A method for preparing functionalized graphene-modified ABS composite material
By introducing modified graphene and modified mica powder into ABS materials, its performance and service life in high temperature environments are improved, and the aging and performance degradation of ABS materials in electric faucet applications is solved, thus achieving higher Thermal deformation temperature, anti-aging and scratch resistance.
Patent Information
- Application Number
- CN202410507964.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-25
AI Technical Summary
ABS materials are prone to aging and deteriorating in high temperature environments, and their high molding shrinkage rate, low thermal deformation temperature and insufficient bending strength, limiting their service life and performance in applications such as electric hot faucets.
By blending graphene oxide with nano zinc oxide and modified mica powder, modifying graphene and modified mica powder are formed, which improves the thermal deformation temperature, anti-aging ability and mechanical properties of ABS composite materials, and uses ultrasound, Techniques such as radio frequency plasma discharge improve the dispersion and compatibility of materials.
It significantly improves the thermal deformation temperature, anti-aging properties, tensile strength, bending strength and scratch resistance of ABS composite materials, extends the service life of electric hot faucets and improves the surface aesthetics.
Smart Images

Figure BDA0004810845290000121
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a method for preparing a functionalized graphene-modified ABS composite material. Background Art
[0002] ABS (Acrylonitrile-Butadiene-Styrene Terpolymer) is an important engineering plastic. It is a polymer material obtained by copolymerizing three different monomers: acrylonitrile (Acrylonitrile, A), butadiene (Butadiene, B) and styrene (S). ABS is widely used in many fields such as automotive parts, electronic and electrical housings, household appliances, toys, sports equipment, office equipment, building materials, etc. However, the large molding shrinkage, low heat deformation temperature and low bending strength of ABS bring certain difficulties to the processing and post-assembly of products.
[0003] Related studies have shown that due to its extremely high specific surface area and excellent mechanical strength, graphene can be introduced into ABS resin to form an effective stress transfer network at the microscopic scale, significantly improving the tensile strength, bending strength and impact toughness of ABS materials; at the same time, graphene is also an excellent conductive material. Adding an appropriate amount of graphene can give the originally non-conductive or weakly conductive ABS resin conductive properties. The addition of graphene makes ABS composite materials have excellent mechanical, thermal, electrical and other comprehensive properties. However, directly incorporating graphene into the matrix is not conducive to the dispersion and compatibility of graphene in the ABS matrix. The structurally complete graphene is composed of benzene rings, has high chemical stability, is inert on the surface, and has weak interaction with other media. In addition, there is a strong van der Waals force between graphene sheets, which is easy to agglomerate, greatly limiting its research and application.
[0004] How to efficiently realize the modification of ABS materials with graphene is the key to preparing high-performance graphene-modified ABS composite materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a functionalized graphene-modified ABS composite material.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a functionalized graphene-modified ABS composite material, the method comprising the following steps, calculated by weight:
[0008] (1) adding 1 part of graphene oxide, 2-3 parts of nano zinc oxide, and 0.03-0.05 parts of silane coupling agent KH570 to 7-10 parts of 55% ethanol aqueous solution, ultrasonicating at 20-30kHz for 1.5-1.7h, filtering, and drying to obtain graphene oxide loaded with nano zinc oxide;
[0009] (2) mixing 1 part of graphene oxide loaded with nano zinc oxide, 0.2-0.4 parts of hexadecylamine, 0.1-0.3 parts of silane coupling agent KH550 and 10-12 parts of water, stirring at 30-35° C. for 20-30 min, continuing to heat to 80-85° C., stirring for 80-100 min, centrifuging and drying to obtain modified graphene;
[0010] (3) mixing 70-75 parts of ABS, 6-13 parts of polybutylene terephthalate, 15-19 parts of polycarbonate, 4-7 parts of modified graphene, 3-6 parts of modified mica powder, 0.5-1 parts of antioxidant, 1-2 parts of lubricant and 2-3 parts of toughening agent, and stirring at 210-230° C. for 15-20 minutes to obtain a mixture;
[0011] (4) The mixed material is fed into a twin-screw extruder, and subjected to extrusion, cooling, drying, and granulation to obtain a functionalized graphene-modified ABS composite material.
[0012] Furthermore, the graphene oxide has a particle size of 0.5 to 3 μm and a number of layers of 1 to 5. Beijing Dekedaojin Technology Co., Ltd.
[0013] Further, nano zinc oxide, average particle size 20nm, specific surface area 20-60㎡ / g. Zhejiang Zhitai Nano Micro New Materials Co., Ltd., model ZT-J20.
[0014] An electric water faucet is a device installed on a kitchen or bathroom sink that can quickly heat and convert cold water into hot water, and is very popular among consumers. One of its main components is a shell or internal structural parts made of heat-resistant materials. ABS has become an ideal raw material for the casing and internal parts of the electric water faucet due to its good heat resistance and impact resistance. However, the long-term heat resistance of ABS on the market is not ideal. Under continuous use, the ABS material may deform, soften or lose mechanical strength. Long-term exposure of ABS material to hot water environment may accelerate the aging and performance degradation of the material. The present invention improves the heat deformation temperature and aging resistance of the ABS composite material by compounding ABS with polybutylene terephthalate and polycarbonate, and adding modified graphene, especially graphene oxide with a specific particle size and number of layers. The analysis shows that by using the blending modification technology, PBT and PC are blended with ABS to form an interpenetrating network structure, which can produce a synergistic effect and improve the heat deformation temperature of the composite material. At the same time, the graphene oxide is loaded with nano zinc oxide and then coated with hexadecylamine. The nanoparticles can be evenly dispersed in the graphene oxide sheet, which can enhance the interface interaction and improve the heat conduction efficiency. At the same time, the graphene oxide and nano zinc oxide produce a synergistic effect, capture free radicals, and slow down the thermal oxidation degradation process of the polymer chain. The modified graphene can also improve the compatibility of ABS, polybutylene terephthalate, and polycarbonate, thereby improving the heat deformation temperature and anti-aging ability of the ABS composite material. The inventor unexpectedly discovered that under this condition, the tensile strength and bending strength of the ABS composite material are also improved.
[0015] Furthermore, the preparation method of the modified mica powder is: by weight,
[0016] S1: 10 parts of mica powder, 0.3-0.5 parts of silane coupling agent KH550 and 40-50 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 2-4 hours, filtered and dried to obtain pre-modified mica powder;
[0017] S2: Under vacuum conditions, radio frequency plasma discharge is used to polymerize and coat the composite monomer on the surface of the pre-modified mica powder to obtain modified mica powder.
[0018] Furthermore, the composite monomer is a mixture of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 0.4-0.8:1:1.3-1.7.
[0019] Furthermore, the vacuum degree of the vacuum condition is 70-90Pa.
[0020] Furthermore, the radio frequency of the radio frequency plasma is 12-13 MHz, the output power is 150-170 W, and the discharge time is 90-100 s.
[0021] Furthermore, the mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.4-1.7:0.3-0.6. Shijiazhuang Chenxing Industrial Co., Ltd.
[0022] Furthermore, the antioxidant is one or more of antioxidant 245, antioxidant 1076, and antioxidant 168.
[0023] Furthermore, the toughening agent is methyl methacrylate-butadiene-styrene copolymer. Brand: Nippon Electric Chemical, product model TP-SX.
[0024] Furthermore, the lubricant is one or a combination of glyceryl monostearate, glyceryl tristearate, ethylene bisstearamide, and ethylene bislauramide.
[0025] Mica has good heat resistance and helps to improve the heat deformation temperature and thermal stability of ABS resin. However, the inventors found that the interface compatibility was poor when mica powder was added to the ABS system. After the inventors modified the mica powder, the compatibility of the mica powder in the system was improved, and the heat resistance of the mica powder to ABS resin was improved. At the same time, the inventors unexpectedly found that adding modified mica powder can also improve the scratch resistance of ABS composite materials, which can solve the problem of surface scratches affecting the appearance of electric faucets after long-term use and extend the service life. The analysis shows that mica powder is more evenly dispersed in the resin mixture, and the groups introduced on the surface can enhance the interface bonding with the resin matrix composed of ABS, polybutylene terephthalate, and polycarbonate, increase the density, reduce micropores, and thus improve the scratch resistance.
[0026] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0027] 1. The ABS composite material of the present invention has excellent heat deformation temperature, aging resistance, mechanical properties and scratch resistance, and can be used to prepare materials for electric water faucets, thereby extending the service life and making the faucets more beautiful during use.
[0028] 2. The present invention improves the heat deformation temperature and anti-aging ability of the ABS composite material by adding modified graphene. The tensile strength and bending strength of the ABS composite material are also improved.
[0029] 3. After the inventor modified the mica powder, the compatibility of the mica powder in the system was improved, and the heat resistance of the mica powder to the ABS resin was improved. The scratch resistance of the ABS composite material can be improved, and the problem of surface scratches affecting the appearance of the electric faucet after long-term use can be solved. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Example 1
[0032] This embodiment provides a method for preparing a functionalized graphene-modified ABS composite material. The preparation method comprises the following steps, calculated by weight:
[0033] (1) adding 1 part of graphene oxide, 2.4 parts of nano zinc oxide, and 0.04 parts of silane coupling agent KH570 to 8 parts of 55% ethanol aqueous solution, ultrasonicating at 25 kHz for 1.6 hours, filtering, and drying to obtain graphene oxide loaded with nano zinc oxide;
[0034] (2) mixing 1 part of graphene oxide loaded with nano zinc oxide, 0.3 part of hexadecylamine, 0.2 part of silane coupling agent KH550 and 11 parts of water, stirring at 33° C. for 25 min, heating to 82° C., stirring for 90 min, centrifuging and drying to obtain modified graphene;
[0035] (3) 72 parts of ABS, 9 parts of polybutylene terephthalate, 17 parts of polycarbonate, 6 parts of modified graphene, 5 parts of modified mica powder, 0.7 parts of antioxidant, 1.4 parts of lubricant and 2.6 parts of toughening agent were mixed, and stirred at 220° C. for 18 min to obtain a mixture;
[0036] (4) The mixed material is fed into a twin-screw extruder, and subjected to extrusion, cooling, drying, and granulation to obtain a functionalized graphene-modified ABS composite material.
[0037] ABS, Brand: Chimei Industrial, PA-707ABS.
[0038] Polybutylene terephthalate, MacLean, P909269.
[0039] Polycarbonate, Wanhua Chemical, FR3730.
[0040] The graphene oxide has a particle size of 0.5 to 3 μm and a number of layers of 1 to 5. Beijing Dekedaojin Technology Co., Ltd.
[0041] Nano zinc oxide, average particle size 20nm, specific surface area 20-60㎡ / g. Zhejiang Zhitai Nano New Materials Co., Ltd., model ZT-J20.
[0042] The preparation method of the modified mica powder is as follows: by weight:
[0043] S1: 10 parts of mica powder, 0.4 parts of silane coupling agent KH550 and 45 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 3 hours, filtered and dried to obtain pre-modified mica powder;
[0044] S2: Under vacuum conditions, radio frequency plasma discharge is used to polymerize and coat the composite monomer on the surface of the pre-modified mica powder to obtain modified mica powder.
[0045] The composite monomer is a mixture of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 0.6:1:1.5.
[0046] The vacuum degree of the vacuum condition is 80Pa.
[0047] The radio frequency of the radio frequency plasma is 13 MHz, the output power is 160 W, and the discharge time is 95 s.
[0048] The mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.6:0.4. Shijiazhuang Chenxing Industrial Co., Ltd.
[0049] The antioxidant is antioxidant 245. Brand: BASF.
[0050] The toughening agent is methyl methacrylate-butadiene-styrene copolymer. Brand: Nippon Electric Chemical, product model TP-SX.
[0051] The lubricant is glyceryl monostearate. CAS: 123-94-4.
[0052] Example 2
[0053] This embodiment provides a method for preparing a functionalized graphene-modified ABS composite material. The preparation method comprises the following steps, calculated by weight:
[0054] (1) adding 1 part of graphene oxide, 2 parts of nano zinc oxide, and 0.03 parts of silane coupling agent KH570 to 7 parts of 55% ethanol aqueous solution, ultrasonicating at 20 kHz for 1.5 h, filtering, and drying to obtain graphene oxide loaded with nano zinc oxide;
[0055] (2) mixing 1 part of graphene oxide loaded with nano zinc oxide, 0.2 parts of hexadecylamine, 0.1 parts of silane coupling agent KH550 and 10 parts of water, stirring at 30° C. for 20 min, heating to 80° C., stirring for 80 min, centrifuging and drying to obtain modified graphene;
[0056] (3) 70 parts of ABS, 6 parts of polybutylene terephthalate, 15 parts of polycarbonate, 4 parts of modified graphene, 3 parts of modified mica powder, 0.5 parts of antioxidant, 1 part of lubricant and 2 parts of toughening agent were mixed, and stirred at 210° C. for 15 min to obtain a mixture;
[0057] (4) The mixed material is fed into a twin-screw extruder, and subjected to extrusion, cooling, drying, and granulation to obtain a functionalized graphene-modified ABS composite material.
[0058] ABS, Brand: Chimei Industrial, PA-707ABS.
[0059] Polybutylene terephthalate, MacLean, P909269.
[0060] Polycarbonate, Wanhua Chemical, FR3730.
[0061] The graphene oxide has a particle size of 0.5 to 3 μm and a number of layers of 1 to 5. Beijing Dekedaojin Technology Co., Ltd.
[0062] Nano zinc oxide, average particle size 20nm, specific surface area 20-60㎡ / g. Zhejiang Zhitai Nano New Materials Co., Ltd., model ZT-J20.
[0063] The preparation method of the modified mica powder is as follows: by weight:
[0064] S1: 10 parts of mica powder, 0.3 parts of silane coupling agent KH550 and 40 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 2 h, filtered and dried to obtain pre-modified mica powder;
[0065] S2: Under vacuum conditions, radio frequency plasma discharge is used to polymerize and coat the composite monomer on the surface of the pre-modified mica powder to obtain modified mica powder.
[0066] The composite monomer is a mixture of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 0.4:1:1.3.
[0067] The vacuum degree of the vacuum condition is 70Pa.
[0068] The radio frequency of the radio frequency plasma is 12 MHz, the output power is 150 W, and the discharge time is 90 s.
[0069] The mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.4:0.3. Shijiazhuang Chenxing Industrial Co., Ltd.
[0070] The antioxidant is antioxidant 1076. Brand: BASF.
[0071] The toughening agent is methyl methacrylate-butadiene-styrene copolymer. Brand: Nippon Electric Chemical, product model TP-SX.
[0072] The lubricant is tristearate glyceryl. CAS: 555-43-1.
[0073] Example 3
[0074] This embodiment provides a method for preparing a functionalized graphene-modified ABS composite material. The preparation method comprises the following steps, calculated by weight:
[0075] (1) adding 1 part of graphene oxide, 3 parts of nano zinc oxide, and 0.05 parts of silane coupling agent KH570 to 10 parts of 55% ethanol aqueous solution, ultrasonicating at 30kHz for 1.7h, filtering, and drying to obtain graphene oxide loaded with nano zinc oxide;
[0076] (2) mixing 1 part of graphene oxide loaded with nano zinc oxide, 0.4 part of hexadecylamine, 0.3 part of silane coupling agent KH550 and 12 parts of water, stirring at 35° C. for 30 min, heating to 85° C., stirring for 100 min, centrifuging and drying to obtain modified graphene;
[0077] (3) 75 parts of ABS, 13 parts of polybutylene terephthalate, 19 parts of polycarbonate, 7 parts of modified graphene, 6 parts of modified mica powder, 1 part of antioxidant, 2 parts of lubricant and 3 parts of toughening agent were mixed, and stirred at 230° C. for 20 min to obtain a mixture;
[0078] (4) The mixed material is fed into a twin-screw extruder, and subjected to extrusion, cooling, drying, and granulation to obtain a functionalized graphene-modified ABS composite material.
[0079] ABS, Brand: Chimei Industrial, PA-707ABS.
[0080] Polybutylene terephthalate, MacLean, P909269.
[0081] Polycarbonate, Wanhua Chemical, FR3730.
[0082] The graphene oxide has a particle size of 0.5 to 3 μm and a number of layers of 1 to 5. Beijing Dekedaojin Technology Co., Ltd.
[0083] Nano zinc oxide, average particle size 20nm, specific surface area 20-60㎡ / g. Zhejiang Zhitai Nano New Materials Co., Ltd., model ZT-J20.
[0084] The preparation method of the modified mica powder is as follows: by weight:
[0085] S1: 10 parts of mica powder, 0.5 parts of silane coupling agent KH550 and 50 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 4 hours, filtered and dried to obtain pre-modified mica powder;
[0086] S2: Under vacuum conditions, radio frequency plasma discharge is used to polymerize and coat the composite monomer on the surface of the pre-modified mica powder to obtain modified mica powder.
[0087] The composite monomer is a mixture of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 0.8:1:1.7.
[0088] The vacuum degree of the vacuum condition is 90Pa.
[0089] The radio frequency of the radio frequency plasma is 13 MHz, the output power is 170 W, and the discharge time is 100 s.
[0090] The mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.7:0.6. Shijiazhuang Chenxing Industrial Co., Ltd.
[0091] The antioxidant is antioxidant 168. Brand: BASF.
[0092] The toughening agent is methyl methacrylate-butadiene-styrene copolymer. Brand: Nippon Electric Chemical, product model TP-SX.
[0093] The lubricant is ethylene bislauramide. CAS: 7003-56-7.
[0094] Comparative Example 1
[0095] The difference between this comparative example and Example 1 is that the proportions of ABS, polybutylene terephthalate and polycarbonate are different.
[0096] Specifically, step (3): 68 parts of ABS, 19 parts of polybutylene terephthalate, 12 parts of polycarbonate, 6 parts of modified graphene, 5 parts of modified mica powder, 0.7 parts of antioxidant, 1.4 parts of lubricant and 2.6 parts of toughening agent are mixed, and stirred at 220° C. for 18 minutes to obtain a mixture.
[0097] Comparative Example 2
[0098] The difference between this comparative example and Example 1 is that polybutylene terephthalate and polycarbonate are replaced by epoxy resin and polymethyl methacrylate respectively.
[0099] Specifically, step (3): 72 parts of ABS, 9 parts of polymethyl methacrylate, 17 parts of epoxy resin, 6 parts of modified graphene, 5 parts of modified mica powder, 0.7 parts of antioxidant, 1.4 parts of lubricant and 2.6 parts of toughening agent are mixed, and stirred at 220° C. for 18 minutes to obtain a mixture.
[0100] Comparative Example 3
[0101] The difference between this comparative example and Example 1 is that the graphene oxide and the nano zinc oxide are different.
[0102] The graphene oxide has an average particle size of 5-10 μm and a number of layers of 15-20. Sigma-Aldrich.
[0103] Nano zinc oxide, average particle size 50nm, specific surface area 15-30㎡ / g. Zhejiang Zhitai Nano Micro New Materials Co., Ltd., model ZT-J50.
[0104] Comparative Example 4
[0105] The difference between this comparative example and Example 1 is that the preparation method of the modified mica powder is different.
[0106] The preparation method of the modified mica powder is as follows: by weight:
[0107] 10 parts of mica powder, 0.4 parts of silane coupling agent KH550 and 45 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 3 hours, filtered and dried to obtain modified mica powder.
[0108] The mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.6:0.4. Shijiazhuang Chenxing Industrial Co., Ltd.
[0109] Comparative Example 5
[0110] The difference between this comparative example and Example 1 is that the particle size of the mica powder is different.
[0111] The mica powder is mica powder with a D90 particle size of 10 μm. Shijiazhuang Chenxing Industrial Co., Ltd.
[0112] Comparative Example 6
[0113] The difference between this comparative example and Example 1 is that the composite monomer is a compound of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 1:1:1.
[0114] Performance Testing
[0115] The ABS composite materials of Examples 1-3 and Comparative Examples 1-6 were tested for performance:
[0116] 1. The tensile strength is tested according to the national standard GB / T1040.2-2006;
[0117] 2. The bending strength is tested according to the national standard GB / T9341-2000;
[0118] 3. The heat deformation temperature is tested in accordance with the national standard GB / T1634.2-2019;
[0119] 4. Scratch resistance: The composite material is injection molded into a high-gloss board, and a scratch test is performed on the sample using a Martindale scratch tester (refer to Volkswagen PV3975-2010 standard). The glossiness A0 of the sample before the scratch test and the glossiness A1 after the scratch test are tested using a gloss meter. The gloss retention rate of the sample after the test is calculated (A1 / A0)×100%. The higher the gloss retention rate, the better the scratch resistance.
[0120] 5. The aging resistance is measured by the national standard GB-T16422 xenon lamp accelerated aging test. Specifically, the mechanical properties test specimens are subjected to a xenon lamp accelerated aging test according to the standard GB29344. The color change before and after 1000h of xenon lamp aging is tested with a colorimeter, and the color difference ΔE is obtained.
[0121] Table 1 Performance test results
[0122]
[0123] The results show that the ABS composite materials prepared in Examples 1-3 have excellent comprehensive performance and are suitable for preparing electric faucets. When the preparation conditions are changed, the performance decreases to varying degrees.
[0124] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a functionalized graphene-modified ABS composite material, characterized in that: Calculated by weight, the preparation method comprises the following steps: (1) adding 1 part of graphene oxide, 2-3 parts of nano zinc oxide, and 0.03-0.05 parts of silane coupling agent KH570 to 7-10 parts of 55% ethanol aqueous solution, ultrasonicating at 20-30kHz for 1.5-1.7h, filtering, and drying to obtain graphene oxide loaded with nano zinc oxide; (2) mixing 1 part of graphene oxide loaded with nano zinc oxide, 0.2-0.4 parts of hexadecylamine, 0.1-0.3 parts of silane coupling agent KH550 and 10-12 parts of water, stirring at 30-35° C. for 20-30 min, continuing to heat to 80-85° C., stirring for 80-100 min, centrifuging and drying to obtain modified graphene; (3) mixing 70-75 parts of ABS, 6-13 parts of polybutylene terephthalate, 15-19 parts of polycarbonate, 4-7 parts of modified graphene, 3-6 parts of modified mica powder, 0.5-1 parts of antioxidant, 1-2 parts of lubricant and 2-3 parts of toughening agent, and stirring at 210-230° C. for 15-20 minutes to obtain a mixture; (4) feeding the mixed material into a twin-screw extruder, and performing extrusion, cooling, drying, and granulation to obtain a functionalized graphene-modified ABS composite material; The graphene oxide has a particle size of 0.5 to 3 μm and a number of layers of 1 to 5; Nano zinc oxide, average particle size 20nm, specific surface area 20-60m 2 / g; The preparation method of the modified mica powder is as follows: by weight: S1: 10 parts of mica powder, 0.3-0.5 parts of silane coupling agent KH550 and 40-50 parts of 50% by mass ethanol aqueous solution were mixed, stirred at 200 rpm for 2-4 hours, filtered and dried to obtain pre-modified mica powder; S2: Under vacuum conditions, radio frequency plasma discharge is used to polymerize and coat the composite monomer on the surface of the pre-modified mica powder to obtain modified mica powder; The composite monomer is a mixture of N-methylpyrrole, 1,3-propylenediamine and methacrylic acid in a mass ratio of 0.4-0.8:1:1.3-1.7; The mica powder is a compound of mica powder with a D90 particle size of 3 μm, mica powder with a D90 particle size of 6 μm, and mica powder with a D90 particle size of 10 μm in a mass ratio of 1:1.4-1.7:0.3-0.6; The toughening agent is methyl methacrylate-butadiene-styrene copolymer; The vacuum degree of the vacuum condition is 70-90Pa; The radio frequency of the radio frequency plasma is 12-13 MHz, the output power is 150-170 W, and the discharge time is 90-100 s.
2. The method for preparing the functionalized graphene-modified ABS composite material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 245, antioxidant 1076, and antioxidant 168.