A method for preparing a carbon / carbon PECVD carrier frame
Through the preparation method of the carbon/carbon PECVD load-bearing frame, the mixing of composite raw materials and resin glue and high-temperature treatment are used to solve the problem of low strength of the existing PECVD load-bearing frame, achieve high mechanical properties and ablation resistance, and reduce replacement frequency and cost.
Patent Information
- Application Number
- CN202410939743.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The existing PECVD load-bearing frame is made of graphite, which has low strength and is easily damaged, resulting in high replacement frequency and high cost. Existing improvement methods fail to solve the strength problem from the root cause.
Using the preparation method of carbon/carbon PECVD load-bearing frame, by mixing composite raw materials and resin glue, and undergoing injection molding, carbonization, liquid phase impregnation, high-temperature graphitization, pyrolytic carbon coating and purification, a frame with high mechanical properties is prepared and carbon/carbon PECVD bearing frame with ablation resistance.
Significantly improves the mechanical properties and ablation resistance of the carbon/carbon PECVD bearing frame, reduces replacement frequency and usage costs, and provides a solution with high strength and short preparation cycle.
Smart Images

Figure CN118459241B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials, and in particular relates to a method for preparing a carbon / carbon PECVD carrier frame. Background Art
[0002] The PECVD carrier frame is one of the main consumable parts of the silicon wafer coating equipment. Its working principle is to place the silicon wafer to be coated flatly on the station of the PECVD carrier frame, transport it to the plasma chamber in the PECVD coating equipment via a conveyor belt, and then perform PECVD coating under certain process conditions. In view of the complex process environment of PECVD, the PECVD boat or boat plate generally used is mainly made of graphite. However, the graphite boat is difficult to operate and has low strength, resulting in high frequency of replacement and high cost. The current solution to this problem is to improve the plate preparation process, increase density, and increase strength. Although some problems have been solved, the problem of low strength and susceptibility to damage has not been solved from the root, which greatly increases the replacement frequency and cost of the carrier frame. Summary of the invention
[0003] The object of the present invention is to provide a method for preparing a carbon / carbon PECVD carrier frame, improve the mechanical properties and performance of the carbon / carbon PECVD carrier frame, and reduce the replacement frequency and use cost.
[0004] In order to solve the above technical problems, the present invention specifically provides the following technical solutions:
[0005] A method for preparing a carbon / carbon PECVD carrier frame comprises the following steps:
[0006] The composite raw materials are added to the resin glue to prepare a mixed slurry, and the carbon fiber composite material sheet is obtained through the injection molding process, and then the carbon-carbon composite material sheet is obtained through carbonization and liquid phase impregnation resin treatment. Finally, the carbon / carbon PECVD carrier frame is obtained through high-temperature graphitization treatment, pyrolytic carbon coating treatment and purification treatment.
[0007] Preferably, the composite raw material includes modified chopped carbon fibers, which include chopped carbon fibers and surface-grafted vinyl caprolactam structures thereof; the resin in the resin adhesive is phenolic resin or furfural resin; and the liquid phase impregnating resin is impregnated phenolic resin or furfural resin.
[0008] Preferably, the composite raw material further includes additives to prepare a mixed slurry containing the additives.
[0009] Preferably, the additive is at least one of flake graphite or silicon powder.
[0010] Preferably, the mesh size of the flake graphite is 50-200 mesh.
[0011] Preferably, the mesh size of the silicon powder is 50-200 mesh.
[0012] Preferably, in the mixed slurry, by weight, the amount of modified chopped carbon fiber is 10-30 parts, the amount of resin glue is 40-60 parts, and the amount of additives is 5-20 parts.
[0013] Preferably, the density of the carbon fiber composite material plate is ≥1.5 g / cm 3 .
[0014] Preferably, the carbonization temperature is 900-950° C. and the time is 1-3 h.
[0015] Preferably, the temperature of the liquid phase impregnation resin is 120-200° C., the pressure is 2-4 MPa, and the time is 1-3 h.
[0016] Preferably, the temperature of the high-temperature graphitization treatment is 2000-2500° C., and the time of the high-temperature graphitization treatment is 1-3 h.
[0017] Preferably, the pyrolytic carbon coating treatment conditions are as follows: hydrocarbons are introduced, nitrogen is used as the diluent gas, the volume ratio of hydrocarbons to nitrogen is 100:20-40, the furnace pressure is controlled at 2000-4000 Pa, the temperature is 1000-1150° C., and the treatment is performed for 10-30 h.
[0018] More preferably, the hydrocarbon comprises natural gas or propane.
[0019] Preferably, the purified gas used in the purification process is a halogenated alkane with a concentration of 1-10 kg / m 3 The purification treatment temperature is 1800-2400℃, and the purification treatment time is 2-4 h.
[0020] More preferably, the halogenated alkane comprises carbon hexafluoride.
[0021] The invention discloses a carbon / carbon PECVD bearing frame, comprising resin carbon and modified short-cut carbon fibers coated in the resin carbon.
[0022] Preferably, the modified chopped carbon fiber comprises chopped carbon fiber and a vinyl caprolactam structure grafted on the surface thereof.
[0023] Preferably, the resin charcoal is obtained by pyrolysis of resin glue.
[0024] Preferably, the resin glue is phenolic resin or furfural resin.
[0025] Preferably, the average length of the modified chopped carbon fibers is 1-2 cm.
[0026] Preferably, the method for preparing modified chopped carbon fibers comprises: preparing desized chopped carbon fibers, oxidizing, chlorinating, and finally reacting with vinyl caprolactam to prepare modified chopped carbon fibers.
[0027] The present invention also provides the use of the carbon / carbon PECVD supporting frame prepared by the above-mentioned preparation method in supporting silicon wafer coating.
[0028] In one embodiment, a method for preparing a carbon / carbon PECVD carrier frame comprises the following steps:
[0029] Preparation of chopped carbon fiber: provide Toray T700-12K carbon fiber precursor with a carbon content of ≥95%, and cut it into chopped carbon fiber; add the chopped carbon fiber into acetone, reflux at 40-60°C for 36-60 h, take out after reflux, wash, and dry to obtain desizing chopped carbon fiber.
[0030] Preferably, the average length of the chopped carbon fibers is 1-2 cm.
[0031] Preferably, the amount of chopped carbon fibers used is 20-40 wt % of acetone.
[0032] More preferably, the modified chopped carbon fiber is prepared by providing a carbon fiber precursor having a carbon content of ≥95% of Toray T700-12K, and cutting it into chopped carbon fibers; adding the chopped carbon fibers to acetone, refluxing at 40-60°C for 36-60 h, removing the reflux after the reflux, washing, and drying to obtain desized chopped carbon fibers; adding the desized chopped carbon fibers to a potassium permanganate solution with a mass concentration of 60-75% for oxidation, reacting at 70-90°C for 2-4 h, removing the chopped carbon fibers, washing, and drying to obtain oxidized chopped carbon fibers; adding the oxidized chopped carbon fibers to a mixed solution of thionyl chloride / N,N-dimethylformamide, refluxing at 60-80°C for 35-55 h, removing the reflux after the reflux, washing, and drying to obtain chlorinated chopped carbon fibers; adding the chlorinated chopped carbon fibers to a mixed solution of ethylene glycol / triethylamine, refluxing at 60-80°C for 35-55 h, h, reflux is finished, taken out, washed, and dried to obtain alcoholysis chopped carbon fibers; alcoholysis chopped carbon fibers are added to a vinyl caprolactam / carbon tetrachloride mixed solution, ammonium cerium nitrate is added, and reacted at 30-50°C for 3-6 h to obtain modified chopped carbon fibers. Modification of chopped carbon fibers is beneficial to the wetting of carbon fibers with resins, and improves the interface bonding quality between carbon fibers and resins, thereby improving the performance of the composite material.
[0033] Preferably, the average length of the chopped carbon fibers is 1-2 cm.
[0034] Preferably, the amount of chopped carbon fibers used is 20-40 wt % of acetone.
[0035] Preferably, the desized chopped carbon fibers are used in an amount of 10-30 wt % of the potassium permanganate solution.
[0036] Preferably, the thionyl chloride / N,N-dimethylformamide mixed solution contains 10-20 wt % of thionyl chloride.
[0037] Preferably, the amount of the oxidized chopped carbon fibers used is 10-30 wt % of the thionyl chloride / N,N-dimethylformamide mixed solution.
[0038] Preferably, the ethylene glycol / triethylamine mixed solution contains 5-20 wt % of triethylamine.
[0039] Preferably, the amount of chlorinated chopped carbon fibers used is 10-30 wt % of the ethylene glycol / triethylamine mixed solution.
[0040] Preferably, the vinyl caprolactam / carbon tetrachloride mixed solution contains 5-20 wt % of vinyl caprolactam.
[0041] Preferably, the amount of alcoholysis chopped carbon fibers used is 10-30 wt % of the vinyl caprolactam / carbon tetrachloride mixed solution.
[0042] Preferably, the amount of cerium ammonium nitrate added is 1-3 wt % of the vinyl caprolactam / carbon tetrachloride mixed solution.
[0043] The present invention also discloses a method for preparing a modified phenolic resin, comprising the following steps:
[0044] Add phenol and barium hydroxide to the formaldehyde solution, react at 50-70°C for 1-3 h, at 65-75°C for 1-3 h, at 75-90°C for 15-30 min, add phenyltrimethoxysilane / methanol mixed solution and ammonia water, heat to 80-95°C, react until the solution becomes turbid, react for 20-30 min to stop the reaction, and perform rotary evaporation. When there is no distillate, stop rotary evaporation to obtain modified phenolic resin. The modified phenolic resin is used to prepare carbon / carbon PECVD carrier frames, which can improve the volume density, mechanical properties and ablation resistance of carbon / carbon PECVD carrier frames. The reason may be that the modified phenolic resin improves the bonding effect between fibers, and the phenyltrimethoxysilane used has a certain promoting effect on the impregnation of resin and short-cut carbon fibers.
[0045] Preferably, the formaldehyde solution contains 37-40 wt % of formaldehyde.
[0046] Preferably, the molar ratio of phenol to formaldehyde is 1:1-1.5.
[0047] Preferably, the phenyltrimethoxysilane / methanol mixed solution contains 10-30 wt % of phenyltrimethoxysilane.
[0048] Preferably, the molar ratio of phenol to phenyltrimethoxysilane is 1:0.2-0.3; the mass ratio of phenol to barium hydroxide is 1:0.05-0.1.
[0049] Preferably, the mass fraction of aqueous ammonia is 25-28%.
[0050] Preferably, the amount of ammonia is 2-10 wt% of phenol.
[0051] Raw material mixing: fully mix the desized chopped carbon fiber, phenolic resin and additives at a mixing temperature of 40-60°C, a rotation speed of 120-180 r / min, and a mixing time of 1-3 h to obtain a mixed slurry.
[0052] More preferably, the modified chopped carbon fiber, the modified phenolic resin and the additive are fully mixed at a mixing temperature of 40-60° C., a rotating speed of 120-180 r / min and a mixing time of 1-3 h to obtain a mixed slurry.
[0053] Preferably, the additives include flake graphite and silicon powder.
[0054] Preferably, the mass ratio of graphite to silicon powder is 1:1-2.
[0055] Preferably, in parts by weight, the amount of the modified chopped carbon fiber is 10-30 parts, the amount of the phenolic resin is 40-60 parts, and the amount of the additive is 5-20 parts.
[0056] Injection molding: Add the mixed slurry into the barrel of the injection molding machine, maintain the material temperature at 40-60°C, then inject it into the cavity of the injection mold and maintain the pressure at 5-20 MPa.
[0057] Heating and curing: Heat the injection mold to 120-200℃ and keep it for 10-30 min.
[0058] Open the mold and take out the material: take out the injection mold, put it into 5-20℃ cooling water to cool the mold, and obtain the carbon fiber composite material sheet.
[0059] Preparation of carbon-carbon composite material sheet: The carbon fiber composite material sheet is subjected to carbonization and liquid phase impregnation resin treatment to obtain the carbon-carbon composite material sheet.
[0060] Preferably, the liquid impregnating resin is a phenolic resin or a furfural resin.
[0061] Preferably, the carbonization temperature is 900-950° C. and the time is 1-3 h.
[0062] Preferably, the temperature of the liquid phase impregnation resin is 120-200° C., the pressure is 2-4 MPa, and the time is 1-3 h.
[0063] Preferably, the density of the carbon-carbon composite material sheet is ≥1.5 g / cm 3 .
[0064] Preparation of a carbon / carbon PECVD carrier frame: subjecting a carbon-carbon composite material sheet to high-temperature graphitization treatment, pyrolytic carbon coating treatment, and purification treatment to prepare a carbon / carbon PECVD carrier frame.
[0065] Preferably, the temperature of the high-temperature graphitization treatment is 2000-2500° C., and the time of the high-temperature graphitization treatment is 1-3 h.
[0066] Preferably, the pyrolytic carbon coating treatment conditions are: introducing natural gas, using nitrogen as the diluent gas, and the volume ratio of natural gas to nitrogen is 100:20-40; controlling the furnace pressure to 2000-4000 Pa, the temperature to 1000-1150° C., and treating for 10-30 h.
[0067] Preferably, the purification process is carried out under the condition that the purified gas is carbon hexafluoride with a concentration of 1-10 kg / m 3 The purification treatment temperature is 1800-2400℃, and the purification treatment time is 2-4 h.
[0068] The present invention obtains a method for preparing a carbon / carbon PECVD bearing frame, wherein the carbon / carbon PECVD bearing frame is prepared by injection molding a mixed slurry composed of short-cut carbon fibers modified by grafted vinyl caprolactam, resin glue, and additives to prepare a carbon fiber composite material plate, and then carbonized and liquid-phase impregnated with resin to obtain a carbon-carbon composite material plate, and finally high-temperature graphitization treatment, pyrolytic carbon coating treatment, and purification treatment are performed to prepare a carbon / carbon PECVD bearing frame, which has good volume density, mechanical properties, and ablation resistance; the present invention also uses phenyltrimethoxysilane to modify the resin, and then uses it for the preparation of the carbon / carbon PECVD bearing frame, so that the carbon / carbon PECVD bearing frame has better mechanical properties and ablation resistance. The present invention also provides a carbon / carbon PECVD bearing frame with high strength, short preparation cycle, and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. Obviously, the drawings in the following description are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0070] Figure 1 This is the infrared image of modified chopped carbon fiber;
[0071] Figure 2 This is the bending strength diagram of carbon / carbon PECVD carrier frame;
[0072] Figure 3 Frame line burn rate diagram for carbon / carbon PECVD bearing. DETAILED DESCRIPTION
[0073] The present invention is further described in detail below in conjunction with specific embodiments, and the examples provided are only for illustrating the present invention, rather than for limiting the scope of the present invention. The examples provided below can be used as a guide for further improvements by those of ordinary skill in the art, and do not constitute a limitation of the present invention in any way.
[0074] The preparation method of the phenolic resin used in the present invention comprises the following steps:
[0075] Phenol and barium hydroxide were added to the formaldehyde solution, and the reaction was carried out at 60°C for 1.5 h, at 73°C for 2 h, and at 85°C for 25 min. Ammonia water was added, and the temperature was raised to 90°C. The reaction was continued until the solution became turbid, and then the reaction was stopped for 25 min. The phenolic resin was obtained by rotary evaporation. The formaldehyde solution contained 38 wt% of formaldehyde; the molar ratio of phenol to formaldehyde was 1:1.2; the mass fraction of ammonia water was 25%, and the amount of ammonia water was 5 wt% of phenol; and the mass ratio of phenol to barium hydroxide was 1:0.05.
[0076] The experimental methods in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples are commercially available unless otherwise specified.
[0077] Example 1: A method for preparing a carbon / carbon PECVD carrier frame
[0078] S1, raw material mixing: provide Toray T700-12K carbon fiber precursor with a carbon content of ≥95%, cut into short-cut carbon fiber; add the short-cut carbon fiber to acetone, reflux at 50℃ for 48 hours, take out after reflux, wash, dry, and obtain desizing short-cut carbon fiber; fully mix the desizing short-cut carbon fiber, phenolic resin, and additives, the mixing temperature is 50℃, the speed is 150 r / min, and the mixing time is 2 hours to obtain a mixed slurry. Among them, the average length of the short-cut carbon fiber is 1.5 cm; the amount of the short-cut carbon fiber used is 30 wt% of acetone; the additives include flake graphite and silicon powder, and the mass ratio of flake graphite to silicon powder is 1:1; the mesh number of flake graphite is 100 mesh, and the mesh number of silicon powder is 100 mesh. In terms of weight, the amount of desizing short-cut carbon fiber is 20 parts; the amount of phenolic resin is 50 parts; and the amount of additive is 10 parts.
[0079] S2, injection molding: add the mixed slurry into the barrel of the injection molding machine, maintain the material temperature at 50°C, and then inject it into the cavity of the injection mold and maintain the pressure at 10 MPa.
[0080] S3, heating and curing: heat the injection mold to 180°C and keep it for 20 min.
[0081] S4, mold opening and material taking: take out the injection mold, put it into cooling water at 15°C to cool and open the mold, and obtain the carbon fiber composite material plate.
[0082] S5, preparation of carbon-carbon composite material sheet: carbonizing and liquid phase impregnation resin treatment of carbon fiber composite material sheet to obtain carbon-carbon composite material sheet; wherein the carbonization temperature is 1600℃, the time is 2 h; the liquid phase impregnation resin is impregnation phenolic resin, the liquid phase impregnation resin temperature is 180℃, the pressure is 2 MPa, and the time is 2 h. After the liquid phase impregnation resin treatment, the density reaches 1.5 g / cm 3 .
[0083] S6, preparation of carbon / carbon PECVD support frame: subjecting the carbon / carbon composite material plate to high-temperature graphitization treatment, pyrolytic carbon coating treatment, and purification treatment to prepare a carbon / carbon PECVD support frame; wherein, the temperature of the high-temperature graphitization treatment is 2200°C, and the time of the high-temperature graphitization treatment is 2 h; the conditions for the pyrolytic carbon coating treatment are to introduce natural gas, with nitrogen as the dilution gas, the volume ratio of natural gas to nitrogen is 100:30, the furnace pressure is controlled to be 3000 Pa, the temperature is 1050°C, and the treatment is carried out for 20 h; the conditions for the purification treatment are that the purification gas is carbon hexafluoride, and the concentration is 5 kg / m 3 The purification temperature is 2200℃ and the purification time is 3 h.
[0084] Example 2: A method for preparing a carbon / carbon PECVD carrier frame
[0085] The difference from Example 1 is that the desized chopped carbon fiber is replaced by modified chopped carbon fiber.
[0086] The preparation method of modified chopped carbon fiber comprises the following steps:
[0087] Preparation of modified chopped carbon fiber: provide Toray T700-12K carbon fiber precursor with a carbon content of ≥95%, and cut it into chopped carbon fiber; add the chopped carbon fiber to acetone, reflux at 50°C for 48 hours, remove it after reflux, wash it, and dry it to obtain desized chopped carbon fiber; add the desized chopped carbon fiber to a potassium permanganate solution with a mass concentration of 65% for oxidation, react at 80°C for 3 hours, remove it, wash it, and dry it to obtain oxidized chopped carbon fiber; add the oxidized chopped carbon fiber to a mixed solution of thionyl chloride / N,N-dimethylformamide, reflux at 70°C for 45 hours, remove it, wash it, and dry it to obtain chlorinated chopped carbon fiber; add the chlorinated chopped carbon fiber to a mixed solution of ethylene glycol / triethylamine, reflux at 75°C for 45 hours, remove it, wash it, and dry it to obtain alcoholysis chopped carbon fiber; add the alcoholysis chopped carbon fiber to a mixed solution of vinyl caprolactam / carbon tetrachloride, add ammonium cerium nitrate, and react at 40°C for 4 hours. h to obtain modified short chopped carbon fibers. Among them, the average length of the short chopped carbon fibers is 1.5 cm; the amount of short chopped carbon fibers used is 30 wt% of acetone; the amount of desized short chopped carbon fibers used is 20 wt% of potassium permanganate solution; the thionyl chloride / N,N-dimethylformamide mixed solution contains 10 wt% of thionyl chloride; the amount of oxidized short chopped carbon fibers used is 20 wt% of the thionyl chloride / N,N-dimethylformamide mixed solution; the ethylene glycol / triethylamine mixed solution contains 10 wt% of triethylamine; the amount of chlorinated short chopped carbon fibers used is 20 wt% of the ethylene glycol / triethylamine mixed solution; the vinyl caprolactam / carbon tetrachloride mixed solution contains 10 wt% of vinyl caprolactam; the amount of alcoholysis short chopped carbon fibers used is 20 wt% of the vinyl caprolactam / carbon tetrachloride mixed solution; and the amount of cerium ammonium nitrate added is 2 wt% of the vinyl caprolactam / carbon tetrachloride mixed solution.
[0088] Example 3: A method for preparing a carbon / carbon PECVD carrier frame
[0089] The difference between this embodiment and embodiment 2 is that the vinyl caprolactam / carbon tetrachloride mixed solution contains 20 wt % of vinyl caprolactam.
[0090] Example 4: A method for preparing a carbon / carbon PECVD carrier frame
[0091] The difference between this embodiment and embodiment 2 is that modified phenolic resin is used instead of phenolic resin.
[0092] Preparation of modified phenolic resin: Add phenol and barium hydroxide to formaldehyde solution, react at 60℃ for 1.5 h, at 73℃ for 2 h, at 85℃ for 25 min, add phenyltrimethoxysilane / methanol mixed solution and ammonia water, heat to 90℃, react until the solution becomes turbid, react for 25 min to stop the reaction, and rotary evaporate until there is no distillate to obtain modified phenolic resin. Among them, the formaldehyde solution contains 38 wt% formaldehyde; the molar ratio of phenol to formaldehyde is 1:1.2; the phenyltrimethoxysilane / methanol mixed solution contains 20 wt% phenyltrimethoxysilane; the mass fraction of ammonia water is 25%, the amount of ammonia water is 5 wt% of phenol, the molar ratio of phenol to phenyltrimethoxysilane is 1:0.2; the mass ratio of phenol to barium hydroxide is 1:0.05.
[0093] Example 5: A method for preparing a carbon / carbon PECVD carrier frame
[0094] The difference between this embodiment and embodiment 4 is that in the preparation of the modified phenolic resin, the molar ratio of phenol to phenyltrimethoxysilane is 1:0.3.
[0095] Comparative Example 1: Preparation method of a carbon / carbon PECVD carrier frame
[0096] S1, 3D puncture preform preparation: An automated robotic arm 3D puncture braiding machine was used to perform 3D puncture every 5 mm on a domestic 700-grade 3K carbon fiber cloth to prepare a 3D puncture preform with a density of 1.0 g / cm 3 Three-dimensional puncture preformed plate with left and right dimensions of 1200 mm*1300 mm*5.5 mm;
[0097] S2, resin vacuum introduction and autoclave resin pressure curing: the three-dimensional puncture plate preform is impregnated with phenolic resin by conventional resin vacuum introduction and autoclave processes, heated to 120°C, and pressurized to 0.2 MPa for curing, and the pores of the preform are completely filled with resin, so that the porosity of the plate reaches 1%;
[0098] S3, carbonization of the resin sheet: placing the solidified three-dimensional puncture resin sheet flat in a carbonization furnace, slowly heating it up and carbonizing it according to the carbonization curve of the phenol-formaldehyde resin, the carbonization temperature is 800°C, and then slowly cooling it down to room temperature;
[0099] S4, Chemical Vapor Deposition: The carbonized carbon / carbon sheet is hoisted in a chemical vapor deposition furnace for vapor deposition to make the sheet density reach the product density requirement of 1.63 g / cm 3 .
[0100] S5, machining to obtain a PECVD carbon / carbon support frame.
[0101] Comparative Example 2: Preparation method of a carbon / carbon PECVD carrier frame
[0102] The difference between this embodiment and embodiment 2 is that the vinyl caprolactam / carbon tetrachloride mixed solution contains 3 wt % of vinyl caprolactam.
[0103] Test Example 1:
[0104] 1. Infrared test
[0105] The FTIR spectrum of the sample was measured by the KBr pellet method using a NICOLET 5700 infrared spectrometer with a resolution of 6 cm -1 , test range 4000-500cm -1 , each sample was scanned 100 times.
[0106] The modified chopped carbon fiber and the desizing chopped carbon fiber prepared in Example 1 were subjected to infrared testing. The results are as follows: Figure 1 As shown, Figure 1 a is desizing chopped carbon fiber, b is modified chopped carbon fiber, which is composed of Figure 1 It can be seen that the modified chopped carbon fiber basically maintains the characteristics of the desizing chopped carbon fiber itself, but the 3310 cm -1 and 3180 cm -1 The characteristic absorption peak of NH appeared at 1620 cm -1 is C=O stretching vibration, 1460 cm -1 and 1420 cm -1 It is the characteristic absorption peak of CN stretching vibration, indicating that the grafting of vinyl caprolactam is successful.
[0107] Test Example 2:
[0108] 1. Mechanical properties test
[0109] The bending strength of the carbon / carbon PECVD bearing frames prepared in Examples 1-5 and Comparative Examples 1-2 was measured using an electronic universal testing machine Instron 5569. The three-point bending test method was used. The carbon / carbon PECVD bearing frames were cut into samples of 3 mm×4 mm×35 mm in size by an electric spark wire cutting machine. The span was 30 mm, and the pressure head loading speed was 0.5 mm / min. The obtained samples were tested in groups, with 5 in each group. The maximum load (N) during the loading process and at fracture was recorded through the obtained stress-strain curve, and the bending strength was obtained by theoretical calculation and averaging. The calculation formula for the three-point bending strength is: , where is the bending strength of the specimen (MPa), P is the maximum load when the specimen breaks (N), L is the specimen span (mm),b is the width of the specimen (mm), h is the specimen thickness (mm).
[0110] Figure 2 The bending strength of the carbon / carbon PECVD support frame prepared in Examples 1-5 and Comparative Examples 1-2 shows that the bending strength of the carbon / carbon PECVD support frame prepared in Examples 1-5 is greater than that in Comparative Example 1, indicating that the bending strength of the carbon / carbon PECVD support frame can be improved by using the preparation method of the present invention; the bending strength of Example 2 is greater than that of Example 1, indicating that replacing the chopped carbon fibers with the modified chopped carbon fibers prepared in the present invention can improve the bending strength of the carbon / carbon PECVD support frame; the bending strength of Example 3 is greater than that of Example 2, indicating that in the process of preparing the modified chopped carbon fibers, increasing the mass concentration of vinyl caprolactam can improve the bending strength of the carbon / carbon PECVD support frame; the bending strength of Example 4 is greater than that of Example 3, indicating that the bending strength of the carbon / carbon PECVD support frame can be improved by modifying the phenolic resin; the bending strength of Example 5 is greater than that of Example 4, indicating that adjusting the molar ratio of phenol to phenyltrimethoxysilane can improve the bending strength of the carbon / carbon PECVD support frame. The bending strength of Example 1 and Comparative Example 2 is substantially the same, indicating that in the process of preparing the modified chopped carbon fibers, a certain mass concentration of vinyl caprolactam needs to be used for modification, otherwise there is no better performance improvement effect.
[0111] 2. Line ablation rate test
[0112] The carbon / carbon PECVD carrier frames prepared in Experimental Examples 1-5 and Comparative Examples 1-2 were cut into φ20×10mm cylinders and placed in a mold. After vacuum cracking and surface oxidation treatment, the ablation performance of the samples was examined using an oxyacetylene test. The temperature change during the ablation of the samples was measured. The linear ablation rate was calculated using the formula R 1: , where R 1 is the burning rate of the sample line (mm / s), is the thickness of the sample before burning (mm), is the thickness of the sample after burning (mm), t is the burning time (s). The flame temperature is 2000℃, the gas flow rate is 1200 L / h for oxygen, 850 L / h for acetylene and 1300 L / h for oxygen, 950 L / h for acetylene, the distance between the nozzle and the sample is 30±0.2mm, and the test time is 400 s.
[0113] Figure 3The wire ablation rate of the carbon / carbon PECVD support frame prepared in Examples 1-5 and Comparative Examples 1-2 shows that the wire ablation rate of the carbon / carbon PECVD support frame prepared in Examples 1-5 is less than that in Comparative Example 1, indicating that the preparation method of the present invention can reduce the wire ablation rate of the carbon / carbon PECVD support frame; the wire ablation rate of Example 2 is less than that of Example 1, indicating that replacing the chopped carbon fibers with the modified chopped carbon fibers prepared in the present invention can reduce the wire ablation rate of the carbon / carbon PECVD support frame; the wire ablation rate of Example 3 is less than that of Example 2, indicating that in the process of preparing the modified chopped carbon fibers, increasing the mass concentration of vinyl caprolactam can reduce the wire ablation rate of the carbon / carbon PECVD support frame; the wire ablation rate of Example 4 is greater than that of Example 3, indicating that the modification of the phenolic resin can reduce the wire ablation rate of the carbon / carbon PECVD support frame; the wire ablation rate of Example 5 is less than that of Example 4, indicating that adjusting the molar ratio of phenol to phenyltrimethoxysilane can reduce the wire ablation rate of the carbon / carbon PECVD support frame. The linear ablation rates of Example 1 and Comparative Example 2 are not much different, indicating that in the process of preparing the modified chopped carbon fibers, a certain mass concentration of vinyl caprolactam needs to be used for modification, otherwise there will be no better performance improvement effect.
[0114] The embodiments and / or implementation methods described above are only used to illustrate the preferred embodiments and / or implementation methods for realizing the technology of the present invention, and are not intended to limit the implementation methods of the technology of the present invention in any form. Any technical personnel in this field may make slight changes or modifications to other equivalent embodiments without departing from the scope of the technical means disclosed in the content of the present invention, but they should still be regarded as technologies or embodiments that are essentially the same as the present invention.
Claims
1. A method for preparing a carbon / carbon PECVD carrier frame, characterized in that: The following steps are involved: The composite raw material is added into the resin glue to prepare a mixed slurry, and a carbon fiber composite material sheet is obtained by injection molding process, and then a carbon-carbon composite material sheet is obtained by carbonization and liquid phase impregnation resin treatment, and finally a carbon / carbon PECVD carrier frame is obtained by high temperature graphitization treatment, pyrolytic carbon coating treatment and purification treatment; The composite raw material includes modified chopped carbon fibers, wherein the modified chopped carbon fibers include chopped carbon fibers and a vinyl caprolactam structure grafted on the surface thereof, the resin in the resin glue is a modified phenolic resin, and the resin in the liquid phase impregnation resin is a modified phenolic resin; In the preparation of the modified phenolic resin, phenol and barium hydroxide are added to the formaldehyde solution, reacted at 50-70°C for 1-3 h, reacted at 65-75°C for 1-3 h, reacted at 75-90°C for 15-30 min, phenyltrimethoxysilane / methanol mixed solution and ammonia water are added, the temperature is raised to 80-95°C, reacted until the solution becomes turbid, reacted for another 20-30 min to stop the reaction, and rotary evaporation is performed until no more distilled products are produced, thereby obtaining the modified phenolic resin; In the preparation of modified chopped carbon fibers, desizing chopped carbon fibers are prepared, oxidized, and chlorinated; The acyl chloride chopped carbon fibers are added to a mixed solution of ethylene glycol / triethylamine, refluxed at 60-80°C for 35-55 h, and after the reflux is completed, the carbon fibers are taken out, washed, and dried to obtain alcoholysis chopped carbon fibers. The alcoholysis chopped carbon fibers are added to a mixed solution of vinyl caprolactam / carbon tetrachloride, ammonium cerium nitrate is added, and the mixture is reacted at 30-50°C for 3-6 h to obtain modified chopped carbon fibers.
2. The preparation method according to claim 1, characterized in that: The mixed slurry also includes an additive; the additive is at least one of flake graphite or silicon powder.
3. The preparation method according to claim 2, characterized in that: In the mixed slurry, by weight, the amount of modified chopped carbon fiber is 10-30 parts, the amount of resin glue is 40-60 parts, and the amount of additives is 5-20 parts.
4. The preparation method according to claim 1, characterized in that: The density of the carbon fiber composite material plate is ≥1.5 g / cm 3 .
5. The preparation method according to claim 1, characterized in that: The carbonization temperature is 900-950°C and the time is 1-3 h; the liquid phase impregnation resin treatment temperature is 120-200°C, the pressure is 2-4 MPa and the time is 1-3 h.
6. The preparation method according to claim 1, characterized in that: The temperature of the high-temperature graphitization treatment is 2000-2500°C, and the time of the high-temperature graphitization treatment is 1-3 h; the conditions for the pyrolytic carbon coating treatment are to introduce hydrocarbons, use nitrogen as the dilution gas, the volume ratio of hydrocarbons to nitrogen is 100:20-40, control the furnace pressure to 2000-4000 Pa, the temperature to 1000-1150°C, and treat for 10-30 h, and the hydrocarbons include natural gas or propane.
7. The preparation method according to claim 1, characterized in that: The purified gas used in the purification process is halogenated alkane with a concentration of 1-10 kg / m 3 The purification treatment temperature is 1800-2400° C., the purification treatment time is 2-4 h, and the halogenated alkane includes carbon hexafluoride.
8. A carbon / carbon PECVD carrier frame prepared by the method of any one of claims 1 to 7.
9. Use of the carbon / carbon PECVD carrier frame according to claim 8 in carrying silicon wafers for coating.