TPU for high-speed rail track shock-absorbing pad and preparation method thereof
Through the combination of polyamide-modified polyol and silicon carbide, the hydrolysis, heat and high-temperature wear resistance of TPU is improved, and the shortcomings of TPU in hydrolysis, heat and high-temperature wear resistance are solved, and the mechanical properties are achieved. Thermal conductivity.
Patent Information
- Application Number
- CN202410928653.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing TPUs have shortcomings in hydrolysis resistance, heat resistance and high-temperature wear resistance, especially compression deformation and high-temperature wear resistance.
Polyamide-modified polyol and silicon carbide are used as the main raw materials to improve the mechanical properties and chemical resistance of the TPU by adjusting the molecular structure and additive combination, and high-speed rail shock absorbing pads are prepared through the granulation process of twin-screw extruder.
It significantly improves the thermal deformation temperature, hydrolysis resistance and high-temperature wear performance of TPU, increases tensile strength by 20%, reduces high-temperature wear by more than 50%, thermal conductivity reaches 1.4w·(mk)-1, and hydrolysis retention rate is ≥90%. .
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermoplastic polyurethane and its preparation, and particularly relates to TPU for high-speed railway track shock-absorbing pads and a preparation method thereof. Background Art
[0002] In the construction of railway tracks, it is necessary to consider the impact of high-speed, high-frequency and overloaded trains on the roadbed, roadbed substructure, track and dynamic stability. Therefore, in order to meet the requirements of high-speed railways for the roadbed system, railway builders introduced high-speed railway shock-absorbing pads. High-speed railway shock-absorbing pads are special pads used for laying high-speed railway tracks. Compared with traditional concrete roadbeds, high-speed railway shock-absorbing pads have the advantages of shock absorption and noise reduction, roadbed protection and improved safety performance.
[0003] Thermoplastic polyurethane elastomer (TPU) is a high-molecular synthetic material with excellent performance and a wide range of hardness. It has both the elasticity of rubber and the hardness of plastic. It also has the advantages of good resilience, impact resistance, bending fatigue resistance, wear resistance, and dimensional stability. In particular, polyester TPU has high strength and excellent solvent resistance, making it an ideal shock-absorbing pad material. However, its hydrolysis resistance and heat resistance are somewhat lacking, and its compression deformation and wear resistance, especially high-temperature wear resistance, need to be further improved.
[0004] CN107383368A discloses a polyester polyol containing amide groups and its application in the preparation of polyurethane, wherein a lactam is added with a molecular weight regulator for ring-opening polymerization, and then an alkyd, an amine or a diol is used for end-capping to obtain a polyester polyol containing amide groups. CN109880081A discloses the preparation of a polyester polyol containing a polyamide segment, wherein a high-rigidity polyamide segment is introduced into the polyester polyol, so that the downstream product of the polyester polyol has excellent heat resistance and hydrolysis resistance, and at the same time, a side group or an aromatic ring can be introduced into the main chain of the polyester polyol to adjust the ratio of the polyamide segment to the polyester segment in the main chain of the polyester polyol, thereby improving the mechanical properties. Although the above two patents can improve the heat resistance and hydrolysis resistance of TPU to a certain extent, they do not solve the problem of improving the compression deformation and high-temperature wear resistance of polyester-type TPU.
[0005] CN114316198A discloses a vibration-damping polyurethane elastomer material for rail transit and a preparation method thereof, comprising a terminal hydroxyl hyperbranched polymer, a flame retardant, a catalyst, a chain extender, and an isocyanate. By adjusting the ratio of the soft and hard segments in the molecular structure, on the one hand, the tensile stress can be effectively reduced; on the other hand, the original vibration-damping and buffering effect of the pad will not be affected by the polyurethane elastomer material replacing the polyethylene foam material. Although the use of hyperbranched terminal hydroxyl hyperbranched polymer to synthesize polyurethane elastomer improves the permanent compression deformation of the material, the branching degree of the polymer is too high, which destroys the regularity of the soft segment structure, is not conducive to crystallization, and reduces the mechanical strength of the polyurethane material. Summary of the invention
[0006] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide TPU for high-speed rail track shock-absorbing pads, which has excellent mechanical properties, low temperature resistance, chemical resistance, and good hydrolysis resistance, and improves high-temperature wear resistance. The present invention also provides a preparation method thereof, which is simple and easy.
[0007] The TPU for high-speed rail track shock-absorbing pads of the present invention comprises the following raw material components in parts by weight:
[0008] Diisocyanate: 25-36.1 parts;
[0009] Polyamide modified polyol: 52.5-68 parts;
[0010] Chain extender: 6.9-11.4 parts;
[0011] Silicon carbide: 0.2-0.5 parts;
[0012] Antioxidant: 0.1-0.5 parts;
[0013] Hydrolysis stabilizer: 0.3-1 part;
[0014] Catalyst: 0.5-1 part;
[0015] The polyamide modified polyol is composed of raw materials of dibasic acid, diamine and small molecule alcohol, and has a number average molecular weight of 2000-3000; wherein the dibasic acid is one of succinic acid, adipic acid and sebacic acid; the diamine is one of butanediamine, hexamethylenediamine and decanediamine; the small molecule alcohol is a mixture of diol and trimethylolpropane; the diol is one of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol.
[0016] The diisocyanate is one of 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.
[0017] The chain extender is one of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol.
[0018] The silicon carbide has an average particle size of 20-50 μm, a purity of ≥99wt%, and is in powder form.
[0019] The antioxidant is one of antioxidant 1010, antioxidant 1024 and antioxidant 264.
[0020] The hydrolysis stabilizer is a monomeric carbodiimide or a polycarbodiimide.
[0021] The catalyst is one of dibutyltin dilaurate and stannous octoate or a mixture of the two.
[0022] The method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0023] (1) Mixing polyamide modified polyol and chain extender, and then sequentially adding antioxidant and hydrolysis stabilizer and stirring at 80-110° C. to obtain a premix;
[0024] (2) adding diisocyanate and catalyst into storage tank A, adding the premix of step (1) into storage tank B, mixing the materials in storage tank A and storage tank B, dehydrating under vacuum under stirring conditions, and pumping into a twin-screw extruder;
[0025] (3) Add silicon carbide to the second zone of the screw, react in a twin-screw extruder at 110-190° C., and granulate to obtain TPU particles for high-speed rail track shock-absorbing pads.
[0026] In step (2), the stirring rate is 400-800 r / min, and the vacuum dehydration temperature is 90-120°C.
[0027] In step (3), the feeding section temperature of the twin-screw extruder is 110-120°C, the mixing section temperature is 130-150°C, the extrusion section temperature is 170-180°C, and the die head temperature is 150-160°C.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The thermal conductivity of the TPU used in the high-speed rail track shock-absorbing pad of the present invention can reach 1.4w·(mk) -1 Above, the thermal transition temperature increased by about 16 °C, and the 14-day hydrolysis retention rate of the double 85 system was ≥90%.
[0030] (2) The tensile strength of the TPU used in the high-speed rail track shock-absorbing pad of the present invention is 20% higher than that of the traditional TPU, and the high-temperature wear is reduced by more than 50%. DETAILED DESCRIPTION
[0031] The present invention will be further described below in conjunction with specific embodiments.
[0032] Specifically, the method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0033] (1) Mixing polyamide modified polyol and chain extender, and then sequentially adding antioxidant and hydrolysis stabilizer and stirring at 80-110° C. to obtain a premix;
[0034] (2) adding diisocyanate and catalyst into storage tank A, adding the premix of step (1) into storage tank B, mixing the materials in storage tank A and storage tank B, dehydrating under vacuum at 90-120° C. under stirring conditions of 400-800 r / min, and injecting into a twin-screw extruder;
[0035] (3) Add silicon carbide to the second zone of the screw and react in a twin-screw extruder. The feeding section temperature of the twin-screw extruder is 110-120°C, the mixing section temperature is 130-150°C, the extrusion section temperature is 170-180°C, and the head temperature is 150-160°C. Granulation is performed to obtain TPU particles for high-speed rail track shock-absorbing pads.
[0036] The raw materials used in the following examples and comparative examples are all normal commercially available products.
[0037] The silicon carbide used below has an average particle size of 20-50 μm and a purity of ≥99 wt %, and is commercially available from Shanghai Baishun Biotechnology Co., Ltd.
[0038] The preparation steps of the polyamide modified polyol are as follows: a measured dibasic acid and a diamine are mixed in a reaction kettle, the temperature is raised to 160°C for reaction for 2 hours, and a carboxyl-terminated polyamide and a dibasic acid mixed solution are obtained; then, diol and trimethylolpropane are added into the reaction kettle, the temperature is raised to 200°C for 2 hours, a catalyst tetrabutyl titanate is added, the temperature is maintained for reaction until the hydroxyl value and the acid value are qualified, the temperature is lowered to stop the reaction, and a polyamide modified polyester polyol is obtained.
[0039] Monomeric carbodiimide: Shanghai Langyi Functional Materials Co., Ltd., HyMax®1010.
[0040] Polycarbodiimide: LANXESS Chemical (China) Co., Ltd., Stabaxol P 200.
[0041] The following weight parts are all calculated according to the same mass unit.
[0042] Example 1
[0043] The TPU for high-speed rail track shock-absorbing pads comprises the following raw material components in parts by weight:
[0044] 4,4'-diphenylmethane diisocyanate: 25 parts;
[0045] Polyamide modified polyol: 68 parts;
[0046] 1,4-Butanediol: 7 parts;
[0047] Silicon carbide: 0.4 parts;
[0048] Antioxidant 1010: 0.3 parts;
[0049] Monomeric carbodiimide: 0.5 parts;
[0050] Stannous octoate: 0.8 parts;
[0051] The polyamide modified polyol has a dibasic acid of adipic acid, a diamine of butanediamine, a small molecule alcohol of a mixture of 1,4-butanediol and trimethylolpropane, a number average molecular weight of 3000, and a functionality of 2.005; and an average particle size of silicon carbide powder particles of 30 μm.
[0052] The method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0053] (1) Mix polyamide-modified polyol and 1,4-butanediol, then add antioxidant 1010 and monomer carbodiimide in sequence, and stir thoroughly at 90° C. to obtain a premix;
[0054] (2) Add 4,4'-diphenylmethane diisocyanate and stannous octoate into storage tank A, add the premix of step (1) into storage tank B, stir at a rate of 500 r / min, vacuum dehydrate at 110°C, and pump into a twin-screw extruder;
[0055] (3) Silicon carbide powder is added to the second zone of the screw through an external device, reacted in a twin-screw extruder, and granulated to obtain TPU particles for high-speed rail track shock-absorbing pads; wherein the feeding section temperature of the twin-screw extruder is 110°C, the mixing section temperature is 130°C, the extrusion section temperature is 170°C, and the head temperature is 150°C.
[0056] Example 2
[0057] The TPU for high-speed rail track shock-absorbing pads comprises the following raw material components in parts by weight:
[0058] Hexamethylene diisocyanate: 28.1 parts;
[0059] Polyamide modified polyol: 65 parts;
[0060] 1,3-Propanediol: 6.9 parts;
[0061] Silicon carbide: 0.2 parts;
[0062] Antioxidant 1024: 0.5 parts;
[0063] Polycarbodiimide: 1 part;
[0064] Stannous octoate: 1 part;
[0065] The polyamide modified polyol has a dibasic acid of succinic acid, a diamine of hexamethylenediamine, a small molecule alcohol of a mixture of ethylene glycol and trimethylolpropane, a number average molecular weight of 2500, and a functionality of 2.008; and an average particle size of silicon carbide powder particles of 20 μm.
[0066] The method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0067] (1) Mixing polyamide-modified polyol and 1,3-propylene glycol, and then sequentially adding antioxidant 1024 and polycarbodiimide, and stirring thoroughly at 100° C. to obtain a premix;
[0068] (2) adding hexamethylene diisocyanate and stannous octoate into storage tank A, adding the premix of step (1) into storage tank B, stirring at a rate of 400 r / min, vacuum dehydrating at 100° C., and pumping into a twin-screw extruder;
[0069] (3) Silicon carbide powder is added to the second zone of the screw through an external device, reacted in a twin-screw extruder, and granulated to obtain TPU particles for high-speed rail track shock-absorbing pads; wherein the feeding section temperature of the twin-screw extruder is 120°C, the mixing section temperature is 150°C, the extrusion section temperature is 170°C, and the head temperature is 160°C.
[0070] Example 3
[0071] The TPU for high-speed rail track shock-absorbing pads comprises the following raw material components in parts by weight:
[0072] Isophorone diisocyanate: 30.7 parts;
[0073] Polyamide modified polyol: 60 parts;
[0074] Ethylene glycol: 9.3 parts;
[0075] Silicon carbide: 0.5 parts;
[0076] Antioxidant 264: 0.1 part;
[0077] Polycarbodiimide: 0.3 parts;
[0078] Dibutyltin dilaurate: 0.5 parts;
[0079] The polyamide modified polyol has a dibasic acid of sebacic acid, a diamine of decanediamine, a small molecule alcohol of a mixture of 1,3-propylene glycol and trimethylolpropane, a number average molecular weight of 2000, and a functionality of 2.01; and an average particle size of silicon carbide powder particles of 50 μm.
[0080] The method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0081] (1) Mixing polyamide-modified polyol and ethylene glycol, and then sequentially adding antioxidant 264 and polycarbodiimide, and fully stirring at 100° C. to obtain a premix;
[0082] (2) adding isophorone diisocyanate and dibutyltin dilaurate into storage tank A, adding the premix of step (1) into storage tank B, stirring at a speed of 600 r / min, vacuum dehydrating at 120° C., and pumping into a twin-screw extruder;
[0083] (3) Silicon carbide powder is added to the second zone of the screw through an external device, reacted in a twin-screw extruder, and granulated to obtain TPU particles for high-speed rail track shock-absorbing pads; wherein the feeding section temperature of the twin-screw extruder is 120°C, the mixing section temperature is 150°C, the extrusion section temperature is 180°C, and the head temperature is 160°C.
[0084] Example 4
[0085] The TPU for high-speed rail track shock-absorbing pads comprises the following raw material components in parts by weight:
[0086] 4,4'-diphenylmethane diisocyanate: 36.1 parts;
[0087] Polyamide modified polyol: 52.5 parts;
[0088] Ethylene glycol: 11.4 parts;
[0089] Silicon carbide: 0.4 parts;
[0090] Antioxidant 264: 0.2 parts;
[0091] Polycarbodiimide: 0.3 parts;
[0092] Dibutyltin dilaurate: 0.5 parts;
[0093] The polyamide modified polyol has a dibasic acid of sebacic acid, a diamine of decanediamine, a small molecule alcohol of a mixture of 1,3-propylene glycol and trimethylolpropane, a number average molecular weight of 2000, and a functionality of 2.006; and an average particle size of silicon carbide powder particles of 35 μm.
[0094] The method for preparing the TPU for the high-speed railway track shock-absorbing pad comprises the following steps:
[0095] (1) Mixing polyamide-modified polyol and ethylene glycol, and then sequentially adding antioxidant 264 and polycarbodiimide, and fully stirring at 100° C. to obtain a premix;
[0096] (2) Add 4,4'-diphenylmethane diisocyanate and dibutyltin dilaurate into storage tank A, add the premix of step (1) into storage tank B, stir at a speed of 500 r / min, vacuum dehydrate at 120°C, and pump into a twin-screw extruder;
[0097] (3) Silicon carbide powder is added to the second zone of the screw through an external device, reacted in a twin-screw extruder, and granulated to obtain TPU particles for high-speed rail track shock-absorbing pads; wherein the feeding section temperature of the twin-screw extruder is 120°C, the mixing section temperature is 150°C, the extrusion section temperature is 180°C, and the head temperature is 160°C.
[0098] Comparative Example 1
[0099] The TPU comprises the following raw material components in parts by weight:
[0100] 4,4'-diphenylmethane diisocyanate: 25 parts;
[0101] Polyamide modified polyol: 68 parts;
[0102] 1,4-Butanediol: 7 parts;
[0103] Silicon carbide: 0.4 parts;
[0104] Antioxidant 1010: 0.3 parts;
[0105] Monomeric carbodiimide: 0.5 parts;
[0106] Stannous octoate: 0.8 parts;
[0107] The dibasic acid of the polyamide modified polyol is adipic acid, the diamine is butanediamine, the small molecule alcohol is 1,4-butanediol, the number average molecular weight is 3000, the functionality is 2.00, and the average particle size of the silicon carbide powder particles is 30 μm. The preparation method is the same as that of Example 1.
[0108] Comparative Example 2
[0109] The TPU comprises the following raw material components in parts by weight:
[0110] 4,4'-diphenylmethane diisocyanate: 25 parts;
[0111] Polyamide modified polyol: 68 parts;
[0112] 1,4-Butanediol: 7 parts;
[0113] Antioxidant 1010: 0.3 parts;
[0114] Monomeric carbodiimide: 0.5 parts;
[0115] Stannous octoate: 0.8 parts;
[0116] The dibasic acid of the polyamide modified polyol is adipic acid, the diamine is butanediamine, the small molecule alcohol is a mixture of 1,4-butanediol and trimethylolpropane, the number average molecular weight is 3000, the functionality is 2.005; the average particle size of the silicon carbide powder particles is 30 μm. The preparation method is the same as that of Example 1.
[0117] Comparative Example 3
[0118] The TPU comprises the following raw material components in parts by weight:
[0119] 4,4'-diphenylmethane diisocyanate: 25 parts;
[0120] Polybutylene adipate polyol: 68 parts;
[0121] 1,4-Butanediol: 7 parts;
[0122] Silicon carbide: 0.4 parts;
[0123] Antioxidant 1010: 0.3 parts;
[0124] Monomeric carbodiimide: 0.5 parts;
[0125] Stannous octoate: 0.8 parts;
[0126] The preparation method is the same as that in Example 1.
[0127] The TPU particles obtained in the above examples and comparative examples were converted into test samples by injection molding, and their Shore hardness, mechanical properties, abrasion, thermal conductivity, heat deformation temperature, hydrolysis resistance, and permanent compression deformation were measured.
[0128] The tensile strength and tear strength are tested according to GB / T529-2009.
[0129] The hydrolysis retention rate is the percentage of the tensile strength of the tested material to the tensile strength of the material before the hydrolysis test when the material is placed in a constant temperature and humidity chamber with 85% humidity and 85°C for 14 days.
[0130] Abrasion, thermal conductivity and heat deformation temperature are tested according to ISO4649, ASTM D5470 and GB / T-1634B.
[0131] The permanent compression deformation was determined in accordance with GB / T7759.1-2015, at 70°C for 22 hours. The results are shown in Tables 1 and 2.
[0132] Table 1 TPU mechanical properties, abrasion, thermal wear test results
[0133]
[0134] Table 2 Thermal conductivity, hydrolysis resistance, thermal transition temperature and permanent compression deformation test results
[0135]
[0136] From the results in Table 1 and Table 2, it can be seen that the present invention uses polyamide modified polyol to introduce amide groups into the structure of polyester polyol, which can significantly improve the heat deformation temperature and hydrolysis resistance of TPU; increase the functionality of polyester polyol to produce micro-crosslinking of TPU and reduce the permanent compression deformation of the material; the thermal conductivity of silicon carbide is 80w·(mk) -1 Above, after adding silicon carbide to the material, the thermal conductivity of TPU is increased to 1.4w·(mk) -1 As mentioned above, the friction coefficient of the material increases with the increase of temperature. The temperature of the material increases during the friction process. The increase in thermal conductivity can accelerate the heat dissipation of the material. The combined effect of silicon carbide and multifunctional polyamide-modified polyols can significantly reduce the high-temperature wear of the product.
Claims
1. A TPU for high-speed rail track shock-absorbing pads, characterized by: The raw material components include the following parts by weight: Diisocyanate: 25-36.1 parts; Polyamide modified polyol: 52.5-68 parts; Chain extender: 6.9-11.4 parts; Silicon carbide: 0.2-0.5 parts; Antioxidant: 0.1-0.5 parts; Hydrolysis stabilizer: 0.3-1 part; Catalyst: 0.5-1 part; The polyamide modified polyol is composed of raw materials of dibasic acid, diamine and small molecule alcohol, and has a number average molecular weight of 2000-3000; wherein the dibasic acid is one of succinic acid, adipic acid and sebacic acid; the diamine is one of butanediamine, hexamethylenediamine and decanediamine; the small molecule alcohol is a mixture of diol and trimethylolpropane; the diol is one of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol; The preparation method of TPU for high-speed rail track shock-absorbing pads comprises the following steps: (1) Mixing polyamide modified polyol and chain extender, and then sequentially adding antioxidant and hydrolysis stabilizer and stirring at 80-110° C. to obtain a premix; (2) adding diisocyanate and catalyst into storage tank A, adding the premix of step (1) into storage tank B, mixing the materials in storage tank A and storage tank B, dehydrating under vacuum at 90-120° C. under stirring at a rate of 400-800 r / min, and injecting into a twin-screw extruder; (3) Add silicon carbide to the second zone of the screw and react in a twin-screw extruder at 110-190°C. The feeding section temperature of the twin-screw extruder is 110-120°C, the mixing section temperature is 130-150°C, the extrusion section temperature is 170-180°C, and the head temperature is 150-160°C. Granulation is performed to obtain TPU particles for high-speed rail track shock-absorbing pads.
2. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The diisocyanate is one of 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate and isophorone diisocyanate.
3. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The chain extender is one of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol.
4. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The average particle size of the silicon carbide is 20-50 μm, and the purity is ≥99wt%.
5. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The antioxidant is one of antioxidant 1010, antioxidant 1024 and antioxidant 264.
6. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The hydrolysis stabilizer is a monomeric carbodiimide or a polycarbodiimide.
7. The TPU for high-speed rail track shock-absorbing pad according to claim 1, characterized in that: The catalyst is one of dibutyltin dilaurate and stannous octoate or a mixture of the two.