A ceramic roller and its preparation method and application
By introducing an intermediate layer into the alumina ceramic roller, the glass liquid phase and mullite crystal structure are used to enhance the bonding strength, solving the problems of alumina ceramic coating shedding and insufficient performance, and improving the wear resistance and performance of the ceramic roller. Thermal shock resistance for high temperature thick coating applications.
Patent Information
- Application Number
- CN202410931125.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-12
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of rollers, and in particular to a ceramic roller and a preparation method and application thereof. Background Art
[0002] Alumina ceramic rollers have good oxidation resistance, mechanical strength, thermal stability and wear resistance, etc., and the raw material source is wide and the production cost is low. They are widely used in the support and rolling devices of roller kilns. By forming a special protective coating (such as silicate coating, carbide coating, nitride coating, aluminum oxide coating, etc.) on the surface of alumina ceramic rollers, additional thermal isolation and wear protection can be provided to reduce the thermal stress and uneven wear of sintered products caused by rapid temperature changes when they are used in roller kilns, and expand their further application in high-load ceramic product roller kilns. However, the heat resistance of silicate, carbide, nitride and other coatings is only 1200℃~1400℃. They have good performance when used in the low temperature range, but when the temperature is higher than the heat resistance temperature, the coating will soften and melt and fall off, limiting its high-temperature application. Alumina ceramic coating and alumina ceramic roller have similar components, similar thermal expansion coefficients and high temperature resistance. When the coating is thin, it is not easy to fall off during the application of roller kiln, which can play a certain protective role. However, the thermal shock resistance and wear resistance of thin alumina ceramic coating are generally not enough to meet the needs of existing production. Therefore, it is necessary to develop a technology that makes the alumina ceramic roller not easy to fall off during the preparation process and the application process in the roller kiln even if the alumina ceramic coating is thick. Summary of the invention
[0003] The purpose of the present application is to overcome the deficiencies of the above-mentioned prior art and to provide a ceramic roller and a preparation method and application thereof, so that even if the alumina ceramic roller has a thicker alumina ceramic coating, the alumina ceramic coating is not easy to fall off during the preparation process and the application process in the roller kiln.
[0004] To achieve the above-mentioned purpose, the technical solution adopted by the present application is: a ceramic roller, which includes an alumina ceramic inner layer, an intermediate layer and an alumina ceramic outer layer connected in sequence from the inside to the outside, wherein the intermediate layer is mainly prepared from the following raw materials in parts by weight:
[0005] 43~77 parts of alumina powder,
[0006] 10~30 parts of aluminum sol,
[0007] 10~30 parts of kaolin,
[0008] Dispersant 5~15 parts,
[0009] 15~35 parts of solvent.
[0010] The intermediate layer has the following functions: first, during the high-temperature sintering process, a glass liquid phase is generated, which penetrates into the pores on the surface of the inner layer and the outer layer of the alumina ceramic, thereby enhancing the bonding strength between the inner and outer layers of the alumina ceramic; second, it has similar components to the inner and outer layers of the alumina ceramic, and has a similar thermal expansion coefficient. During high-temperature co-sintering and use in a high-temperature roller kiln, the layers are not easy to fall off, thereby ensuring that the inner and outer layers of the alumina ceramic have a high bonding strength; third, the alumina micropowder and aluminum sol used with kaolin will form columnar and / or needle-shaped mullite crystals during the high-temperature sintering process. The mullite crystals are staggered to form a solid mesh skeleton, which can well buffer the extrusion force.
[0011] The ceramic roller can effectively prevent the outer layer of the alumina ceramic from falling off during the preparation process and when used in a high-temperature roller kiln by arranging an intermediate layer prepared with a specific formula between the inner and outer layers of the alumina ceramic. The obtained ceramic roller is suitable for both the case where the outer layer of the alumina ceramic is thinner and the case where the outer layer of the alumina ceramic is thicker (such as the case where the thickness of the outer layer of the alumina ceramic is above 15 mm, specifically 15 mm, 20 mm, 25 mm, 30 mm or 35 mm, etc.); when the ceramic roller is used in the case where the outer layer of the alumina ceramic is thicker, the wear resistance and thermal shock resistance are better.
[0012] The amounts of alumina powder, aluminum sol, kaolin, dispersant and solvent in the raw materials for preparing the intermediate layer should be controlled within the above-mentioned specific range to make it easy to coat while having a higher bonding strength between the inner and outer layers of the alumina ceramic and a higher flexural strength of the roller.
[0013] The middle layer uses aluminum sol as a binder. On the one hand, it is not easy to decompose during the sintering process, ensuring that the inner and outer layers have a strong bonding force. On the other hand, it lays the foundation for the layer to have a similar thermal expansion coefficient to the inner and outer layers.
[0014] In the raw materials for preparing the intermediate layer, the aluminum oxide powder is 43 to 77 parts, such as 43, 45, 50, 55, 60, 65, 70, 75 or 77 parts by weight;
[0015] The aluminum sol is 10 to 30 parts by weight, such as 10, 12, 15, 18, 20, 23, 25, 27 or 30 parts by weight;
[0016] 10 to 30 parts by weight of kaolin, such as 10, 12, 15, 18, 20, 23, 25, 27 or 30 parts by weight;
[0017] The dispersant is 5 to 15 parts by weight, such as 5, 7, 9, 10, 12, 14 or 15 parts by weight;
[0018] The solvent is 15 to 35 parts by weight, such as 15, 18, 20, 23, 25, 27, 30, 33 or 35 parts by weight.
[0019] Preferably, in the raw material for preparing the intermediate layer, the mass ratio of alumina powder to kaolin is (2.9-7.1): 1. When the mass ratio of alumina powder to kaolin in the raw material for preparing the intermediate layer is in the range of (2.9-7.1): 1, such as 2.9: 1, 3: 1, 4: 1, 5: 1, 6: 1, 7: 1 or 7.1: 1, the bonding strength between the inner and outer layers of the alumina ceramic is higher, and the flexural strength of the roller is higher.
[0020] In the raw materials for preparing the intermediate layer, the weight of alumina powder is more than 29% of the total weight of the raw materials for preparing the intermediate layer, such as 29%, 30%, 32%, 35%, 37%, 40%, 42%, 45%, 47%, 50%, 52%, 55%, 57%, 60%, 62%, 65% or 67%.
[0021] Preferably, the alumina ceramic inner layer is mainly prepared from the following raw materials in parts by weight:
[0022] 50~70 parts of alumina powder,
[0023] 10~30 parts of kaolin,
[0024] 28~52 parts of corundum sand,
[0025] 1~5 parts of binder,
[0026] 15~35 parts of solvent.
[0027] The above formula is used to prepare the inner layer of alumina ceramics, which is not only more conducive to the formation of columnar and / or needle-shaped mullite crystals by alumina micropowder and kaolin during high-temperature sintering, so that it can better buffer the extrusion force, but also produces a liquid phase at high temperature, has adhesion, and avoids the occurrence of rod falling during the hanging firing process. The amount of alumina micropowder can be selected as 50, 52, 55, 58, 60, 63, 65, 68 or 70 parts by weight; the amount of kaolin can be selected as 10, 12, 15, 18, 20, 23, 25, 27 or 30 parts by weight; the amount of corundum sand can be selected as 28, 30, 33, 35, 37, 40, 43, 45, 47, 50 or 52 parts by weight; the amount of binder can be selected as 1, 2, 3, 4 or 5 parts by weight; the amount of solvent can be selected as 15, 18, 20, 23, 25, 27, 30, 33 or 35 parts by weight.
[0028] Preferably, in the raw material for preparing the inner layer of the alumina ceramic, the mass ratio of alumina powder to kaolin is (4.4-6.6): 1. When the mass ratio of alumina powder to kaolin in the raw material for preparing the inner layer of the alumina ceramic is in the range of (4.4-6.6): 1, such as 4.4: 1, 4.5: 1, 5: 1, 5.5: 1, 6: 1, 6.5: 1 or 6.6: 1, the bearing capacity of the inner layer of the alumina ceramic is higher.
[0029] Among the raw materials for preparing the alumina ceramic inner layer, the weight of corundum sand is more than 15% of the total weight of the raw materials for preparing the alumina ceramic inner layer, such as 15%, 18%, 20%, 23%, 25%, 27%, 30%, 32%, 35%, 37%, 40%, 42%, 45%, 47%, 50%, 52% or 55%.
[0030] The common corundum-mullite ceramic rollers on the market have a low volume density of about 2.9g / cm 3 ; And the apparent porosity is relatively high, at 15-20%, which results in unsatisfactory effects when used in high-corrosion and high-load fields such as sodium-lithium batteries, short service life, and a general service life of 5-7 days. Frequent replacement of rollers will inevitably reduce production efficiency. Traditional corundum-mullite alumina ceramic rollers need to be added with high-temperature clay during the preparation process, resulting in the introduction of more metal oxides such as MgO, CaO, K2O and Na2O. These metal oxides are easily corroded by acidic electrolytes in the roller kiln for sintering sodium-lithium batteries, which limits their application in the roller kiln for sintering sodium-lithium battery materials.
[0031] Preferably, the alumina ceramic outer layer is mainly prepared from the following raw materials in parts by weight:
[0032] Alumina powder 75~95 parts,
[0033] 1~10 parts of kaolin,
[0034] 28~52 parts of corundum sand,
[0035] 1~5 parts of binder,
[0036] 15~35 parts of solvent. The alumina ceramic outer layer of the above formula reduces the amount of kaolin used to reduce the amount of metal oxides such as MgO, CaO, K2O and Na2O introduced by the addition of kaolin, thereby reducing the adverse effects of these metal oxides on the corrosion resistance of the roller; by increasing the amount of alumina micropowder, the density and corrosion resistance of the roller are improved. The roller made with the above alumina ceramic outer layer formula not only has good mechanical properties, but also has better corrosion resistance, and is more suitable for use in the sintering roller kiln of corrosive materials such as sodium battery materials, lithium battery materials, and carbon fiber. The amount of alumina micropowder can be selected from 75, 77, 80, 82, 85, 87, 90, 92 or 95 parts by weight; the amount of kaolin can be selected from 1, 3, 5, 7, 9 or 10 parts by weight; the amount of corundum sand can be selected from 28, 30, 33, 35, 37, 40, 43, 45, 47, 50 or 52 parts by weight; the amount of binder can be selected from 1, 2, 3, 4 or 5 parts by weight; the amount of solvent can be selected from 15, 18, 20, 23, 25, 27, 30, 33 or 35 parts by weight. In the above-mentioned alumina ceramic outer layer formula, the weight of corundum sand is more than 15% of the total weight of the raw materials for preparing the alumina ceramic outer layer, such as 15%, 17%, 20%, 22%, 25%, 27%, 30%, 32%, 34%, 36%, 38%, 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58% or 60%, etc. More preferably, in the raw materials for preparing the alumina ceramic outer layer, the mass ratio of alumina micropowder to kaolin is (7.9~10.1):1. When the mass ratio of alumina micropowder to kaolin in the raw materials for preparing the alumina ceramic outer layer is in the range of (7.9~10.1):1, such as 7.9:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1 or 10.1:1, the corrosion resistance of the obtained alumina ceramic outer layer is better.
[0037] Preferably, the alumina ceramic outer layer is mainly prepared from the following raw materials in parts by weight:
[0038] 25~45 parts of alumina powder,
[0039] 10~30 parts of kaolin,
[0040] 28~52 parts of corundum sand,
[0041] 1~10 parts of thermal conductivity agent,
[0042] 1~10 parts of toughening agent,
[0043] 1~5 parts of binder,
[0044] 15~35 parts of solvent. The heat transfer agent can disperse the thermal stress concentration and improve the thermal shock resistance; the toughening agent can reduce the crack extension and thermal stress generation caused by thermal shock. When the outer layer of the alumina ceramic is prepared using the above-mentioned specific formula, it has good mechanical properties and better thermal shock resistance, making the roller more suitable for high-temperature and high-load roller kilns, such as daily-use porcelain, sanitary porcelain, architectural porcelain, rare earth calcination and other high-temperature firing belt roller kilns. The amount of alumina micropowder can be selected from 25, 27, 30, 32, 35, 37, 40, 43 or 45 parts by weight; the amount of kaolin can be selected from 10, 12, 15, 18, 20, 23, 25, 27 or 30 parts by weight; the amount of corundum sand can be selected from 28, 30, 33, 35, 37, 40, 43, 45, 47, 50 or 52 parts by weight; the amount of thermal conductivity agent can be selected from 1, 2, 4, 6, 8 or 10 parts by weight; the amount of toughening agent can be selected from 1, 2, 4, 6, 8 or 10 parts by weight; the amount of binder can be selected from 1, 2, 3, 4 or 5 parts by weight; the amount of solvent can be selected from 15, 18, 20, 23, 25, 27, 30, 33 or 35 parts by weight. Preferably, in the above-mentioned alumina ceramic outer layer formula, the weight of corundum sand is more than 15% of the total weight of the raw materials for preparing the alumina ceramic outer layer, such as 15%, 17%, 19.5%, 20%, 22%, 25%, 27%, 30%, 32%, 35%, 33%, 40%, 42%, 45%, 47%, 50%, 52%, 54% or 56%, etc. When the mass ratio of alumina powder to kaolin in the raw materials for preparing the alumina ceramic outer layer is in the range of (1.9~4.1):1, such as 1.9:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or 4.1:1, etc., the thermal shock resistance of the obtained alumina ceramic outer layer is better.
[0045] Preferably, the binders in the raw materials for preparing the inner layer and the outer layer of alumina ceramics independently include at least one of carboxymethyl cellulose, polyvinyl alcohol, phenolic resin, hydroxypropyl methyl cellulose, polyvinyl pyrrolidone and cyclodextrin.
[0046] Preferably, the solvents in the raw materials for preparing the inner layer, the middle layer and the outer layer of alumina ceramics each independently include at least one of water and ethanol.
[0047] Preferably, the dispersant in the raw material for preparing the intermediate layer includes at least one of polyacrylamide, sodium polyacrylate, hydroxymethyl cellulose and polypropylene alcohol.
[0048] Preferably, the thermal conductive agent includes at least one of cordierite and silicon carbide. Preferably, the average particle size of the cordierite is 1-10 μm. Preferably, the average particle size of the silicon carbide is 0.1-2 μm.
[0049] Preferably, the toughening agent comprises at least one of fibers and whiskers, wherein the fibers and whiskers each independently comprise at least one of mullite and zirconia. Preferably, the average particle size of the mullite is 1 to 3 μm. Preferably, the average particle size of the zirconia is 1 to 10 μm.
[0050] Preferably, the average particle size of the alumina powder in the raw materials for preparing the alumina ceramic inner layer, the middle layer and the alumina ceramic outer layer is independently 1 to 10 μm.
[0051] Preferably, the average particle size of the corundum sand in the raw materials for preparing the inner alumina ceramic layer and the outer alumina ceramic layer is independently 5 to 25 μm.
[0052] Preferably, the inner layer of alumina ceramic is in the shape of a hollow tube, and the thickness of the inner layer of alumina ceramic is 1-10 mm;
[0053] And / or, the thickness of the outer layer of alumina ceramic is 15-35 mm;
[0054] And / or, the outer diameter of the inner layer of alumina ceramic is 20-40 mm;
[0055] And / or, the thickness of the intermediate layer is 0.1-1 mm.
[0056] When the thickness of the inner layer of the alumina ceramic is in the range of 1 to 10 mm, and the thickness of the outer layer of the alumina ceramic is in the range of 15 to 35 mm, the roller has better thermal conductivity, and can better avoid the generation of thermal stress caused by rapid temperature changes, and better reduce the risk of cracks and damage under thermal cycling conditions. At the same time, the wear resistance and thermal shock resistance of the obtained roller are better.
[0057] The present application also provides a method for preparing the ceramic roller, which comprises the following steps:
[0058] The raw materials for preparing the inner layer of the alumina ceramic, the raw materials for preparing the middle layer, and the raw materials for preparing the outer layer of the alumina ceramic are mixed and dispersed respectively to obtain the mud material for the inner layer of the alumina ceramic, the coating material for the middle layer, and the mud material for the outer layer of the alumina ceramic;
[0059] The alumina ceramic inner layer mud material is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body;
[0060] The tubular alumina ceramic green body is sequentially subjected to a first drying, a cold isostatic pressing, a second drying, a first sintering and a grinding process to obtain an alumina ceramic inner layer;
[0061] The outer surface of the inner layer of alumina ceramic is coated with the intermediate layer coating to form a tube core, and the outer layer of alumina ceramic is extruded on its outer surface by vertical extrusion to form an outer layer, and then subjected to a third drying and a second sintering treatment in sequence to obtain a ceramic roller.
[0062] A high-strength and dense inner layer of alumina ceramic green body is initially prepared by combining vacuum extrusion and cold isostatic pressing processes; and it is sintered to a certain strength through the first sintering, which is conducive to subsequent sintering. During the third drying and second sintering processes, the inner layer of alumina ceramic has been sintered, so its thermal shrinkage stress is small. During the third drying process, the outer layer of alumina ceramic green body shrinks in volume due to the evaporation of water, the reduction of voids, and the gradual shortening of the distance between particles; during the second sintering process, due to the generation of liquid phase, the voids between particles are filled, and the generation of mullite whiskers, the volume of this layer is further shrunk, which causes the outer layer of alumina ceramic green body to exert an extrusion force on the inner layer, and the stress difference prompts the intermediate layer coating to tighten the inner alumina ceramic outer layer more firmly, thereby better enhancing the bonding strength of the inner and outer layers.
[0063] Preferably, the vacuum degree of the vacuum extrusion process is -0.1~0MPa, and the extrusion force is 10~20kN. Wherein, vacuum degree = absolute atmospheric pressure - atmospheric pressure.
[0064] Preferably, the temperature of the first drying is 60-120° C., and the time of the first drying is 12-48 h.
[0065] Preferably, the cold isostatic pressing pressure is 120-240 MPa, and the cold isostatic pressing time is 1-8 min.
[0066] Preferably, the temperature of the second drying is 50-100° C., and the time of the second drying is 6-12 hours.
[0067] Preferably, the first sintering is hanging sintering, the temperature of the first sintering is 1300-1600° C., and the time of the first sintering is 2-10 h.
[0068] Preferably, when the outer surface of the inner layer of the alumina ceramic is coated with the intermediate layer coating, the number of coating times is 1 to 4 times.
[0069] Preferably, the vertical extrusion pressure is 20-60 MPa.
[0070] Preferably, the temperature of the third drying is 60-100° C., and the time of the third drying is 15-30 h.
[0071] Preferably, the second sintering is hanging sintering, the temperature of the second sintering is 1400-1800° C., and the time of the second sintering is 24-48 h.
[0072] Preferably, the first sintering temperature is 1300-1600°C, and the second sintering temperature is 1400-1800°C, so that the organic matter contained in the green billet can be fully decomposed and the water can be fully volatilized after the first sintering, while retaining some unreacted kaolin and alumina powder, reducing the risk of rod breaking during the second sintering process. In addition, this has lower energy consumption and lower cost.
[0073] The present application also provides the use of the ceramic roller in a roller kiln for sintering at least one of sodium battery materials, lithium battery materials, and carbon fiber, or in a roller kiln for firing at least one of daily-use porcelain, sanitary porcelain, architectural porcelain, and rare earth calcination.
[0074] Compared with the prior art, the beneficial effects of the present application are as follows: the present application can effectively prevent the inner and outer layers of the alumina ceramic from falling off during the preparation process and when used in a high-temperature roller kiln by arranging an intermediate layer prepared with a specific formula between the inner and outer layers of the alumina ceramic of the ceramic roller, so that the obtained ceramic roller is suitable for both the case where the outer layer of the alumina ceramic is thinner and the case where the outer layer of the alumina ceramic is thicker (such as the case where the thickness of the outer layer of the alumina ceramic is above 15 mm, such as 15 mm, 20 mm, 25 mm, 30 mm or 35 mm, etc.); when the ceramic roller of the present application is used in the case where the outer layer of the alumina ceramic is thicker, the wear resistance and thermal shock resistance are better. DETAILED DESCRIPTION
[0075] In order to better illustrate the purpose, technical scheme and advantages of the present application, the present application will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present application in detail, rather than to limit the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. The experimental reagents and instruments involved in the implementation of this application are all commonly used ordinary reagents and instruments unless otherwise specified. In the present application, the technical features described in an open manner include closed technical schemes composed of the listed features, and also include open technical schemes containing the listed features.
[0076] In the following groups of parallel tests, unless otherwise specified, the raw materials used are all the same; the solid content of the aluminum sol used in Examples 1 to 34 and each comparative example is 33%, and the solid content of the aluminum sol used in Examples 35 and 36 is 25% and 40%, respectively.
[0077] Example 1
[0078] An embodiment of the ceramic roller described in the present application. The ceramic roller of this embodiment comprises an alumina ceramic inner layer, a middle layer and an alumina ceramic outer layer connected in sequence from the inside to the outside;
[0079] Among them, the inner layer of alumina ceramic is in the shape of a hollow tube with an outer diameter of 30 mm and a thickness of 5 mm;
[0080] The thickness of the middle layer is 0.5mm;
[0081] The thickness of the alumina ceramic outer layer is 25mm.
[0082] The preparation method of the ceramic roller in this embodiment comprises the following steps:
[0083] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 67:13:40:3:25 to obtain an alumina ceramic inner layer mud material, wherein the average particle size of the alumina powder is 5 μm, the average particle size of the corundum sand is 15 μm, the binder is carboxymethyl cellulose, and the solvent is water;
[0084] Alumina powder, aluminum sol, kaolin, dispersant and solvent are mixed and dispersed in a mass ratio of 70:20:15:10:25 to obtain a uniform intermediate layer coating, wherein the average particle size of the aluminum powder is 5 μm, the dispersant is polyacrylamide, and the solvent is water;
[0085] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 76.5:8.5:40:3:25 to obtain an alumina ceramic outer layer mud material, wherein the average particle size of the alumina powder is 5 μm, the average particle size of the corundum sand is 15 μm, the binder is carboxymethyl cellulose, and the solvent is water;
[0086] The alumina ceramic inner layer mud material is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.05MPa, and extrusion force is 15kN;
[0087] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic inner layer, wherein the first drying temperature is 100°C, the first drying time is 30 hours, the cold isostatic pressing pressure is 180 MPa, the cold isostatic pressing time is 5 minutes, the second drying temperature is 80°C, the second drying time is 8 hours, the first sintering is hanging firing, the first sintering temperature is 1400°C, and the first sintering time is 6 hours;
[0088] The outer surface of the alumina ceramic inner layer is coated with the above-mentioned intermediate layer coating as a tube core, and the above-mentioned alumina ceramic outer layer mud is extruded on its outer surface by vertical extrusion to form an outer layer, and then subjected to a third drying and a second sintering treatment in sequence to obtain a ceramic roller, wherein the vertical extrusion pressure is 40 MPa, the third drying temperature is 80°C, the third drying time is 22h, the second sintering is hanging firing, the second sintering temperature is 1600°C, and the second sintering time is 36h.
[0089] Example 2
[0090] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that:
[0091] The mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the inner layer mud of alumina ceramics is 70:10:30:5:15;
[0092] The mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 45:30:30:15:35;
[0093] The mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the outer layer mud of alumina ceramics is 75:10:50:1:15.
[0094] Example 3
[0095] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that:
[0096] The mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the inner layer mud of alumina ceramics is 50:30:50:1:35;
[0097] The mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 75:10:10:5:15;
[0098] The mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the outer layer mud of alumina ceramics is 95:1:30:5:35.
[0099] Example 4
[0100] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 60:20:25:10:25.
[0101] Example 5
[0102] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 63.75:20:21.25:10:25.
[0103] Example 6
[0104] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 74.375:20:10.625:10:25.
[0105] Example 7
[0106] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent used in preparing the intermediate layer coating is 75:20:10:10:25.
[0107] Example 8
[0108] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 50:30:40:3:25.
[0109] Example 9
[0110] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 65.45:14.55:40:3:25.
[0111] Example 10
[0112] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 69.33:10.67:40:3:25.
[0113] Embodiment 11
[0114] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 70:10:40:3:25.
[0115] Example 12
[0116] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 47:13:60:3:25.
[0117] Embodiment 13
[0118] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic inner layer mud is 82:25:40:3:25.
[0119] Embodiment 14
[0120] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 75:10:40:3:25.
[0121] Embodiment 15
[0122] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 75.56:9.44:40:3:25.
[0123] Example 16
[0124] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 77.27:7.73:40:3:25.
[0125] Embodiment 17
[0126] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 78.46:6.54:40:3:25.
[0127] Embodiment 18
[0128] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 91.5:8.5:25:3:25.
[0129] Embodiment 19
[0130] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the mass ratio of alumina powder, kaolin, corundum sand, binder and solvent used in preparing the alumina ceramic outer layer mud is 56.5:8.5:60:3:25.
[0131] Embodiment 20
[0132] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0133] Alumina micropowder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 41.25:13.75:40:5:5:3:20 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0134] Embodiment 21
[0135] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0136] Alumina micropowder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 45:10:30:1:1:1:15 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0137] Embodiment 22
[0138] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0139] Alumina micropowder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 25:30:50:10:10:5:35 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0140] Embodiment 23
[0141] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0142] Alumina micropowder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 25:30:40:5:5:3:20 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0143] Embodiment 24
[0144] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0145] Alumina micropowder, kaolin, corundum sand, thermal conductivity agent, binder and solvent are mixed and dispersed in a mass ratio of 36.67:18.33:40:5:5:3:20 to obtain alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0146] Embodiment 25
[0147] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0148] Alumina micropowder, kaolin, corundum sand, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 44:11:40:5:5:3:20 to obtain an alumina ceramic outer layer mud material, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0149] Embodiment 26
[0150] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0151] Alumina micropowder, kaolin, corundum sand, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 45:10:40:5:5:3:20 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0152] Embodiment 27
[0153] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0154] Alumina micropowder, kaolin, corundum sand, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 56.25:13.75:25:5:5:3:20 to obtain an alumina ceramic outer layer mud material, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0155] Embodiment 28
[0156] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the preparation method of the outer layer of alumina ceramic mud is different. The preparation method of the outer layer of alumina ceramic mud of this embodiment is as follows:
[0157] Alumina micropowder, kaolin, corundum sand, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 26.25:13.75:55:5:5:3:20 to obtain an alumina ceramic outer layer mud, wherein the average particle size of the alumina micropowder is 5 μm, the average particle size of the corundum sand is 15 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water.
[0158] Embodiment 29
[0159] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the thickness of the inner layer of alumina ceramic is 10 mm, and the thickness of the outer layer of alumina ceramic is 20 mm.
[0160] Embodiment 30
[0161] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the thickness of the inner layer of alumina ceramic is 15 mm, and the thickness of the outer layer of alumina ceramic is 15 mm.
[0162] Embodiment 31
[0163] An embodiment of the ceramic roller described in the present application. The difference between the ceramic roller of this embodiment and the ceramic roller of embodiment 1 is that the thickness of the inner layer of alumina ceramic is 20 mm, and the thickness of the outer layer of alumina ceramic is 10 mm.
[0164] Embodiment 32
[0165] An embodiment of the ceramic roller described in the present application. The ceramic roller of this embodiment comprises an alumina ceramic inner layer, a middle layer and an alumina ceramic outer layer connected in sequence from the inside to the outside;
[0166] Among them, the inner layer of alumina ceramic is in the shape of a hollow tube with an outer diameter of 20 mm and a thickness of 5 mm;
[0167] The thickness of the middle layer is 0.1mm;
[0168] The thickness of the alumina ceramic outer layer is 25mm.
[0169] The preparation method of the ceramic roller in this embodiment comprises the following steps:
[0170] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 67:13:40:3:25 to obtain an alumina ceramic inner layer mud material, wherein the average particle size of the alumina powder is 1 μm, the average particle size of the corundum sand is 5 μm, the binder is phenolic resin, and the solvent is water;
[0171] Alumina powder, aluminum sol, kaolin, dispersant and solvent are mixed and dispersed in a mass ratio of 70:20:15:10:25 to obtain an intermediate layer coating, wherein the average particle size of the aluminum powder is 5 μm, the dispersant is sodium polyacrylate, and the solvent is water;
[0172] Alumina powder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 41.25:13.75:40:5:5:3:20 to obtain an alumina ceramic outer layer mud material, wherein the average particle size of the alumina powder is 1 μm, the average particle size of the corundum sand is 5 μm, the thermal conductivity agent is silicon carbide with an average particle size of 1 μm, the toughening agent is zirconium oxide fiber with an average particle size of 1 μm, the binder is polyvinyl pyrrolidone, and the solvent is ethanol;
[0173] The alumina ceramic inner layer mud material is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.1 MPa, and extrusion force is 10 kN;
[0174] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic inner layer, wherein the first drying temperature is 60°C, the first drying time is 48h, the cold isostatic pressing pressure is 120 MPa, the cold isostatic pressing time is 8min, the second drying temperature is 50°C, the second drying time is 6h, the first sintering is hanging firing, the first sintering temperature is 1300°C, and the first sintering time is 10h;
[0175] The outer surface of the alumina ceramic inner layer is coated with the intermediate layer coating to serve as a tube core, and the alumina ceramic outer layer mud is extruded on its outer surface by vertical extrusion to form an outer layer, and then sequentially subjected to a third drying and a second sintering treatment to obtain a ceramic roller, wherein the vertical extrusion pressure is 20 MPa, the third drying temperature is 60°C, the third drying time is 30h, the second sintering is hanging firing, the second sintering temperature is 1400°C, and the second sintering time is 48h.
[0176] Embodiment 33
[0177] An embodiment of the ceramic roller described in the present application. The ceramic roller of this embodiment comprises an alumina ceramic inner layer, a middle layer and an alumina ceramic outer layer connected in sequence from the inside to the outside;
[0178] Among them, the inner layer of alumina ceramic is in the shape of a hollow tube, with an outer diameter of 40mm and a thickness of 5mm;
[0179] The thickness of the middle layer is 1mm;
[0180] The thickness of the alumina ceramic outer layer is 25mm.
[0181] The preparation method of the ceramic roller in this embodiment comprises the following steps:
[0182] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 67:13:40:3:25 to obtain an alumina ceramic inner layer mud material, wherein the average particle size of the alumina powder is 10 μm, the average particle size of the corundum sand is 25 μm, the binder is polyvinyl alcohol, and the solvent is ethanol;
[0183] Alumina powder, aluminum sol, kaolin, dispersant and solvent are mixed and dispersed in a mass ratio of 70:20:15:10:25 to obtain an intermediate layer coating, wherein the average particle size of the aluminum powder is 5 μm, the dispersant is hydroxymethyl cellulose, and the solvent is ethanol;
[0184] Alumina powder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a mass ratio of 41.25:13.75:40:5:5:3:20 to obtain an alumina ceramic outer layer mud material, wherein the average particle size of the alumina powder is 10 μm, the average particle size of the corundum sand is 25 μm, the thermal conductivity agent is cordierite with an average particle size of 10 μm, the toughening agent is mullite fiber with an average particle size of 1 μm, the binder is hydroxypropyl methylcellulose, and the solvent is ethanol;
[0185] The alumina ceramic inner layer mud material is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.01 MPa, and extrusion force is 20 kN;
[0186] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic inner layer, wherein the first drying temperature is 120°C, the first drying time is 12h, the cold isostatic pressing pressure is 240 MPa, the cold isostatic pressing time is 1min, the second drying temperature is 100°C, the second drying time is 12h, the first sintering is hanging firing, the first sintering temperature is 1600°C, and the first sintering time is 2h;
[0187] The outer surface of the alumina ceramic inner layer is coated with the intermediate layer coating to serve as a tube core, and the alumina ceramic outer layer mud is extruded on its outer surface by vertical extrusion to form an outer layer, and then sequentially subjected to a third drying and a second sintering treatment to obtain a ceramic roller, wherein the vertical extrusion pressure is 60 MPa, the third drying temperature is 100°C, the third drying time is 15h, the second sintering is hanging firing, the second sintering temperature is 1800°C, and the second sintering time is 24h.
[0188] Comparative Example 1
[0189] This comparative example provides a ceramic roller. The difference between the ceramic roller of this comparative example and the ceramic roller of Example 1 is that no intermediate layer is provided, that is, no intermediate layer coating is used during its preparation.
[0190] Comparative Example 2
[0191] This comparative example provides a ceramic roller. The difference between the ceramic roller in this comparative example and the ceramic roller in Example 1 is that boehmite completely replaces the aluminum sol in the intermediate layer coating, and the mass ratio of aluminum oxide powder, boehmite, kaolin, dispersant and solvent in the intermediate layer coating is 70:20:15:10:25.
[0192] Comparative Example 3
[0193] This comparative example provides a ceramic roller. The difference between the ceramic roller in this comparative example and the ceramic roller in Example 1 is that the aluminum sol in the intermediate layer coating is completely replaced by silica sol, and the mass ratio of alumina powder, silica sol, kaolin, dispersant and solvent in the intermediate layer coating is 70:20:15:10:25.
[0194] Comparative Example 4
[0195] This comparative example provides a ceramic roller. The difference between the ceramic roller in this comparative example and the ceramic roller in Example 1 is that carboxymethyl cellulose is used to completely replace the aluminum sol in the intermediate layer coating, and the mass ratio of aluminum oxide powder, carboxymethyl cellulose, kaolin, dispersant and solvent in the intermediate layer coating is 70:20:15:10:25.
[0196] Comparative Example 5
[0197] This comparative example provides a ceramic roller. The difference between the ceramic roller in this comparative example and the ceramic roller in Example 1 is that kaolin is not used in preparing the intermediate layer coating, and the mass ratio of alumina powder, aluminum sol, dispersant and solvent in the intermediate layer coating is 70:20:10:25.
[0198] Comparative Example 6
[0199] This comparative example provides a ceramic roller. The difference between the ceramic roller of this comparative example and the ceramic roller of Example 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent in the intermediate layer coating is 50:20:35:10:25.
[0200] Comparative Example 7
[0201] This comparative example provides a ceramic roller. The difference between the ceramic roller of this comparative example and the ceramic roller of Example 1 is that the mass ratio of alumina powder, aluminum sol, kaolin, dispersant and solvent in the intermediate layer coating is 50:40:15:10:25.
[0202] Comparative Example 8
[0203] This comparative example provides a ceramic roller rod. The ceramic roller rod of this comparative example is in the shape of a hollow tube, with an outer diameter of 55.5 mm and a thickness of 30.5 mm.
[0204] The preparation method of the ceramic roller of this comparative example comprises the following steps:
[0205] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 67:13:40:3:25 to obtain an alumina ceramic mud material, wherein the average particle size of the alumina powder is 5 μm, the average particle size of the corundum sand is 15 μm, the binder is carboxymethyl cellulose, and the solvent is water;
[0206] The alumina ceramic mud is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.05MPa, and extrusion force is 15kN;
[0207] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic, wherein the temperature of the first drying is 100°C, the time of the first drying is 30 hours, the pressure of the cold isostatic pressing is 180 MPa, the time of the cold isostatic pressing is 5 minutes, the temperature of the second drying is 80°C, the time of the second drying is 8 hours, the first sintering is hanging firing, the temperature of the first sintering is 1400°C, and the time of the first sintering is 6 hours;
[0208] The above was sequentially subjected to a third drying and a second sintering treatment to obtain a ceramic roller, wherein the third drying temperature was 80°C, the third drying time was 22h, the second sintering was hanging firing, the second sintering temperature was 1600°C, and the second sintering time was 36h.
[0209] Comparative Example 9
[0210] This comparative example provides a ceramic roller rod. The ceramic roller rod of this comparative example is in the shape of a hollow tube, with an outer diameter of 55.5 mm and a thickness of 30.5 mm.
[0211] The preparation method of the ceramic roller of this comparative example comprises the following steps:
[0212] Alumina powder, kaolin, corundum sand, a binder and a solvent are mixed and dispersed in a mass ratio of 76.5:8.5:40:3:25 to obtain an alumina ceramic mud material, wherein the average particle size of the alumina powder is 5 μm, the average particle size of the corundum sand is 15 μm, the binder is carboxymethyl cellulose, and the solvent is water;
[0213] The alumina ceramic mud is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.05MPa, and extrusion force is 15kN;
[0214] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic, wherein the temperature of the first drying is 100°C, the time of the first drying is 30 hours, the pressure of the cold isostatic pressing is 180 MPa, the time of the cold isostatic pressing is 5 minutes, the temperature of the second drying is 80°C, the time of the second drying is 8 hours, the first sintering is hanging firing, the temperature of the first sintering is 1400°C, and the time of the first sintering is 6 hours;
[0215] The above-mentioned alumina ceramics are successively subjected to a third drying and a second sintering treatment to obtain a ceramic roller rod, wherein the third drying temperature is 80°C, the third drying time is 22h, the second sintering is hanging firing, the second sintering temperature is 1600°C, and the second sintering time is 36h.
[0216] Comparative Example 10
[0217] This comparative example provides a ceramic roller rod. The ceramic roller rod of this comparative example is in the shape of a hollow tube, with an outer diameter of 55.5 mm and a thickness of 30.5 mm.
[0218] The preparation method of the ceramic roller of this comparative example comprises the following steps:
[0219] Alumina powder, kaolin, corundum sand, thermal conductivity agent, toughening agent, binder and solvent are mixed and dispersed in a weight ratio of 41.25:13.75:40:5:5:3:20 to obtain an alumina ceramic mud, wherein the average particle size of the alumina powder is 5 μm, the average particle size of the corundum sand is 15 μm, the thermal conductivity agent is cordierite with an average particle size of 6 μm, the toughening agent is zirconia whisker with an average particle size of 5 μm, the binder is carboxymethyl cellulose, and the solvent is water;
[0220] The alumina ceramic mud is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body, wherein the vacuum extrusion process meets the following requirements: vacuum degree is -0.05MPa, and extrusion force is 15kN;
[0221] The tubular alumina ceramic green body is sequentially subjected to first drying, cold isostatic pressing, second drying, first sintering and grinding to obtain an alumina ceramic, wherein the temperature of the first drying is 100°C, the time of the first drying is 30 hours, the pressure of the cold isostatic pressing is 180 MPa, the time of the cold isostatic pressing is 5 minutes, the temperature of the second drying is 80°C, the time of the second drying is 8 hours, the first sintering is hanging firing, the temperature of the first sintering is 1400°C, and the time of the first sintering is 6 hours;
[0222] The above-mentioned alumina ceramics are successively subjected to a third drying and a second sintering treatment to obtain a ceramic roller rod, wherein the third drying temperature is 80°C, the third drying time is 22h, the second sintering is hanging firing, the second sintering temperature is 1600°C, and the second sintering time is 36h.
[0223] The following test methods were used to test the performance of the above examples and comparative examples:
[0224] Flexural strength: GB / T 6569-1986, tested by three-point bending method;
[0225] Bulk density: GB / T 25995-2010, the immersion liquid is deionized water, and the immersion liquid is immersed by boiling method;
[0226] Acid and alkali corrosion resistance: GB / T 1970-1996;
[0227] Thermal shock cycle resistance: YB / T 376.2-1995, sample preheating temperature is 300℃, sample preheating temperature is 2h, heating furnace temperature is 1300℃.
[0228] The test results are shown in Table 1 and Table 2.
[0229] Table 1
[0230]
[0231] Table 2
[0232]
[0233] From the above data, we can see that the flexural strength is above 82MPa and the bulk density is 3.03~3.15g / cm 3 Among them, the acid corrosion loss rate and the mass loss rate after alkali corrosion of Examples 1 to 19 and 29 to 36 are all below 0.42%, and the number of thermal shock resistance cycles of Examples 20 to 28 is above 7.
[0234] In Comparative Examples 1 to 4, since the raw material of the middle layer does not contain aluminum sol, or boehmite, silica sol or carboxymethyl cellulose is used instead of aluminum sol, the bonding strength of the inner and outer layers is low, and the flexural strength of the roller is low.
[0235] In Comparative Example 5, since the intermediate layer raw material does not contain kaolin, the roller buffer extrusion force deviates and the flexural strength is low.
[0236] In Comparative Example 6, the kaolin content in the intermediate layer raw material was excessive, and SiO2 glass phase remained, resulting in low flexural strength of the roller.
[0237] In Comparative Example 7, due to excessive aluminum sol, defects between the inner and outer layers are easily generated, the bonding strength is reduced, and the flexural strength of the roller is relatively low.
[0238] Comparative Example 8 has low surface density and poor acid and alkali corrosion resistance; at the same time, its thermal shock resistance is also poor.
[0239] In Comparative Example 9, the amount of liquid phase produced during the first sintering process was too small, resulting in poor adhesion and rod breakage.
[0240] The comparative example 10 has a low aluminum oxide content, resulting in deviation in its thermal shock resistance.
[0241] From the comparison of Examples 1, 4 to 7, it can be seen that the mass ratio of alumina to kaolin in the intermediate layer raw material will affect the flexural strength of the roller. It is preferred that the mass ratio of alumina to kaolin is in the range of (2.9 to 7.1):1, so that the roller has a higher alumina content and a more suitable liquid phase amount during the second sintering process, and the inner and outer layer bonding strength is higher, and the roller has a higher flexural strength.
[0242] From the comparison between Examples 1 and 8 to 10, it can be seen that the mass ratio of alumina to kaolin in the inner layer raw material will affect the flexural strength of the roller. It is preferred that the mass ratio of alumina to kaolin is in the range of (4.4 to 6.6):1, so that the roller has a higher alumina content and at the same time, the amount of liquid phase produced during sintering is more appropriate and the adhesion is stronger, thereby making the roller have higher flexural strength.
[0243] From the comparison of Examples 1 and 14 to 17, it can be seen that the mass ratio of alumina to kaolin in the outer layer raw material will affect the flexural strength and corrosion resistance of the roller. It is preferred that the mass ratio of alumina to kaolin is in the range of (7.9 to 10.1):1. On the one hand, the alumina content of the roller is higher, and the amount of liquid phase generated during the second sintering process is more appropriate, the bonding strength of the inner and outer layers is higher, and the flexural strength of the roller is higher. On the other hand, the surface density of the roller is higher, and it has better corrosion resistance.
[0244] From the comparison of Examples 20, 23 to 26, it can be seen that the mass ratio of alumina to kaolin in the outer layer raw material will affect the flexural strength and thermal shock resistance of the roller. Preferably, the mass ratio of alumina to kaolin is in the range of (1.9 to 4.1):1 to make the roller have higher flexural strength and better thermal shock resistance.
[0245] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A ceramic roller, characterized in that: It includes an alumina ceramic inner layer, an intermediate layer and an alumina ceramic outer layer connected in sequence from the inside to the outside, wherein the intermediate layer is mainly prepared from the following raw materials in parts by weight: 43~77 parts of alumina powder, 10~30 parts of aluminum sol, 10~30 parts of kaolin, Dispersant 5~15 parts, 15-35 parts of solvent; In the raw materials for preparing the intermediate layer, the mass ratio of alumina powder to kaolin is (2.9-7.1):
1.
2. The ceramic roller according to claim 1, characterized in that: The alumina ceramic inner layer is mainly prepared from the following raw materials in parts by weight: 50~70 parts of alumina powder, 10~30 parts of kaolin, 28~52 parts of corundum sand, 1~5 parts of binder, 15~35 parts of solvent.
3. The ceramic roller according to claim 2, characterized in that: In the raw materials for preparing the inner layer of alumina ceramics, the mass ratio of alumina powder to kaolin is (4.4-6.6):
1.
4. The ceramic roller according to claim 2, characterized in that: The alumina ceramic outer layer is mainly prepared from the following raw materials in parts by weight: Alumina powder 75~95 parts, 1~10 parts of kaolin, 28~52 parts of corundum sand, 1~5 parts of binder, 15-35 parts of solvent; Or the alumina ceramic outer layer is mainly prepared from the following raw materials in parts by weight: Alumina powder 25~45 parts, 10~30 parts of kaolin, 28~52 parts of corundum sand, 1~10 parts of thermal conductivity agent, 1~10 parts of toughening agent, 1~5 parts of binder, 15~35 parts of solvent.
5. The ceramic roller according to claim 4, characterized in that: In the raw materials for preparing the outer layer of alumina ceramics, the mass ratio of alumina powder to kaolin is (7.9-10.1):1 or (1.9-4.1):
1.
6. The ceramic roller according to claim 4, characterized in that: Satisfy at least one of the following conditions (A) to (G): (A) the binder in the raw materials for preparing the inner layer and the outer layer of alumina ceramics independently comprises at least one of carboxymethyl cellulose, polyvinyl alcohol, phenolic resin, hydroxypropyl methyl cellulose, polyvinyl pyrrolidone and cyclodextrin; (B) the solvents in the raw materials for preparing the inner layer, the middle layer and the outer layer of the alumina ceramics independently include at least one of water and ethanol; (C) the dispersant in the raw material for preparing the intermediate layer includes at least one of polyacrylamide, sodium polyacrylate, hydroxymethyl cellulose and polypropylene alcohol; (D) the thermal conductive agent comprises at least one of cordierite and silicon carbide, the average particle size of the cordierite is 1-10 μm, and the average particle size of the silicon carbide is 0.1-2 μm; (E) the toughening agent comprises at least one of fibers and whiskers, wherein the fibers and whiskers each independently comprise at least one of mullite and zirconia, the average particle size of the mullite is 1 to 3 mm, and the average particle size of the zirconia is 1 to 10 μm; (F) the average particle size of the alumina powder in the raw materials for preparing the alumina ceramic inner layer, the intermediate layer and the alumina ceramic outer layer is independently 1 to 10 μm; (G) The average particle size of the corundum sand in the raw materials for preparing the inner layer and the outer layer of alumina ceramics is independently 5 to 25 μm.
7. The ceramic roller according to claim 1, characterized in that: The inner layer of the alumina ceramic is in the shape of a hollow tube, and the thickness of the inner layer of the alumina ceramic is 1 to 10 mm; And / or, the thickness of the outer layer of alumina ceramic is 15-35 mm; And / or, the outer diameter of the inner layer of alumina ceramic is 20-40 mm; And / or, the thickness of the intermediate layer is 0.1-1 mm.
8. A method for preparing a ceramic roller according to any one of claims 1 to 7, characterized in that: The following steps are involved: The raw materials for preparing the inner layer of the alumina ceramic, the raw materials for preparing the middle layer, and the raw materials for preparing the outer layer of the alumina ceramic are mixed and dispersed respectively to obtain the mud material for the inner layer of the alumina ceramic, the coating material for the middle layer, and the mud material for the outer layer of the alumina ceramic; The alumina ceramic inner layer mud material is subjected to a vacuum extrusion process to obtain a tubular alumina ceramic green body; The tubular alumina ceramic green body is sequentially subjected to a first drying, a cold isostatic pressing, a second drying, a first sintering and a grinding process to obtain an alumina ceramic inner layer; The outer surface of the inner layer of alumina ceramic is coated with the intermediate layer coating to form a tube core, and the outer layer of alumina ceramic is extruded on its outer surface by vertical extrusion to form an outer layer, and then subjected to a third drying and a second sintering treatment in sequence to obtain a ceramic roller.
9. The method for preparing a ceramic roller according to claim 8, characterized in that: At least one of the conditions S1 to S9 is met: S1. The vacuum degree of the vacuum extrusion process is -0.1~0MPa, and the extrusion force is 10~20kN; S2, the temperature of the first drying is 60-120°C, and the time of the first drying is 12-48 h; S3, the pressure of the cold isostatic pressing is 120-240 MPa, and the time of the cold isostatic pressing is 1-8 min; S4, the temperature of the second drying is 50-100°C, and the time of the second drying is 6-12h; S5, the first sintering is hanging sintering, the temperature of the first sintering is 1300-1600°C, and the time of the first sintering is 2-10 h; S6, coating the outer surface of the inner layer of the alumina ceramic with the intermediate layer coating for 1 to 4 times; S7, the vertical extrusion pressure is 20~60 MPa; S8, the temperature of the third drying is 60-100°C, and the time of the third drying is 15-30 hours; S9. The second sintering is hanging sintering, the temperature of the second sintering is 1400-1800° C., and the time of the second sintering is 24-48 h.
10. Use of the ceramic roller according to any one of claims 1 to 7 in a sintering roller kiln for at least one of sodium battery materials, lithium battery materials, and carbon fibers, or in a belt roller kiln for firing at least one of daily-use porcelain, sanitary porcelain, architectural porcelain, and rare earth calcination.
Citation Information
Patent Citations
Ultrahigh-temperature high-strength ceramic roller and preparation method thereof
CN110894162A
Thermal insulation coating for ceramic roller tube and preparation method thereof
CN112679194A