A cable material for charging pile and preparation method thereof

By using thermoplastic polyurethane, microencapsulated ammonium polyphosphate and flame retardant and heat-retardant components in cable materials for charging piles, the problem that existing materials do not have both flame retardant, mechanical and moisture-heat resistance is solved, and a higher level of Flame retardancy, mechanical properties and water resistance meet the requirements of relevant standards.

CN118459973BActive Publication Date: 2024-12-03JIANGSU XINDE POLYMER MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410664574.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-12-03
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

The existing thermoplastic polyurethane materials do not have good flame retardant properties, mechanical properties and moisture and heat resistance in charging pile cables.

Method used

Using thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant synergistic components and molecular chain repair agents, cable materials are prepared through specific process steps, including amidation modification, reaction of melamine and stearoyl chloride, hydrothermal synthesis and Microcapsule coating and other technologies form flame retardant and synergistic components with isocyanate groups and alkyl long chains, improving the flame retardant and mechanical properties of the material.

Benefits of technology

It significantly improves the flame retardant properties, mechanical properties and moisture and heat resistance of cable materials, meets the requirements of GB/T 33594-2017 for thermoplastic polyurethane elastomer sheathing materials, extends the long-term flame retardant properties of the material and the physical properties after water aging. Retention rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004860715070000081
    Figure BDA0004860715070000081
  • Figure BDA0004860715070000091
    Figure BDA0004860715070000091
Patent Text Reader

Abstract

The invention discloses a cable material for a charging pile and a preparation method thereof, belonging to the technical field of cable materials. The cable material comprises the following raw materials in parts by weight: 60-90 parts of thermoplastic polyurethane, 3-5 parts of microencapsulated ammonium polyphosphate, 18-27 parts of flame retardant and synergistic components, 0.5-2 parts of molecular chain repair agents, and 0.5-2 parts of antioxidants. The cable material preparation method is as follows: thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic components, molecular chain repair agents and antioxidants are weighed in parts by weight, and mixed to obtain a mixture; the mixture is fed into a twin-screw extruder, and the mixture is extruded and granulated to obtain the cable material for the charging pile. The invention introduces the flame retardant and synergistic components and microencapsulated ammonium polyphosphate into the cable material, so that the obtained cable material meets the requirements of GB / T 33594-2017 electric vehicle charging cables for thermoplastic polyurethane elastomer sheath materials, and can be applied to charging pile cables and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of cable materials, and in particular relates to a cable material for a charging pile and a preparation method thereof. Background Art

[0002] In recent years, new energy vehicles have developed rapidly. Under such a background, the charging pile industry chain supporting electric vehicles has become a hot industry, and cables are an important part of charging piles. At present, the materials used to produce charging pile cable sheaths on the market mainly include TPE, TPU, and PVC elastomers. Among them, TPE materials have low density, good softness, and excellent environmental resistance, but poor oil resistance, poor dirt resistance, dust sticking, and sticky hands. PVC materials contain halogen elements and produce toxic substances after combustion, which is not environmentally friendly and healthy. Thermoplastic polyurethane (TPU) is a type of molecular chain containing urethane groups. The block copolymer thermoplastic elastomer has a unique molecular structure that makes TPU have excellent flexibility, mechanical strength and wear resistance, and is a suitable sheath material for flexible cables. Halogen-free flame retardant TPU material is prepared by introducing halogen-free flame retardant into TPU to meet the flame retardant requirements of cables. However, due to the poor compatibility of flame retardant with TPU body, the introduction of flame retardant improves the flame retardant properties of TPU sheath material, while the mechanical properties and moisture and heat resistance of the material are declining. Therefore, providing a thermoplastic polyurethane material with flame retardant, mechanical and moisture and heat resistance is a technical problem that needs to be solved at present. Summary of the invention

[0003] The object of the present invention is to provide a cable material for a charging pile and a preparation method thereof, so as to solve the problem that the existing thermoplastic polyurethane material for charging piles does not have good flame retardant properties, mechanical properties and moisture and heat resistance.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A cable material for a charging pile, comprising the following raw materials in parts by weight:

[0006] 60-90 parts of thermoplastic polyurethane, 3-5 parts of microencapsulated ammonium polyphosphate, 18-27 parts of flame retardant and synergistic components, 0.5-2 parts of molecular chain repair agents, and 0.5-2 parts of antioxidants.

[0007] Further, the flame retardant synergistic component is prepared by the following steps:

[0008] Step S1, adding melamine and n-hexane into a flask, stirring at 20°C and 200 r / min for 20 min, then dropping stearyl chloride, keeping the temperature for 1 h, allowing to stand for stratification, recovering n-hexane, washing the precipitate with distilled water, filtering it, and drying it to obtain product a;

[0009] Step S2, add product a and acetone to a flask, stir at 50° C. for 5-10 min, then add acetone solution of p-hydroxybenzaldehyde, after the addition is complete, heat to reflux for 6-8 h, then remove acetone by rotary evaporation to obtain product b;

[0010] Step S3, under nitrogen protection, add product b and toluene diisocyanate into a hydrothermal synthesis reactor with a polytetrafluoroethylene liner, stir for 5-10 minutes, place the hydrothermal synthesis reactor in an oven, react at 150° C. and 180° C. for 1 hour, respectively. After the reaction is completed, take out the reaction product and crush it, place the crushed product in a torque rheometer, and react at 180-200° C. for 3 hours to obtain a flame retardant synergistic component.

[0011] Firstly, melamine is amidated and modified with stearyl chloride to obtain product a containing a long alkyl chain and two amino groups. Then, the amino group of product a is subjected to condensation reaction with the aldehyde group of hydroxybenzaldehyde to obtain product b with phenolic hydroxyl group and Schiff base structure. Then, product b and toluene diisocyanate are used as raw materials, and the ratio of the two is controlled to obtain a flame retardant synergistic component with terminal isocyanate group.

[0012] Furthermore, in step S1, the molar ratio of melamine to stearyl chloride is 1:1.

[0013] Furthermore, in step S2, the mass ratio of product a to p-hydroxybenzaldehyde is 3.9:2.4.

[0014] Furthermore, in step S3, the mass ratio of product b to toluene diisocyanate is 6.3:1.7-2.2.

[0015] Further, microencapsulated ammonium polyphosphate is prepared by the following steps:

[0016] Add ammonium polyphosphate to the ethanol aqueous solution, stir evenly, then add ammonia water to adjust the pH value to 10, add 3-aminopropyltriethoxysilane and tetraethyl orthosilicate, stir for 10-20 minutes, transfer to a flask, react at 45°C for 2-3 hours, filter, wash the filter cake with anhydrous ethanol for 3 times, and finally dry at 80°C for 24 hours. The dosage ratio of the ethanol aqueous solution, ammonium polyphosphate, 3-aminopropyltriethoxysilane and tetraethyl orthosilicate is 350-450mL:100g:15-20g:15-20g, and the volume ratio of anhydrous ethanol to deionized water in the ethanol aqueous solution is 2:1. 3-aminopropyltriethoxysilane and tetraethyl orthosilicate are used as precursors, and the ammonium polyphosphate is microencapsulated and coated by a sol-gel process, so that the Si iOS i bond and amino group in the silicone are grafted to the surface of the ammonium polyphosphate, thereby improving the hydrophobicity and flame retardancy of the ammonium polyphosphate.

[0017] Furthermore, the antioxidant is one or more of antioxidant 1010 , antioxidant 1035 and antioxidant 1024 .

[0018] Furthermore, the molecular chain repair agent is bis(2,6-diisopropylphenyl)carbodiimide and / or bis(4-phenoxy-2,6-diisopropylphenyl)carbodiimide. The addition of the molecular chain repair agent can recouple the degraded thermoplastic polyurethane resin molecular chains under high temperature conditions, thereby effectively maintaining the molecular weight and physical properties of the high molecular weight thermoplastic polyurethane resin.

[0019] The method for preparing the above-mentioned cable material for charging pile comprises the following steps:

[0020] (1) Weighing thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic component, molecular chain repair agent and antioxidant according to weight, placing in a high-speed mixer, and mixing for 3-5 minutes to obtain a mixture;

[0021] (2) The mixed material is fed into a twin-screw extruder, and after extrusion and granulation, a cable material for a charging pile is obtained.

[0022] Further, the temperature of the twin-screw extruder is set to 140-200°C.

[0023] Beneficial effects of the present invention:

[0024] The present invention provides a cable material for a charging pile, which is prepared from thermoplastic polyurethane, microencapsulated ammonium polyphosphate, a flame retardant synergistic component, a molecular chain repair agent and an antioxidant. Compared with ammonium polyphosphate, microencapsulated ammonium polyphosphate has better dispersibility in a thermoplastic polyurethane system, and after microcapsule coating treatment, water resistance is improved, decomposition and migration of ammonium polyphosphate after water absorption are avoided, the problem of water absorption of ammonium polyphosphate is solved, and the long-term flame retardancy of the cable material and the retention rate of physical properties after water aging are improved. The shell layer of the microcapsule also has a P / N / S i synergistic flame retardant effect with the ammonium polyphosphate, which further improves the flame retardant performance of the cable material.

[0025] The flame retardant synergistic component contains isocyanate groups, which can form chemical bonds with thermoplastic polyurethane and microencapsulated ammonium polyphosphate to play a cross-linking role, thereby improving the microscopic bonding degree of the composite material and improving the mechanical properties of the composite material; the flame retardant synergistic component also contains structures such as triazine rings, Schiff bases and benzene rings, which on the one hand improve the heat resistance of the cable material, and on the other hand coordinate with microencapsulated ammonium polyphosphate to play a flame retardant role; in addition, the flame retardant synergistic component also carries a long alkyl chain and is hydrophobic, which can improve the water resistance of the cable material and meet the requirements for thermoplastic polyurethane elastomer sheath materials in GB / T 33594-2017 electric vehicle charging cables, and can be used in charging pile cables and other fields. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] This embodiment provides a flame retardant synergistic component, which is prepared by the following steps:

[0029] Step S1, adding 0.1 mol melamine and 120 mL n-hexane into a flask, stirring at 20° C. and 200 r / min for 20 min, then dropping 0.1 mol stearoyl chloride, keeping the temperature for 1 h, allowing the flask to stand for stratification, recovering the n-hexane, washing the precipitate with distilled water, filtering it, and drying it to obtain product a;

[0030] Step S2, add 3.9 g of product a and 40 mL of acetone to a flask, stir at 50° C. for 5 min, then add a solution consisting of 2.4 g of p-hydroxybenzaldehyde and 30 mL of acetone, and after the addition is complete, heat to reflux for 6 h, then remove acetone by rotary evaporation to obtain product b;

[0031] Step S3, under nitrogen protection, add 6.3g of product b and 1.7g of toluene diisocyanate into a hydrothermal synthesis reactor with a polytetrafluoroethylene liner, stir for 5 minutes, place the hydrothermal synthesis reactor in an oven, and react at 150°C and 180°C for 1h, respectively. After the reaction, take out the reaction product and crush it. The crushed product is placed in a torque rheometer and reacted at 180°C for 3h to obtain a flame retardant synergistic component.

[0032] Example 2

[0033] This embodiment provides a flame retardant synergistic component, which is prepared by the following steps:

[0034] Step S1, adding 0.1 mol melamine and 150 mL n-hexane into a flask, stirring at 20°C and 200 r / min for 20 min, then dropping 0.1 mol stearoyl chloride, keeping the temperature for reaction for 1 h, allowing to stand for stratification and recovering n-hexane, washing the precipitate with distilled water, filtering it, and drying it to obtain product a;

[0035] Step S2, add 3.9 g of product a and 60 mL of acetone to a flask, stir at 50° C. for 10 min, then add a solution consisting of 2.4 g of p-hydroxybenzaldehyde and 30 mL of acetone, after the addition is complete, heat to reflux for reaction for 8 h, then remove acetone by rotary evaporation to obtain product b;

[0036] Step S3, under nitrogen protection, add 6.3g of product b and 2.2g of toluene diisocyanate into a hydrothermal synthesis reactor with a polytetrafluoroethylene liner, stir for 10 minutes, place the hydrothermal synthesis reactor in an oven, and react at 150°C and 180°C for 1h, respectively. After the reaction, take out the reaction product and crush it, place the crushed product in a torque rheometer, and react at 200°C for 3h to obtain a flame retardant synergistic component.

[0037] Comparative Example 1

[0038] This embodiment provides a flame retardant synergistic component, which is prepared by the following steps:

[0039] Step S1, adding 0.1 mol melamine and 120 mL n-hexane into a flask, stirring at 20° C. and 200 r / min for 20 min, then dropping 0.1 mol stearoyl chloride, keeping the temperature for 1 h, allowing the flask to stand for stratification, recovering the n-hexane, washing the precipitate with distilled water, filtering it, and drying it to obtain product a;

[0040] Step S2, add 3.9 g of product a and 60 mL of acetone to a flask, stir at 50° C. for 10 min, then add a solution consisting of 2.4 g of p-hydroxybenzaldehyde and 30 mL of acetone. After the addition is complete, heat to reflux for 8 h, then remove the acetone by rotary evaporation to obtain a flame retardant synergistic component.

[0041] Example 3

[0042] This embodiment provides a microencapsulated ammonium polyphosphate, which is prepared by the following steps:

[0043] Add 100 g of ammonium polyphosphate to 350 mL of ethanol aqueous solution, stir evenly, then add ammonia water (28 wt%) dropwise to adjust the pH value to 10, add 15 g of 3-aminopropyltriethoxysilane and 15 g of ethyl orthosilicate, stir for 10 min, transfer to a flask, react at 45 ° C for 2 h, then filter, wash the filter cake with anhydrous ethanol 3 times, and finally dry at 80 ° C for 24 h. The volume ratio of anhydrous ethanol to deionized water in the ethanol aqueous solution is 2:1.

[0044] Example 4

[0045] This embodiment provides a microencapsulated ammonium polyphosphate, which is prepared by the following steps:

[0046] Add 100 g of ammonium polyphosphate to 450 mL of ethanol aqueous solution, stir evenly, then add ammonia water (28 wt%) to adjust the pH value to 10, add 20 g of 3-aminopropyltriethoxysilane and 20 g of ethyl orthosilicate, stir for 20 min, transfer to a flask, react at 45 ° C for 3 h, then filter, wash the filter cake with anhydrous ethanol 3 times, and finally dry at 80 ° C for 24 h. The volume ratio of anhydrous ethanol to deionized water in the ethanol aqueous solution is 2:1.

[0047] Comparative Example 2

[0048] This embodiment provides a microencapsulated ammonium polyphosphate. Compared with Example 3, only 3-aminopropyltriethoxysilane in Example 3 is replaced by methyltriethoxysilane, and the remaining raw materials and preparation process are the same as Example 3.

[0049] Comparative Example 3

[0050] This comparative example is ammonium polyphosphate.

[0051] Example 5

[0052] A cable material for a charging pile, comprising the following raw materials in parts by weight:

[0053] 60 parts of TPU 585A resin, 3 parts of microencapsulated ammonium polyphosphate according to Example 3, 18 parts of the flame retardant synergistic component according to Example 1, 0.5 parts of a molecular chain repair agent, and 0.5 parts of an antioxidant.

[0054] The antioxidant is antioxidant 1010, and the molecular chain repair agent is bis(2,6-diisopropylphenyl)carbodiimide.

[0055] The method for preparing the above-mentioned cable material for charging pile comprises the following steps:

[0056] (1) Weighing thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic component, molecular chain repair agent and antioxidant according to weight, placing in a high-speed mixer, and mixing for 3 minutes to obtain a mixture;

[0057] (2) The mixed material is fed into a twin-screw extruder, and after extrusion and granulation, the temperature zones 1 to 10 of the twin-screw extruder are set as follows: 160° C., 170° C., 180° C., 190° C., 195° C., 195° C., 195° C., 195° C., 195° C., 195° C., to obtain a cable material for a charging pile.

[0058] Example 6

[0059] A cable material for a charging pile, comprising the following raw materials in parts by weight:

[0060] 80 parts of TPU 585A resin, 4 parts of microencapsulated ammonium polyphosphate according to Example 3, 22 parts of flame retardant synergistic component according to Example 2, 1 part of molecular chain repair agent, and 1 part of antioxidant.

[0061] The antioxidant is composed of antioxidant 1010 and antioxidant 1035 in a mass ratio of 1:1.

[0062] The molecular chain repair agent is bis(4-phenoxy-2,6-diisopropylphenyl)carbodiimide.

[0063] The method for preparing the above-mentioned cable material for charging pile comprises the following steps:

[0064] (1) Weighing thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic components, molecular chain repair agent and antioxidant according to weight, placing them in a high-speed mixer, and mixing for 4 minutes to obtain a mixture;

[0065] (2) The mixed material is fed into a twin-screw extruder, and after extrusion and granulation, the temperature zones 1 to 10 of the twin-screw extruder are set as follows: 160° C., 170° C., 180° C., 190° C., 195° C., 195° C., 195° C., 195° C., 195° C., 195° C., to obtain a cable material for a charging pile.

[0066] Example 7

[0067] A cable material for a charging pile, comprising the following raw materials in parts by weight:

[0068] 90 parts of TPU 585A resin, 5 parts of microencapsulated ammonium polyphosphate according to Example 4, 27 parts of flame retardant synergistic component according to Example 2, 2 parts of molecular chain repair agent, and 0.5-2 parts of antioxidant.

[0069] The antioxidant is antioxidant 1024, and the molecular chain repair agent is bis(2,6-diisopropylphenyl)carbodiimide.

[0070] The method for preparing the above-mentioned cable material for charging pile comprises the following steps:

[0071] (1) Weighing thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic components, molecular chain repair agent and antioxidant according to weight, placing them in a high-speed mixer, and mixing for 5 minutes to obtain a mixture;

[0072] (2) The mixed material is fed into a twin-screw extruder, and after extrusion and granulation, the temperature zones 1 to 10 of the twin-screw extruder are set as follows: 160° C., 170° C., 180° C., 190° C., 195° C., 195° C., 195° C., 195° C., 195° C., 195° C., to obtain a cable material for a charging pile.

[0073] Comparative Example 4

[0074] A cable material for a charging pile. Compared with Example 5, the flame retardant and synergistic component in Example 5 is replaced by the product prepared in Comparative Example 1, and the remaining raw materials and preparation process are the same as Example 5.

[0075] Comparative Example 5

[0076] A cable material for a charging pile. Compared with Example 5, the microencapsulated ammonium polyphosphate in Example 5 is replaced by the product prepared in Comparative Example 2, and the remaining raw materials and preparation process are the same as Example 5.

[0077] Comparative Example 6

[0078] A cable material for a charging pile. Compared with Example 5, the microencapsulated ammonium polyphosphate in Example 5 is replaced by the substance in Comparative Example 3, and the remaining raw materials and preparation process are the same as in Example 5.

[0079] The performance tests were performed on the cable materials for charging piles obtained in Examples 5 to 7 and Comparative Examples 4 to 6. The water resistance (wet heat aging, temperature 85±2°C, humidity 85±5%, placement time 1000h) and mechanical properties tests were performed according to the requirements for charging pile cables in GB / T 33594-2017. The oxygen index test was performed according to GB / T 2406.2-2009 "Determination of Combustion Behavior of Plastics by Oxygen Index Method". The results are shown in Table 1:

[0080] Table 1

[0081]

[0082]

[0083] It can be seen from the data recorded in Table 1 that, compared with Comparative Examples 4-6, the cable materials obtained in Examples 5-7 have good mechanical properties, flame retardant properties and water resistance. Specifically, compared with Comparative Example 4, Example 5 shows that the introduction of isocyanate groups in the flame retardant synergistic component has a beneficial effect on the mechanical properties, water resistance and flame retardant properties of the cable material. Compared with Comparative Example 5, Example 5 shows that the introduction of amino groups on the surface of microencapsulated ammonium polyphosphate has a beneficial effect on the mechanical properties, water resistance and flame retardant properties of the cable material. Compared with Comparative Example 6, Example 5 shows that microencapsulated ammonium polyphosphate can simultaneously improve the mechanical properties, flame retardant properties and water resistance of the cable material compared with ammonium polyphosphate.

[0084] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0085] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A cable material for a charging pile, characterized in that: It includes the following raw materials in parts by weight: 60-90 parts of thermoplastic polyurethane, 3-5 parts of microencapsulated ammonium polyphosphate, 18-27 parts of flame retardant and synergistic components, 0.5-2 parts of molecular chain repair agent, and 0.5-2 parts of antioxidant; The flame retardant synergistic component is prepared by the following steps: Step S1, adding melamine and n-hexane into a flask, stirring at 20° C. for 20 min, then dropping stearyl chloride, keeping the temperature for reaction for 1 h, allowing to stand for stratification, recovering n-hexane, washing the precipitate with distilled water, filtering it, and drying it to obtain product a; Step S2, add product a and acetone to a flask, stir at 50° C. for 5-10 min, then add acetone solution of p-hydroxybenzaldehyde, after the addition is complete, reflux for 6-8 h, and remove acetone by rotary evaporation to obtain product b; Step S3, under nitrogen protection, adding product b and toluene diisocyanate into a hydrothermal synthesis reactor with a polytetrafluoroethylene liner, stirring for 5-10 minutes, reacting at 150° C. and 180° C. for 1 hour, taking out the reaction product and crushing it, placing the crushed product in a torque rheometer, and reacting at 180-200° C. for 3 hours to obtain a flame retardant synergistic component; Microencapsulated ammonium polyphosphate is prepared by the following steps: Add ammonium polyphosphate to the ethanol aqueous solution, stir evenly, then add ammonia water to adjust the pH value to 10, add 3-aminopropyltriethoxysilane and tetraethyl orthosilicate, stir for 10-20 minutes, transfer to a flask, react at 45°C for 2-3 hours, then filter, wash the filter cake with anhydrous ethanol for 3 times, and finally dry at 80°C for 24 hours. The dosage ratio of ethanol aqueous solution, ammonium polyphosphate, 3-aminopropyltriethoxysilane and tetraethyl orthosilicate is 350-450mL:100g:15-20g:15-20g.

2. A cable material for a charging pile according to claim 1, characterized in that: The molar ratio of melamine to stearyl chloride in step S1 is 1:

1.

3. A cable material for a charging pile according to claim 1, characterized in that: The mass ratio of product a to p-hydroxybenzaldehyde in step S2 is 3.9:2.

4.

4. A cable material for a charging pile according to claim 1, characterized in that: The mass ratio of product b to toluene diisocyanate in step S3 is 6.3:1.7-2.

2.

5. A method for preparing a cable material for a charging pile according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) Weighing thermoplastic polyurethane, microencapsulated ammonium polyphosphate, flame retardant and synergistic component, molecular chain repair agent and antioxidant according to weight, placing in a high-speed mixer, and mixing for 3-5 minutes to obtain a mixture; (2) The mixed material is fed into a twin-screw extruder, and after extrusion and granulation, a cable material for a charging pile is obtained.