A low-permeability coal seam expansion cracking permeability-enhancing material and a preparation method thereof
Hydration is retarded by using high-temperature calcined calcium oxide, standard sand, disintegrants, water storage agents, adsorbents and foaming agents, combined with gel and sodium lauryl sulfate, in the coal seam expansion cracking AR material. The reaction rate is reduced and the hydration temperature is reduced, which solves the problem of heat release from the hydration reaction of coal seam expansion and cracking anti-permeability materials, and improves the gas permeability and safety of coal seams.
Patent Information
- Application Number
- CN202410939157.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-15
AI Technical Summary
The hydration reaction of coal seam expansion cracking anti-permeability materials has a fast heat release rate and high heat release, which leads to an increase in the risk of coal spontaneous combustion and blowholes. Traditional methods cannot effectively reduce this risk, and traditional negative pressure drainage technology cannot solve the problem of low coal seam Penetration problem.
An expansion cracking material composed of high-temperature calcined calcium oxide, standard sand, disintegrant, water storage agent, adsorbent, and foaming agent is used. By adding gel and sodium lauryl sulfate, the hydration reaction rate is delayed. Reduce the hydration peak temperature and increase the density and mechanical properties of the material through standard sand.
It effectively reduces the hydration temperature, increases the expansion pressure, enhances the permeability of the coal seam, reduces the occurrence of underground gas disasters, and ensures the safe production of coal mines.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of coal seam permeability enhancement, in particular to a low-permeability coal seam expansion-fracture-enhancing permeability enhancement material and a preparation method thereof. Background Art
[0002] my country's coal seam structure is complex and the coal permeability is generally low. As shallow coal resources become increasingly depleted, coal development has shifted to deeper areas and become the norm. The low permeability of coal seams has become increasingly obvious, gas extraction has become more difficult, and the pressure on gas disaster prevention and control has increased.
[0003] Traditional negative pressure extraction technology cannot solve the problem of low permeability in coal seams. Pre-extraction takes a long time and has slow effects, which cannot meet the needs of mining succession and underground safety production. Hydraulic fracturing, slitting, punching, loosening blasting and other methods are used to increase the permeability of coal seams, which improves the permeability of coal seams and gas extraction rate, but there are still limitations. Accidents such as induced outbursts and tunnel instability and collapse are prone to occur during use.
[0004] The coal seam expansion fracturing permeability enhancement technology has the advantages of being silent, non-toxic, dust-free, shock-free, and shock-free. However, when drilling coal seams for permeability enhancement, the hydration reaction continuously releases heat, and the temperature of the adjacent coal bodies within a certain range rises, which can easily cause spontaneous combustion and blowout of the coal bodies. In order to reduce the risk of spontaneous combustion and blowout of the coal bodies, a low-permeability coal seam expansion fracturing permeability enhancement material is developed to adapt to the expansion fracturing permeability enhancement of underground coal seam drilling and ensure the safe production of coal mines. Summary of the invention
[0005] The purpose of the invention is to solve the problem of fast heat release rate and high heat release of the hydration reaction of coal seam expansion fracturing and permeability-enhancing materials, and to provide an expansion fracturing material that can delay the reaction rate, reduce the hydration reaction temperature, and have a good fracturing effect, thereby increasing the permeability of low-permeability coal seams and reducing the occurrence of underground gas disasters.
[0006] The first purpose of the present invention is to provide a low permeability coal seam expansion fracturing permeability-enhancing material, which is composed of the following components in parts by mass: 61.13 parts of high-temperature calcined calcium oxide, 28-29 parts of standard sand, 3.71 parts of disintegrant, 2-3 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 0.5-1 parts of foaming agent, and 0.63 parts of magnesium oxide.
[0007] Furthermore, the standard sand is composed of 1mm~2mm coarse sand, 0.5mm~1.0m medium sand, and 0.08mm~0.50mm fine sand in a mass ratio of 1:1:1.
[0008] Furthermore, the disintegrant is silicon dioxide.
[0009] Furthermore, the water storage agent is a gel. Before the experiment, the gel needs to be soaked in water for 3 hours to allow it to fully absorb water and swell.
[0010] Furthermore, the adsorbent is alumina.
[0011] Furthermore, the foaming agent is sodium dodecyl sulfate (SDS).
[0012] The second object of the present invention is to provide a method for preparing the above-mentioned coal seam expansion cracking and permeability-enhancing material, comprising the following steps:
[0013] Step 1: Prepare standard sand
[0014] The sand is screened and divided into 1mm~2mm coarse sand, 0.5~1.0mm medium sand, and 0.08mm~0.50mm fine sand as the raw materials of standard sand.
[0015] Mix the three types of sand screened out evenly to make standard sand.
[0016] Step 2: Add 61.13 parts of high-temperature calcined calcium oxide, 28-29 parts of standard sand, 3.71 parts of disintegrant, 2-3 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 0.5-1 parts of foaming agent, and 0.63 parts of magnesium oxide into the mixer according to the mass proportions, and stir the added dry materials evenly.
[0017] Step 3, select a water-cement ratio of 0.3 for the evenly mixed dry materials, measure an appropriate amount of water and add it to the dry materials, and mix to obtain a prefabricated product.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1) The formula of the present invention contains gel, sodium lauryl sulfate and standard sand. The gel itself can store water, slow down the reaction rate and reduce the hydration peak temperature.
[0020] Sodium dodecyl sulfate contains hydrophilic side chains, which will be adsorbed on the surface of the expansion-cracking material to produce steric hindrance, prevent particle agglomeration, reduce crystallinity, lower hydration peak temperature, and reduce expansion pressure.
[0021] Standard sand, as an inert material, plays the role of aggregate filling in the expansion cracking material. The more the standard sand is added, the fewer voids inside the slurry are and the structure is denser. 2 The increase in crystallinity increases the expansion pressure.
[0022] 2) The coal seam permeability-enhancing expansion material prepared by the present invention has a low hydration temperature and strong expansion performance, can better enhance the permeability of coal seams, and has broad application prospects. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments, but the embodiments are not intended to limit the present invention.
[0024] The standard sand used in the following embodiments is composed of 1 mm~2 mm coarse sand, 0.5 mm~1.0 m medium sand, and 0.08 mm~0.50 mm fine sand in a mass ratio of 1:1:1; the experimental methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are all commercially available unless otherwise specified.
[0025] Example 1
[0026] A low permeability coal seam expansion fracturing permeability-enhancing material is prepared by, in parts by mass, 61.13 parts of high-temperature calcined calcium oxide, 28.12 parts of standard sand, 3.71 parts of a disintegrant, 2.5 parts of a water storage agent, 1.78 parts of iron oxide, 0.75 parts of an adsorbent, 0.73 parts of a foaming agent, and 0.63 parts of magnesium oxide, and by adding an appropriate amount of water at a water-cement ratio of 0.3.
[0027] The specific preparation method is as follows:
[0028] Step 1: Prepare standard sand
[0029] The sand is screened and divided into 1mm~2mm coarse sand, 0.5~1.0mm medium sand, and 0.08mm~0.50mm fine sand as the raw materials of standard sand.
[0030] Mix the three types of sand screened out evenly to make standard sand.
[0031] Step 2, add 61.13 parts of high-temperature calcined calcium oxide, 28.12 parts of standard sand, 3.71 parts of disintegrant, 2.5 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 0.73 parts of foaming agent, and 0.63 parts of magnesium oxide into the mixer, and stir the added dry materials evenly.
[0032] Step 3, select a water-cement ratio of 0.3 for the evenly mixed dry materials, measure an appropriate amount of water, add it to the dry materials, and mix to obtain a prefabricated product.
[0033] Example 2
[0034] A low permeability coal seam expansion fracturing permeability-enhancing material is prepared by, in parts by mass, 61.13 parts of high-temperature calcined calcium oxide, 29 parts of standard sand, 3.71 parts of a disintegrant, 3 parts of a water storage agent, 1.78 parts of iron oxide, 0.75 parts of an adsorbent, 1 part of a foaming agent, and 0.63 parts of magnesium oxide, and by adding an appropriate amount of water at a water-cement ratio of 0.3.
[0035] The specific preparation method is as follows:
[0036] Step 1: Prepare standard sand
[0037] The sand is screened and divided into 1mm~2mm coarse sand, 0.5~1.0mm medium sand, and 0.08mm~0.50mm fine sand as the raw materials of standard sand.
[0038] Mix the three types of sand screened out evenly to make standard sand.
[0039] Step 2, add 61.13 parts of high-temperature calcined calcium oxide, 29 parts of standard sand, 3.71 parts of disintegrant, 3 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 1 part of foaming agent, and 0.63 parts of magnesium oxide into the mixer, and stir the added dry materials evenly.
[0040] Step 3, select a water-cement ratio of 0.3 for the evenly mixed dry materials, measure an appropriate amount of water, add it to the dry materials, and mix to obtain a prefabricated product.
[0041] Example 3
[0042] A low permeability coal seam expansion fracturing permeability-enhancing material is prepared by, in parts by mass, 61.13 parts of high-temperature calcined calcium oxide, 28 parts of standard sand, 3.71 parts of a disintegrant, 2 parts of a water storage agent, 1.78 parts of iron oxide, 0.75 parts of an adsorbent, 0.5 parts of a foaming agent, and 0.63 parts of magnesium oxide, and by adding an appropriate amount of water at a water-cement ratio of 0.3.
[0043] The specific preparation method is as follows:
[0044] Step 1: Prepare standard sand
[0045] The sand is screened and divided into 1mm~2mm coarse sand, 0.5~1.0mm medium sand, and 0.08mm~0.50mm fine sand as the raw materials of standard sand.
[0046] Mix the three types of sand screened out evenly to make standard sand.
[0047] Step 2, add 61.13 parts of high-temperature calcined calcium oxide, 29 parts of standard sand, 3.71 parts of disintegrant, 3 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 1 part of foaming agent, and 0.63 parts of magnesium oxide into the mixer, and stir the added dry materials evenly.
[0048] Step 3, select a water-cement ratio of 0.3 for the evenly mixed dry materials, measure an appropriate amount of water, add it to the dry materials, and mix to obtain a prefabricated product.
[0049] In order to further illustrate the effect of the present invention, the present invention also provides a comparative example, which is as follows.
[0050] Comparative Example 1
[0051] The comparative example is composed of 61.13 parts of high-temperature calcined calcium oxide, 3.71 parts of disintegrant, 1.78 parts of iron oxide, 0.75 parts of adsorbent, and 0.63 parts of magnesium oxide.
[0052] The present invention uses a thermocouple temperature sensor and "JC506-2008-Silent Cracking Agent" to perform temperature tests and expansion pressure tests on Examples 1, 2, 3 and Comparative Example 1, respectively. The test results are shown in Table 1:
[0053] Table 1 Test results
[0054]
[0055] 1) The peak hydration temperature of Example 1 decreased by 36.2% compared with that of Comparative Example 1; the peak hydration temperature of Example 2 decreased by 33% compared with that of Comparative Example 1; and the peak hydration temperature of Example 3 decreased by 24.8% compared with that of Comparative Example 1.
[0056] 2) The mechanical properties of Example 1 are also improved compared to those of Comparative Example 1, and the maximum expansion pressure is increased by 66.8%; the maximum expansion pressure of Example 2 is increased by 48.72% compared to that of Comparative Example 1; and the maximum expansion pressure of Example 3 is increased by 23.6% compared to that of Comparative Example 1.
[0057] After the water storage agent gel is added in the embodiment, the gel molecules are adsorbed on the surface of the swelling and fracturing material particles, reducing the contact between the swelling and fracturing material particles and water, achieving the purpose of partially isolating the swelling and fracturing material particles from water, slowing down the rate of hydration of the swelling and fracturing material particles in the temperature development stage, and prolonging the reaction time. The addition of gel increases the viscosity of water, increases the adhesion of the swelling and fracturing material slurry during the hydration process, reduces the free water in the slurry, reduces the evaporated water in the rapid temperature rise stage, slows down the reaction rate, and retains more water for subsequent hydration to continue. Therefore, the hydration temperature of the embodiment is lower than that of the comparative example.
[0058] The foaming agent SDS molecules contain a large number of hydrophilic groups - hydroxyl groups. Due to adsorption, hydroxyl groups appear on the surface of the expansion-cracking material particles. SDS can associate with water molecules through hydrogen bonds to form a large amount of solvated water film on the surface of the expansion-cracking material particles, releasing the water wrapped in the particles, increasing the fluidity of the slurry, delaying the reaction time, and reducing the hydration temperature.
[0059] The standard sand itself does not generate heat, and as the internal temperature of the expansion-induced cracking material increases during the hydration reaction, the standard sand absorbs part of the heat, thereby lowering the hydration temperature; and the slurry with a high standard sand content has fewer voids, which can make the interior of the material enter a dense state earlier and play a role in aggregate support. Therefore, the mechanical properties of the embodiment with the addition of standard sand are better than those of the comparative example.
[0060] The above description is only a preferred embodiment of the present invention and is not a limitation. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A low permeability coal seam expansion fracturing and permeability-enhancing material, characterized in that: The composition is composed of the following components by weight: 61.13 parts of high-temperature calcined calcium oxide, 28-29 parts of standard sand, 3.71 parts of disintegrant, 2-3 parts of water storage agent, 1.78 parts of iron oxide, 0.75 parts of adsorbent, 0.5-1 parts of foaming agent, and 0.63 parts of magnesium oxide; The disintegrant is silicon dioxide; The water storage agent is a gel; The adsorbent is alumina; The foaming agent is sodium dodecyl sulfate (SDS).
2. A low permeability coal seam expansion fracturing anti-permeability material according to claim 1, characterized in that: The low permeability coal seam expansion fracturing and permeability-enhancing material is made into slurry with a water-cement ratio of 0.
3.
3. The method for preparing a low permeability coal seam expansion fracturing anti-permeability material according to claim 1 or 2, characterized in that: Follow these steps to complete: (1) Place each component in a mixer according to the required mass fraction and mix the dry materials evenly; (2) adding water to the dry material and stirring the dry material sufficiently to obtain a slurry of low permeability coal seam expansion fracturing and permeability-enhancing material; (3) The material slurry is transported into the coal seam through a borehole for fracturing and permeability enhancement.
Citation Information
Patent Citations
Gas-bearing coal mass hydrofracture and acidification combined strengthening anti-reflection assessment method
CN106368733A
Physical anti-reflection and chemical displacement combined control method for coal bed gas and anti-reflection system
CN117722167A