Polyamide fiber filter material for anaerobic biofilter and preparation method of polyamide fiber filter material
By combining the surface plasma and oxidation treatment of polyamide fibers, combined with chitosan and sodium alginate coatings, the problems of slow hanging membranes of microorganisms in traditional filter materials are solved, and the treatment of anaerobic biological filters is significantly improved. Efficiency and effect.
Patent Information
- Application Number
- CN202411386710.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-30
AI Technical Summary
The microbial membrane hanging speed of traditional anaerobic biological filters is slow and has poor stability, which leads to poor treatment effect of difficult degradation of organic wastewater, and the hydrophilicity and biocompatibility of polyamide fibers are insufficient, affecting its application.
By performing surface plasma treatment and oxidation treatment on polyamide fibers, hydrophilic functional groups are introduced and coated with chitosan and sodium alginate coatings, improving the hydrophilicity and biocompatibility of the fibers, enhancing microbial adhesion and Stability of biofilms.
It significantly improves the adhesion of microorganisms and the stability of biofilms, improves the processing efficiency and treatment effect of anaerobic biological filters, and is significantly better than unmodified fibers and traditional fiber filters.
Smart Images

Figure CN119041192A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of difficult-to-degrade organic wastewater treatment, and specifically relates to a polyamide fiber filter material for an anaerobic biofilter and a preparation method thereof. Background Art
[0002] With the advancement of industrialization, the treatment of refractory organic wastewater has become a major problem in environmental engineering. Anaerobic biofilter is a bioreactor commonly used for the treatment of refractory organic wastewater. It uses anaerobic microorganisms attached to solid fillers to form a biofilm, thereby degrading organic matter in the wastewater.
[0003] Although traditional anaerobic biofilters have certain advantages in treating organic wastewater, their wide application is limited by problems such as slow biofilm formation and unstable treatment effect. Therefore, how to improve the biofilm formation efficiency and treatment effect of anaerobic biofilters has become a technical problem that needs to be solved urgently. In anaerobic biofilters, filter media, as a carrier for microbial growth and biofilm formation, directly affects the removal effect of pollutants. Common anaerobic biofilters have low filter media strength and poor corrosion resistance, which seriously affects the treatment performance of anaerobic biofilters. Therefore, preparing filter media with good biofilm formation performance and high stability is the key to improving the treatment efficiency of anaerobic biofilters.
[0004] At present, polyamide fiber is widely used in water treatment due to its excellent mechanical properties and chemical corrosion resistance. However, the hydrophilicity and biocompatibility of polyamide fiber surface are poor, resulting in slow biofilm formation in anaerobic biofilters and weak microbial attachment, which affects the overall treatment effect. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a polyamide fiber filter material for anaerobic biofilter and a preparation method thereof, and performs surface hydrophilization and functional coating modification on the polyamide fiber to improve its hydrophilicity and biocompatibility, thereby accelerating the microbial biofilm formation process, enhancing the stability and degradation efficiency of the biofilm, and solving the problem of low treatment effect of existing difficult-to-degrade organic wastewater.
[0006] The present invention is achieved through the following technical solutions:
[0007] A method for preparing a polyamide fiber filter material for an anaerobic biofilter comprises the following steps:
[0008] S1, subjecting the polyamide fiber to surface plasma treatment at a power of 90-110 W, and then cleaning the residual reactants to obtain the plasma-treated polyamide fiber;
[0009] S2, oxidizing the polyamide fiber after the plasma treatment with a main oxidant and an auxiliary oxidant, wherein when the main oxidant is ammonium persulfate, the auxiliary oxidant is ferric chloride, when the main oxidant is potassium permanganate, the auxiliary oxidant is sulfuric acid, when the main oxidant is ozone, the auxiliary oxidant is hydrogen peroxide, when the main oxidant is benzoyl peroxide, the auxiliary oxidant is silver nitrate, to obtain an oxidized polyamide fiber;
[0010] S3, sequentially coating chitosan coating and sodium alginate coating on the oxidized polyamide fiber, the mass ratio of chitosan, sodium alginate and the polyamide fiber treated with plasma in S1 is (0.075-0.25):(0.075-0.25):1, and obtaining a polyamide fiber filter material for an anaerobic biofilter.
[0011] Preferably, the polyamide fiber type described in S1 is PA6.
[0012] Preferably, in S1, the polyamide fiber is treated at a power of 90-110 W for 12-18 min, and the gas flow rate for generating plasma is 8-12 L / min.
[0013] Preferably, when the main oxidant is ammonium persulfate and the auxiliary oxidant is ferric chloride, the oxidation treatment in S2 is carried out as follows:
[0014] The plasma-treated polyamide fiber obtained in S1 is immersed in a 0.1M ammonium persulfate solution at 45-55°C for 25-35 minutes, then the obtained polyamide fiber is washed, and then immersed in a 0.05M ferric chloride solution for 15-25 minutes, then washed and dried to obtain an oxidized polyamide fiber.
[0015] Preferably, when the main oxidant is potassium permanganate and the auxiliary oxidant is sulfuric acid, the oxidation treatment described in S2 is carried out as follows:
[0016] Sulfuric acid with a concentration of 0.1-0.5 M is added to a 0.01-0.05 M KMnO4 solution to obtain a mixed solution, and then the plasma-treated polyamide fiber obtained in S1 is immersed in the mixed solution at 40-50° C. for 30-60 min, and then washed and dried to obtain oxidized polyamide fiber.
[0017] Preferably, when the primary oxidant is ozone and the auxiliary oxidant is hydrogen peroxide, the oxidation treatment in S2 is carried out as follows:
[0018] The plasma-treated polyamide fiber obtained in S1 is placed in an ozone environment with a concentration of 5-10 ppm for 15-30 minutes, then immersed in a 0.1-0.5 M 30-40° C. H 2 O 2 solution for 20-40 minutes, and then washed and dried to obtain an oxidized polyamide fiber.
[0019] Preferably, when the primary oxidant is benzoyl peroxide and the auxiliary oxidant is silver nitrate, the oxidation treatment described in S2 is carried out as follows:
[0020] The plasma-treated polyamide fiber obtained in S1 is immersed in a 0.05-0.2M benzoyl peroxide solution, and then ultraviolet light or heating to 60-80°C is used to stimulate the decomposition of benzoyl peroxide for 20-30 minutes. The obtained polyamide fiber is then immersed in a 0.01-0.05M silver nitrate solution for 15-25 minutes, and then washed and dried to obtain an oxidized polyamide fiber.
[0021] Preferably, S3 sequentially coats the chitosan coating and the sodium alginate coating on the oxidized polyamide fiber through the following process:
[0022] The pH values of chitosan solution and sodium alginate solution, both of which are 1.5%-2.5% by mass, are adjusted to 4.3-4.7 and 7.0, respectively, to obtain mixed solution a and mixed solution b. The oxidized polyamide fiber obtained by S2 is immersed in the mixed solution a, then dried, immersed in the mixed solution b, and finally dried to obtain a polyamide fiber filter material for an anaerobic biofilter.
[0023] Preferably, the deacetylation degree of chitosan is 80%, the molecular weight range is 50,000-190,000Da, the viscosity of sodium alginate is 200-800mPa.s, and the polyamide fiber is immersed in the mixed solution a for 45-75min, then immersed in the mixed solution b for 45-75min, and then dried.
[0024] A polyamide fiber filter material obtained by any one of the above-mentioned methods for preparing a polyamide fiber filter material for an anaerobic biofilter.
[0025] Compared with the prior art, the present invention has the following beneficial technical effects:
[0026] The invention discloses a method for preparing a polyamide fiber filter material for an anaerobic biofilter. The method introduces polar hydrophilic functional groups hydroxyl, carbonyl and carboxyl groups on the fiber surface through high-energy particles and active species generated by 90-110W, thereby improving the hydrophilicity and surface energy of the fiber, thereby enhancing the adhesion of microorganisms and the stability of the biofilm. The roughness of the fiber surface is improved through ion bombardment etching, the attachment points of microorganisms are increased, and the surface energy of the fiber surface is increased, making it easier for the fiber to interact with water molecules and microorganisms. The synergistic oxidation treatment of four main and auxiliary oxidants can introduce hydrophilic functional groups on the polyamide fiber surface, thereby improving the surface hydrophilicity, biocompatibility and polarity of the fiber, and improving the chemical reaction activity of the fiber surface, thereby enhancing the adhesion of microorganisms and the stability of the biofilm. The fiber surface can be further etched to significantly increase the roughness and chemical activity of the fiber surface, thereby providing favorable conditions for microbial biofilm formation, and making the fiber more suitable as a biofilm formation filler for the biofilter. Biocompatible materials chitosan coating and sodium alginate coating can form a complementary coating structure, which is coated on the surface of polyamide fiber. By regulating the dosage of the two, the functionalized coating formed has a stable cross-linked network, provides more attachment points and a good environment, and promotes the growth and fixation of microorganisms. Chitosan has good antibacterial and biocompatibility, and can promote the attachment and growth of microorganisms; sodium alginate can form a stable gel network structure, improve the mechanical strength and stability of the coating, and the combination of the two can provide more attachment points and a good environment, significantly enhancing the fixation of microorganisms and the stability of biofilms. The present invention combines surface hydrophilization and functionalized coating technology to significantly improve the physical and chemical properties of polyamide fibers and enhance the treatment efficiency and stability of biofilters. Plasma treatment has the effect of coarse carving, oxidation treatment has the effect of microcarving, and the coating is functionalized. This treatment sequence ensures the maximum surface modification effect. Plasma treatment provides initial modification, double oxidation further strengthens, and chemical coating forms a stable coating on the optimized surface, providing the best microbial attachment environment and biofilm stability, significantly improving its biofilm speed and treatment efficiency in hydrolysis biofilters. The modified polyamide fiber has excellent hydrophilicity and biocompatibility, enhances the adhesion of microorganisms and the stability of biofilms, and the treatment effect is significantly better than unmodified fibers and traditional fiber filter materials, with significant technical advantages and market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The thickness of the biofilm observed by 3D reconstruction using a laser confocal optical microscope after two weeks of biofilm growth as described in the embodiment of the present invention.
[0028] Figure 2 This is the biofilm thickness observed by 3D reconstruction using a laser confocal optical microscope after the biofilm has grown for two weeks as described in Control Case 1 of the present invention.
[0029] Figure 3This is the biofilm thickness observed by 3D reconstruction using a laser confocal optical microscope after two weeks of biofilm growth as described in Control Case 2 of the present invention.
[0030] Figure 4 This is a picture of the biofilm growth condition taken by a scanning electron microscope two weeks after the biofilm was formed in the implementation case of the present invention.
[0031] Figure 5 This is a picture of the biofilm growth condition taken by scanning electron microscope two weeks after the biofilm formation described in Control Case 1 of the present invention.
[0032] Figure 6 This is a picture of the biofilm growth condition taken by scanning electron microscope two weeks after the biofilm formation described in Control Case 2 of the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0034] The present invention provides a method for preparing a polyamide fiber filter material for an anaerobic biofilter, which specifically comprises the following steps:
[0035] Step 1. Surface plasma treatment
[0036] Polyamide fiber model: PA6 is selected. PA6 has good toughness and fatigue resistance.
[0037] Equipment type: Low temperature atmospheric pressure plasma discharge equipment is used.
[0038] Processing gas: a mixture of argon and oxygen (volume ratio: 80% argon, 20% oxygen).
[0039] Processing parameters: power is 90-110W, processing time is 12-18 minutes, and gas flow rate is 8-12L / min.
[0040] Specific process: Place the polyamide fiber sample in the reaction chamber; start the low-temperature atmospheric pressure plasma discharge equipment and adjust the power and gas flow rate; during the treatment, the high-energy particles and active species in the plasma react with the fiber surface, introduce hydrophilic functional groups and increase the surface roughness; after the treatment is completed, take out the fiber sample, wash it with deionized water to remove the residual reactants and then dry it to remove the deionized water.
[0041] Effect: The main effect of treating polyamide fiber with low-temperature atmospheric pressure plasma is to introduce polar hydrophilic functional groups hydroxyl (-OH), carbonyl (=O) and carboxyl (-COOH) on the fiber surface through high-energy particles and active species in the plasma, thereby improving its hydrophilicity and surface energy, thereby enhancing the adhesion of microorganisms and the stability of biofilms. The roughness of the fiber surface is increased through etching, increasing the attachment points of microorganisms. The surface energy of the fiber surface is increased, making it easier to interact with water molecules and microorganisms.
[0042] Plasma is a partially ionized gas containing a large number of high-energy electrons, ions, free radicals and neutral atoms. The principle of low-temperature atmospheric pressure plasma treatment of polyamide fibers is as follows:
[0043] Plasma excitation: The electric field excites argon and oxygen to form plasma. High-energy electrons collide with gas molecules to produce various active species (free radicals, ions and ultraviolet photons). In argon plasma, high-energy electrons can excite argon molecules to produce active argon atoms and ions: Ar+e - →Ar*+e - (Excited argon atom) Ar*→Ar+hv (releases ultraviolet photons)
[0044] Surface reaction: High-energy electrons, ions and free radicals react chemically with the surface molecules of polyamide fibers, introducing polar functional groups. Oxygen free radicals (O·) and ozone (O3) in oxygen plasma can react with carbon-hydrogen bonds on the fiber surface to generate hydroxyl, carboxyl and carbonyl groups: O·+RH→R·+HO; O3+RH→ROH+O2
[0045] Etching: High-energy ions in the plasma bombard the fiber surface, physically removing some materials and increasing surface roughness. Based on the following reaction: Ar + +R-CH2-CH2-R'→R-CH2-CH-R'+H+Ar, argon ion (Ar + ) can remove a layer of molecules on the fiber surface through kinetic energy impact, forming a microscopic rough structure:
[0046] Step 2. Chemical modification
[0047] Chemical reagents: Double oxidation treatment is performed using ammonium persulfate (APS) and ferric chloride (FeCl3).
[0048] Processing process:
[0049] Ammonium persulfate treatment: 10 g of plasma-treated polyamide fiber was immersed in 500 ml of 0.1 M APS solution for 25-35 min at a temperature of 45-55 ° C. After treatment, the fiber was thoroughly washed with deionized water to remove the residual APS solution.
[0050] Ferric chloride treatment: The cleaned fibers were transferred to 500 ml of 0.05 M FeCl3 solution for 15-25 minutes at room temperature. After treatment, the fibers were thoroughly washed with deionized water to remove the residual FeCl3 solution and then dried.
[0051] Effect: Double oxidation treatment introduces a large number of hydrophilic functional groups on the fiber surface, increasing the surface polarity and roughness.
[0052] The main function of double oxidation treatment is to introduce hydrophilic functional groups on the surface of polyamide fibers, improve the surface hydrophilicity, biocompatibility and polarity of the fibers, and improve the chemical reaction activity on the fiber surface, thereby enhancing the adhesion of microorganisms and the stability of biofilms. Through this treatment, the roughness and chemical activity of the fiber surface can be significantly increased, providing favorable conditions for microbial biofilm formation, making it more suitable as biofilm filler for biofilters.
[0053] Ammonium persulfate (APS) oxidation treatment: Ammonium persulfate decomposes under heating conditions to produce sulfate radicals (SO4 - ), these free radicals have strong oxidizing properties and can react with the chemical bonds on the surface of polyamide fibers to generate polar functional groups hydroxyl (-OH), carbonyl (=O) and carboxyl (-COOH). Reaction process: APS→2SO4· - +H2O2+H+;SO4· - +R-CH2-CH2-R'→R-CH·-CH2-R'+SO4 2- ; R-CH·-CH2-R'+O2→R-CH(OH)-CH2-R' (generating hydroxyl group); R-CH·-CH2-R'→R-CH=CH-R' (generating carbonyl group and carboxyl group).
[0054] Ferric chloride (FeCl3) oxidation treatment: Ferric chloride is a strong oxidant that can react with organic molecules on the fiber surface to further introduce more polar functional groups. FeCl3 hydrolyzes in aqueous solution to generate Fe(OH)3 and releases H + , can react with the alkaline sites on the fiber surface to generate oxygen-containing functional groups. Reaction process: FeCl3+3H2O→Fe(OH)3+3HCl; Fe(OH)3→Fe 3+ +3OH - ;Fe 3+ +R-CH2-CH2-R'→R-CH·-CH2-R'+Fe 2+ ; R-CH·-CH2-R'+H2O→R-CH(OH)-CH2-R' (generating hydroxyl group).
[0055] Through the above two-step treatment, the hydrophilicity and polarity of the fiber surface can be significantly increased, making it more suitable for the attachment and growth of microorganisms.
[0056] In addition to ammonium persulfate (APS) and ferric chloride (FeCl3), the present invention can also use the following reagents for similar dual oxidation treatment:
[0057] Combination of potassium permanganate (KMnO4) and sulfuric acid (H2SO4): Potassium permanganate is a strong oxidant that can oxidize the chemical bonds on the fiber surface under acidic conditions to generate polar functional groups hydroxyl and carboxyl. Sulfuric acid provides an acidic environment to enhance the oxidizing ability of potassium permanganate.
[0058] Specific steps:
[0059] Prepare potassium permanganate solution: Prepare 0.01-0.05 M KMnO4 aqueous solution in a reaction vessel.
[0060] Add sulfuric acid: Slowly add concentrated sulfuric acid to the KMnO4 solution, control the sulfuric acid concentration to 0.1-0.5M, and maintain an acidic environment.
[0061] Soaking the fiber: Soak the pretreated polyamide fiber sample in the mixed solution for 30-60 minutes at a temperature of 40-50°C.
[0062] Cleaning: After treatment, wash the fiber thoroughly with deionized water to remove residual KMnO4 and H2SO4 solutions and ensure a clean surface.
[0063] Drying: Dry the fiber at 60°C and prepare it for the next step of processing.
[0064] result:
[0065] Under acidic conditions, KMnO4 oxidizes the fiber surface to form hydroxyl (-OH) and carboxyl (-COOH), enhancing the hydrophilicity and biocompatibility of the fiber.
[0066] Combination of ozone (O3) and hydrogen peroxide (H2O2): Ozone has strong oxidizing properties and can directly undergo a series of oxidation reactions with the fiber surface to generate peroxides, =O and ozone compounds. Hydrogen peroxide, as an auxiliary oxidant, can synergize with ozone to further enhance the oxidation effect, produce a large number of hydroxyl groups and COOH, greatly increase the hydrophilicity and biocompatibility of the fiber, and improve the chemical reaction activity of the fiber surface. In particular, the introduction of functional groups makes the fiber more likely to react with microorganisms or other chemicals, thereby improving the stability and adhesion of the biofilm. The oxidation reaction of ozone and hydrogen peroxide will remove or oxidize part of the fiber surface material, making the surface rougher, thereby increasing the microbial attachment points. The oxidation effect in this process is to physically change the surface morphology and provide favorable conditions for microbial biofilm formation. The oxidation reaction can not only modify the fiber surface, but also remove the original hydrophobic pollutants (such as surface grease or organic compounds), thereby making the fiber surface cleaner and more suitable for the formation of biofilms.
[0067] Specific steps:
[0068] Ozone treatment:
[0069] The fiber sample was placed in an ozone generator with an ozone concentration of 5-10 ppm. The reaction time was controlled at 15-30 minutes and the temperature was maintained at 25°C (room temperature).
[0070] Hydrogen Peroxide Treatment:
[0071] Take out the ozone treated fiber and immediately soak it in 0.1-0.5M H2O2 solution. The reaction time is 20-40 minutes and the temperature is controlled at 30-40°C.
[0072] Washing and drying:
[0073] Rinse the fibers with deionized water to remove any residual hydrogen peroxide.
[0074] The fibers were dried at 60°C.
[0075] Peroxide: When ozone reacts with organic molecules on the fiber surface, peroxides (ROO-R') are generated. These peroxides have active oxygen and can further participate in the reaction.
[0076] Hydroxyl (-OH, R-CH2-CH2-R'+O3→R-CH(OH)-CH2-R'): The reaction of ozone and hydrogen peroxide can destroy the CH bond on the fiber surface, introduce polar functional group hydroxyl, and increase the hydrophilicity of the fiber. Carboxyl (-COOH, R-CH2-CH2-R'+O3→R-COOH+O2): Ozone and hydrogen peroxide can oxidize the carbon chain on the surface of organic materials to generate carboxyl. This type of functional group has a strong polarity and can further improve the hydrophilicity and surface energy of the fiber.
[0077] Carbonyl (=O): The strong oxidizing property of ozone can convert carbon-hydrogen bonds (CH) on the fiber surface into carbonyl functional groups (C=O), thereby increasing the chemical reactivity of the surface.
[0078] Ozone compounds: Ozone can react with unsaturated carbon chains (such as C=C) to form ozone compounds (such as ozone rings), which can further decompose into oxidation products.
[0079] Combination of benzoyl peroxide (BPO) and silver nitrate (AgNO3): Benzoyl peroxide is an organic peroxide that can decompose under heat or light to generate free radicals, which react with organic molecules on the fiber surface to produce an oxidation reaction. As an auxiliary oxidant, silver nitrate can synergize with free radicals to introduce hydroxyl and carboxyl groups to the fiber surface, further improving the hydrophilicity and biocompatibility of the fiber.
[0080] Specific steps:
[0081] Benzoyl Peroxide Treatment:
[0082] The fibers were immersed in a 0.05-0.2 M BPO solution at room temperature (25°C).
[0083] Use ultraviolet light or heat to 60-80°C to stimulate the decomposition of BPO, and the reaction time is 20-30 minutes.
[0084] Silver nitrate treatment:
[0085] The BPO treated fibers were transferred to a 0.01-0.05M AgNO3 solution for 15-25 minutes. + ) work synergistically with free radicals to further enhance the oxidation of the fiber surface.
[0086] Washing and drying:
[0087] After treatment, the fibers were immediately rinsed with deionized water to remove residual AgNO3 and BPO.
[0088] The fibers were dried at 60°C.
[0089] Ammonium persulfate (APS) and ferric chloride (FeCl3) have relatively good safety and environmental protection, so this solution is selected in the subsequent examples.
[0090] Step 3. Functionalized coating
[0091] 3.1 Chitosan coating
[0092] Type: Medium molecular weight chitosan, with a degree of deacetylation of 80% and a molecular weight range of 50,000-190,000Da.
[0093] Solution preparation: prepare a chitosan solution with a mass percentage of 1.5-2.5%, add 0.5 mass% acetic acid solution to adjust the pH to 4.3-4.7, and obtain a mixed solution a.
[0094] Coating treatment: The chemically modified polyamide fiber is immersed in the mixed solution a for 45-75 minutes, the weight ratio of the chitosan solution to the fiber is (5-10):1, the chitosan is coated on the polyamide fiber, and then dried in a hot air drying oven at 60°C for 30 minutes.
[0095] 3.2 Sodium alginate coating
[0096] Type: High purity (eg 99%) sodium alginate, viscosity 200-800mPa.s.
[0097] Solution preparation: prepare a sodium alginate solution with a mass percentage of 1.5-2.5%, add acetic acid solution with a mass percentage of 0.5% to adjust the pH to 7.0, and obtain a mixed solution b.
[0098] Coating treatment: The chitosan-coated fiber was immersed in the mixed solution b for 45-75 min, the weight ratio of the sodium alginate solution to the fiber was (5-10):1, and then dried in a hot air drying oven at 60° C. for 30 min.
[0099] Synergistic effect of chitosan and sodium alginate coating
[0100] Synergistic mechanism: Chitosan coating and sodium alginate coating can form a complementary coating structure. Chitosan has good antibacterial and biocompatibility, and can promote the attachment and growth of microorganisms; sodium alginate can form a stable gel network structure, improving the mechanical strength and stability of the coating. The combination of the two can provide more attachment points and a good environment, significantly enhancing the fixation of microorganisms and the stability of biofilms.
[0101] Effect verification: In the experiment, the coating combination of chitosan and sodium alginate significantly increased the amount of microbial attachment and biofilm stability compared to using chitosan or sodium alginate coating alone, and the treatment effect was better.
[0102] Implementation cases and control cases
[0103] Implementation Cases
[0104] Step 1. Surface plasma treatment
[0105] PA6 was selected, and the processing parameters of the low-temperature atmospheric pressure plasma discharge equipment were: power of 100 W, processing time of 15 minutes, and gas flow rate of 10 L / min. After the treatment, the fiber sample was taken out and washed with deionized water to remove the residual reactants.
[0106] Step 2. Chemical modification
[0107] Ammonium persulfate treatment: 10 g of plasma-treated polyamide fiber was immersed in 500 ml of 0.1 M APS solution for 30 min at 50 ° C. After treatment, the fiber was thoroughly washed with deionized water to remove the residual APS solution.
[0108] Ferric chloride treatment: The cleaned fibers were transferred to 500 ml of 0.05 M FeCl3 solution for 20 min at room temperature. After treatment, the fibers were thoroughly washed with deionized water to remove the residual FeCl3 solution.
[0109] Step 3. Functionalized coating
[0110] 3.1 Chitosan coating
[0111] The deacetylation degree is 80%, and the molecular weight range is 50,000-190,000Da. The deacetylation degree is 80%, and the molecular weight range is 50,000-190,000Da. A chitosan solution with a mass percentage of 2% is prepared, and a 0.5% acetic acid solution is added to adjust the pH to 4.5 to obtain a mixed solution a. The chemically modified polyamide fiber is immersed in the mixed solution a for 60 minutes, the volume ratio of the chitosan solution to the fiber is 8:1, and the chitosan is coated on the polyamide fiber, and then dried in a hot air drying oven at 60°C for 30 minutes.
[0112] 3.2 Sodium alginate coating
[0113] Sodium alginate with a purity of 99% and a viscosity of 200-800 mPa.s. A sodium alginate solution with a mass percentage of 2% was prepared, and a 0.5% acetic acid solution was added to adjust the pH to 7.0 to obtain a mixed solution b. The chitosan-coated fiber was immersed in the mixed solution b for 60 minutes, the weight ratio of the sodium alginate solution to the fiber was 8:1, and then dried in a hot air drying oven at 60°C for 30 minutes.
[0114] In the experiment of treating difficult-to-degrade organic wastewater, the polyamide-based composite fiber that had undergone the above-mentioned modification was used as the biofilm filler of the anaerobic biofilter, and the operating conditions were: wastewater flow rate: 500 mL / h; biofilm formation time: 2 weeks; and operating time: 8 weeks.
[0115] The treatment results are as follows: COD removal rate: more than 85%; BOD (biochemical oxygen demand) removal rate: more than 90%; ammonia nitrogen removal rate: 75%; total phosphorus removal rate: 70%; microbial attachment: 1500 CFU / cm 2 ; Biofilm thickness: 600μm.
[0116] Biofilm experiments and the construction and operation of anaerobic biofilters, with detailed descriptions of relevant conditions
[0117] Water sample preparation:
[0118] The water sample used in the treatment is the pre-biochemical wastewater after distillation and dephenolization of coking wastewater.
[0119] Filter media preparation:
[0120] Modified polyamide fiber (PA6) and traditional fiber filter materials were selected as control groups.
[0121] The modified polyamide fibers were plasma treated and double oxidized and coated with chitosan and sodium alginate.
[0122] Film formation steps:
[0123] Cut the treated fiber samples into small pieces (about 5-10 cm) suitable for the size of the biofilter. Evenly distribute the fiber samples in the biofilter, ensuring that there is enough space between the fiber samples to facilitate water flow and microbial attachment.
[0124] Reactor design
[0125] Reactor size: Taking the treatment scale of 500mL / h and hydraulic retention time (HRT) of 12 hours as an example, calculate the total volume: Total volume = treatment scale × hydraulic retention time = 500mL / h × 12h = 6000mL = 6L. Length: 20cm; Width: 10cm; Height: 30cm; Total volume: 20cm × 10cm × 30cm = 6000cm 3 =6L
[0126] Use corrosion-resistant stainless steel or high-density polyethylene (HDPE) as the reactor material to ensure the durability and corrosion resistance of the reactor.
[0127] Water inlet and outlet system
[0128] Water inlet: Installed at the bottom of the reactor to ensure that water flows through the filter material from bottom to top.
[0129] Water outlet: Installed on the top of the reactor to prevent excessive accumulation of biofilm and affect the treatment effect.
[0130] Water inlet pipe: Install flow meter and regulating valve to control the water sample flow.
[0131] Water outlet pipe: Set an overflow port to ensure a constant water level.
[0132] Filter material filling: Select modified polyamide fiber and evenly distribute it in the reactor. The filter material layer thickness is about 20cm. The support grid is set above the filter material layer to prevent the filter material from losing.
[0133] Operating conditions
[0134] Water sample flow rate:
[0135] The treatment scale is 500mL / h and the water inlet flow rate is stable.
[0136] Hydraulic retention time (HRT): HRT = total volume / treatment scale = 6L / 0.5L / h = 12 hours. The temperature is maintained at 25-30°C (or room temperature). The pH value is maintained in the range of 5.5-7.0 and adjusted by adding common acids or bases according to the corresponding standards.
[0137] The total running time is 8 weeks.
[0138] Start-up phase: Conduct a clean water test run to ensure that the system has no leakage or blockage. Gradually introduce pre-biochemical wastewater after distillation and dephenolization of coking wastewater, and gradually increase the water sample flow rate to avoid excessive microbial shock load.
[0139] Normal operation stage:
[0140] Water sample flow rate: maintained at 500mL / h. Temperature: 25-30℃ (or room temperature). pH value maintained at 5.5-7.0. HRT: 12 hours.
[0141] Monitoring and maintenance: Samples were taken every 3 days and the microbial attachment on the fiber surface was observed using a scanning electron microscope (SEM). The colony forming units (CFU / cm 2 ) counting method to quantitatively analyze the amount of microbial attachment. Record the biofilm thickness. Regularly monitor the effluent water quality indicators, including COD, BOD, ammonia nitrogen and total phosphorus concentrations. Check the inlet and outlet water systems weekly to ensure normal operation.
[0142] Comparative Case 1
[0143] Using unmodified PA6 polyamide fiber as biofilter filler, the operating conditions are the same. The treatment results are as follows: COD removal rate: about 60%; BOD removal rate: 65%; ammonia nitrogen removal rate: 50%; total phosphorus removal rate: 45%; microbial attachment: 800 CFU / cm 2 ; Biofilm thickness: 300μm.
[0144] Comparative case 2:
[0145] The conventional polypropylene fiber filter material was used as the biofilter biofilm filler, and the operating conditions were the same as those in the implementation case. The treatment results were as follows: COD removal rate: about 55%; BOD removal rate: 60%; ammonia nitrogen removal rate: 45%; total phosphorus removal rate: 40%; microbial attachment: 700 CFU / cm 2 ; Biofilm thickness: 250μm.
[0146] Figure 4 This is a picture of the biofilm growth taken by a scanning electron microscope two weeks after the biofilm was formed in the implementation case. From the picture, we can see the biofilm growth of the modified polyamide fiber two weeks after the biofilm was formed. The biofilm is evenly distributed on the fiber surface, the film layer is continuous and dense, there is obvious microbial community attached to the surface, the fiber structure is covered by the biofilm more thoroughly, and there is no obvious peeling or defect phenomenon. The surface of the fiber has been modified to effectively promote the attachment of microorganisms and form a stable, dense and thick biofilm. Figure 1 It can be seen that the photos based on 3D reconstruction observation of laser confocal optical microscopy show that the thickness of the biofilm in this case is significantly thicker than in other cases.
[0147] Figure 5 This is a picture of biofilm growth taken by scanning electron microscope two weeks after biofilm formation in case 1. From the picture, we can see that the biofilm is unevenly distributed on the fiber surface, and some areas are incompletely attached. The biofilm structure is loose, and some areas show sparse microbial attachment, and the integrity of the film layer is poor. Unmodified polyamide fiber has low hydrophilicity, weak microbial adhesion, and unstable and thin biofilm formation. Figure 2 It can be seen that the film thickness is significantly lower than that of the implementation case, and the film-forming effect is obviously not as good as the modified fiber.
[0148] Figure 6 This is a picture of biofilm growth taken by scanning electron microscope two weeks after biofilm formation in case 2. From the picture, we can see that the biofilm on the fiber surface is relatively thin, the film structure is relatively loose, unevenly distributed, the density of microbial attachment is low, and almost no effective film layer is formed in some areas. Traditional polypropylene fiber filter materials have poor mechanical strength and hydrophilicity, resulting in low biofilm formation efficiency and poor microbial adhesion. Figure 3 It can be seen that the biofilm thickness is significantly smaller than Figure 2 and Figure 3 , the effect is not as good as polyamide fiber.
[0149] Detailed product performance test comparison data
[0150]
[0151] The required parameters are determined as follows:
[0152] Biofilm stability determination method:
[0153] The filter material after biofilm formation is placed in a nutrient solution with microbial growth, the filter material is weighed every 48 hours, and the biofilm growth morphology of the filter material is observed using a laser confocal microscope to determine the biofilm stability of the filter material. Biofilm stability is a key feature to measure whether the filter material can form a long-lasting, highly adhesive and non-detachable biofilm during use. The following is a description of the specific results of the improvement of biofilm stability in control cases 1 and 2 and the implementation case:
[0154] Implementation case (modified polyamide fiber):
[0155] Biofilm stability: High
[0156] reason:
[0157] The modified polyamide fiber is treated with plasma, chemically oxidized, and coated with chitosan and sodium alginate to greatly enhance the hydrophilicity and surface energy of the fiber. A large number of polar functional groups (such as hydroxyl and carboxyl) are introduced on the fiber surface, making it easier for microorganisms to attach and form a stable biofilm.
[0158] After modification, the microbial attachment reached 1500 CFU / cm 2 , the biofilm thickness is 600μm, which indicates that the microorganisms have formed a thick and dense film layer on the surface of the filter material, which can resist external conditions such as water flow impact.
[0159] The biofilm showed high stability throughout the entire operation cycle, with no film peeling or separation. The biofilm was able to maintain its degradation ability and structural integrity for a long time.
[0160] Comparative case 1 (unmodified polyamide fiber, PA6):
[0161] Biofilm stability: Low
[0162] reason:
[0163] The unmodified PA6 fiber surface has poor hydrophilicity and lacks polar functional groups, so the adhesion of microorganisms is weak. Therefore, although the biofilm can be formed to a certain extent, the film layer is thin and the adhesion is not strong, and it is easy to fall off due to water impact or external interference.
[0164] Microbial attachment is 800 CFU / cm 2 , the biofilm thickness is 300 μm, indicating that the growth of microorganisms on the fiber surface is limited, the formed film layer is relatively sparse, and the structure is not stable enough.
[0165] During actual operation, biofilms often peel off and have poor stability, resulting in unstable treatment efficiency.
[0166] Comparative case 2 (traditional polypropylene fiber filter material):
[0167] Biofilm stability: Low
[0168] reason:
[0169] Traditional polypropylene fiber filter media has low mechanical strength, insufficient hydrophilicity and surface energy, and the adhesion of microorganisms on its surface is very limited. Although a certain amount of biofilm can be formed, the film layer is very thin and easily falls off during operation.
[0170] The amount of microbial attachment is only 700 CFU / cm 2 , the biofilm thickness was 250 μm, indicating that the microbial activity on the fiber surface was low and the biofilm structure was loose and unstable.
[0171] The biofilm of this filter material is easily affected by water flow and operating conditions, and the membrane layer is easily damaged, resulting in unstable performance of the filter material during long-term use.
[0172] The stability of the biofilm in the implementation case was significantly improved. This is because the surface modification of the modified polyamide fiber significantly improved the hydrophilicity and biocompatibility of the fiber surface, allowing microorganisms to quickly attach and form a thicker and more stable biofilm, which was manifested by a higher microbial attachment amount (1500 CFU / cm 2 ) and biofilm thickness (600μm). In control cases 1 and 2, the unmodified fibers and traditional fibers had poor hydrophilicity, which made it difficult for microorganisms to attach, and the biofilm formation was uneven and unstable, especially when they were impacted by water flow or during operation, which affected the continuous degradation ability of the biofilm. The modified polyamide fiber significantly improved the stability of the biofilm, and the microorganisms were able to firmly attach to the fiber surface to form a stable, dense and thick biofilm. This is very important for the long-term stable operation of the anaerobic biofilter. The filter media in control cases 1 and 2 showed poor biofilm stability because they were not modified, and the biofilm was easy to fall off or be destroyed, which affected the treatment effect of the entire filter.
[0173] COD value determination method:
[0174] The COD value is determined by potassium dichromate oxidation microwave digestion titration according to the national standard GB11914-89. 5.00mL of 0.0250mol / L potassium dichromate solution is added to the water sample, and silver salt is used as a catalyst under the action of a strong acid medium (sulphuric acid). After boiling and refluxing, 3 drops of ferrous acid indicator are added, and the unreduced potassium dichromate in the water sample is titrated with ammonium ferrous sulfate with a concentration of 0.005mol / L. The mass concentration of consumed oxygen is calculated from the amount of consumed potassium dichromate, and the COD determination result is obtained.
[0175] BOD value determination method:
[0176] Fill the water sample into a completely sealed dissolved oxygen bottle and culture it in a dark place at (20±1)℃ for 5d±4h. Use a dissolved oxygen meter to measure the mass concentration of dissolved oxygen in the water sample before and after culture. Calculate the amount of dissolved oxygen consumed per liter of sample based on the difference in mass concentration of dissolved oxygen before and after culture, and get the BOD measurement result.
[0177] Ammonia nitrogen value determination method:
[0178] Ammonia nitrogen value is measured by Nessler's reagent photometry. Dilute sulfuric acid solution is used to absorb ammonia in the air, and the generated ammonium ions react with Nessler's reagent to form a yellow-brown complex. The absorbance of the complex is proportional to the ammonia content. The absorbance is measured at a wavelength of 420nm, and the content in the air is calculated based on the absorbance.
[0179] Total phosphorus determination method:
[0180] The total phosphorus value is determined by potassium persulfate digestion method - molybdenum antimony anti-spectrophotometry. The sample is melted with sodium hydroxide under high temperature conditions to convert all phosphorus-containing minerals and organic phosphorus compounds into soluble orthophosphates, which react with molybdenum antimony anti-color developer under acidic conditions to generate phosphomolybdenum blue, and the absorbance is measured at a wavelength of 700nm. Within a certain concentration range, the total phosphorus content and absorbance values conform to the Lambert-Beer law.
[0181] Microbial attachment determination method:
[0182] The amount of microorganisms attached to the filter material was measured by plate count method, and the value was expressed as CFU / cm 2 .
[0183] Biofilm thickness determination method:
[0184] The thickness of biofilm on the filter material was measured using a laser confocal microscope and the quantity was expressed in μm.
[0185] Method for determining the mechanical strength of filter media:
[0186] The mechanical strength of the filter material is measured using a Roell Z 010 universal testing machine, and the strength is divided into three levels: high, medium and low.
Claims
1. A method for preparing a polyamide fiber filter material for an anaerobic biofilter, characterized in that: The steps include: S1, subjecting the polyamide fiber to surface plasma treatment at a power of 90-110 W, and then cleaning the residual reactants to obtain the plasma-treated polyamide fiber; S2, oxidizing the polyamide fiber after the plasma treatment with a main oxidant and an auxiliary oxidant, wherein when the main oxidant is ammonium persulfate, the auxiliary oxidant is ferric chloride, when the main oxidant is potassium permanganate, the auxiliary oxidant is sulfuric acid, when the main oxidant is ozone, the auxiliary oxidant is hydrogen peroxide, when the main oxidant is benzoyl peroxide, the auxiliary oxidant is silver nitrate, to obtain an oxidized polyamide fiber; S3, sequentially coating chitosan coating and sodium alginate coating on the oxidized polyamide fiber, the mass ratio of chitosan, sodium alginate and the polyamide fiber treated with plasma in S1 is (0.075-0.25):(0.075-0.25):1, and obtaining a polyamide fiber filter material for an anaerobic biofilter.
2. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: The polyamide fiber type described in S1 is PA6.
3. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: In S1, the polyamide fiber is treated at a power of 90-110 W for 12-18 min, and the gas flow rate for generating plasma is 8-12 L / min.
4. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: When the main oxidant is ammonium persulfate and the auxiliary oxidant is ferric chloride, the oxidation treatment described in S2 is carried out as follows: The plasma-treated polyamide fiber obtained in S1 is immersed in a 0.1M ammonium persulfate solution at 45-55°C for 25-35 minutes, then the obtained polyamide fiber is washed, and then immersed in a 0.05M ferric chloride solution for 15-25 minutes, then washed and dried to obtain an oxidized polyamide fiber.
5. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: When the main oxidant is potassium permanganate and the auxiliary oxidant is sulfuric acid, the oxidation treatment described in S2 is carried out as follows: Sulfuric acid with a concentration of 0.1-0.5 M is added to a 0.01-0.05 M potassium permanganate solution to obtain a mixed solution, and then the plasma-treated polyamide fiber obtained in S1 is immersed in the mixed solution at 40-50° C. for 30-60 min, and then washed and dried to obtain oxidized polyamide fiber.
6. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: When the primary oxidant is ozone and the auxiliary oxidant is hydrogen peroxide, the oxidation treatment described in S2 is carried out as follows: The plasma-treated polyamide fiber obtained in S1 is placed in an ozone environment with a concentration of 5-10 ppm for 15-30 minutes, then immersed in a 0.1-0.5 M 30-40° C. hydrogen peroxide solution for 20-40 minutes, then washed and dried to obtain an oxidized polyamide fiber.
7. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: When the primary oxidant is benzoyl peroxide and the auxiliary oxidant is silver nitrate, the oxidation treatment described in S2 is carried out as follows: The plasma-treated polyamide fiber obtained in S1 is immersed in a 0.05-0.2M benzoyl peroxide solution, and then ultraviolet light or heating to 60-80°C is used to stimulate the decomposition of benzoyl peroxide for 20-30 minutes. The obtained polyamide fiber is then immersed in a 0.01-0.05M silver nitrate solution for 15-25 minutes, and then washed and dried to obtain an oxidized polyamide fiber.
8. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 1, characterized in that: S3 sequentially coats chitosan coating and sodium alginate coating on oxidized polyamide fibers through the following process: The pH values of chitosan solution and sodium alginate solution, both of which are 1.5%-2.5% by mass, are adjusted to 4.3-4.7 and 7.0, respectively, to obtain mixed solution a and mixed solution b. The oxidized polyamide fiber obtained by S2 is immersed in the mixed solution a, then dried, immersed in the mixed solution b, and finally dried to obtain a polyamide fiber filter material for an anaerobic biofilter.
9. The method for preparing a polyamide fiber filter material for an anaerobic biofilter according to claim 8, characterized in that: The deacetylation degree of chitosan is 80%, the molecular weight range is 50,000-190,000Da, the viscosity of sodium alginate is 200-800mPa.s, and the polyamide fiber is immersed in the mixed solution a for 45-75min, then immersed in the mixed solution b for 45-75min, and then dried.
10. A polyamide fiber filter material obtained by the method for preparing a polyamide fiber filter material for an anaerobic biofilter according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for surface modification of basalt fibre carrier for purifying water quality
CN102887585A
Preparation method and application of basalt fiber surface modified coating
CN107640913A
Functional polysaccharide antimicrobial modified natural fiber and preparation method thereof
CN107869048A
Preparation method of hydrophilic chitosan modified basalt fiber support
CN108330686A
Method for promoting biofilm culturing effect by modifying surface of polyurethane
CN111100321A