reaction cavity are respectively provided with an outlet section coolant inlet and an outlet section coolant outlet, the upper right end of the outlet section reaction cavity is provided with an outlet section thermocouple, an outlet section insulation layer is provided on the outside of the outlet section reaction cavity, the gas output ends of the three coolant inlet gas supply modules are connected to the fifth, sixth and seventh gas output ends, the three thermocouples are electrically connected to the three temperature collection ports of the electric and gas centralized control module respectively Connection; the connection module includes an inlet connection plate, an observation window, a pressure gauge, a thermometer, a pressure transmitter, a safety valve, an outlet connection plate, and a pipeline. The inlet connection plate is installed at the upper end of the pipeline, the observation window is installed at the upper left end of the pipeline, the pressure gauge and the thermometer are installed at the front and right sides of the upper end of the pipeline respectively, the pressure transmitter is installed at the middle of the upper end of the pipeline, the safety valve is installed at the front side of the rear end of the pipeline, the outlet connection plate is installed at the lower right end of the pipeline, the middle and upper parts of the lower left end of the pipeline are respectively installed with a front coolant inlet and a front coolant outlet, and the lower part and the middle of the upper right end of the pipeline are respectively installed with a rear coolant inlet and a rear coolant outlet; the gas output ends of the two coolant inlet air supply modules are connected to the eighth and ninth gas output ends respectively;The collection and filtration module includes an inlet connection plate, a filter tank, a filter cartridge, an outlet connection plate, a filter bag tank connection pipe, a filter bag tank, a filter bag, a filter bag tank connection pipe, a gas tank, a regulating valve a, a regulating valve b, and an exhaust gas discharge port. The right end of the inlet connection plate is installed at the left end of the filter tank, the filter cartridge is installed in the filter tank, and the two ends of the front side of the filter tank have operation ports respectively. The filter tank has a window and a sampling port at the lower end of the filter cartridge. The lower end of the outlet connection plate is installed at the upper end of the filter tank. The two sides of the filter bag tank connection pipe are respectively installed with the upper end of the outlet connection plate and the middle of the left end of the filter bag tank. The filter bag is installed in the filter bag tank. The opening at the lower front end of the filter bag tank has an ash tray. The front side of the filter bag tank at the lower end of the filter bag has a filter bag tank window. The filter bag tank connection pipe is connected in series with the upper left end of the gas tank through the air inlet and exhaust port of the regulating valve a, and the lower right end of the gas tank is connected in series with the left end of the exhaust gas discharge port of the gas tank through the air inlet and exhaust port of the regulating valve b. ; 2. The production process of the device for preparing boron nitride nanotubes based on a plasma method according to claim 1, characterized in that: The method includes the following processes: S1: the precursor pretreatment module processes solid raw material particles, reduces their particle size, and enters the feeding module; S2: the feeding module obtains ultrafine powder with a narrow particle size distribution by screening the raw materials, which is used as a precursor for preparing BNNTs; S3: the induction plasma module generates a plasma flame plume to provide a high-temperature heat source for the synthesis reaction; S4: Under high temperature, the BNNTs precursor ultrafine powder is vaporized in the reaction chamber module and combined with the gaseous nitrogen source. After cooling, the generated BNNTs enter the connection module. S5: The product obtained in step S4 is cooled in the connection module and then collected in the collection and filtration module.
3. The production process of the device for preparing boron nitride nanotubes based on plasma method according to claim 2, characterized in that: The function of the pressure control module is to monitor and regulate the pressure in the feed module, reaction chamber module, connection module and collection and filtration module, thereby affecting the dispersion level of the material, the synthesis reaction conditions and the collection efficiency of the product.
4. The production process of the device for preparing boron nitride nanotubes based on a plasma method according to claim 2, characterized in that: In step S1, the solid raw material particles are pure amorphous elemental boron powder or a multi-component mixture thereof with a catalyst compound; in step S2, the volume of the powder charged at one time accounts for 50-75% of the storage volume in the raw material storage device, and the feeding speed of the screw feeder is controlled at 10-30 ml / min; the number of first-stage cyclone separators can be adjusted according to actual conditions, and the total number of cyclone separators involved in the system is not less than 2; the compressed gas is a mixed gas of one or more of argon, nitrogen, and ammonia, and the flow rate is 10-30 liters / min.