A multi-layer ultrafine polypropylene modified filter bag and its manufacturing method

Through the design of multi-layer ultrafine polypropylene modified filter bags, the composite substrate layer and modified filter material layer are used to solve the wear resistance and filtration effect of existing filter bags in high temperature and corrosion environments, and the problem of wear resistance and filtration effect of existing filter bags in high temperature and corrosion environments is extended. Service life and improve filtration efficiency and antibacterial ability.

CN118461232BActive Publication Date: 2024-11-08JIANGSU SHEKE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410897538.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-08
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

When used in high temperature and aggressive gas environments, the wear resistance, heat resistance and filtration effects are poor, resulting in faster wear and reduced filtration effects.

Method used

Using multi-layer ultrafine polypropylene modified filter bags, the filter efficiency and tensile strength of the filter bag are improved by combining composite base fabric layer and modified filter material layer. , and impart antibacterial and antibacterial ability.

Benefits of technology

It significantly extends the service life of the filter bag, improves filtration efficiency and mechanical properties, and enhances antibacterial ability, and is suitable for high-temperature and corrosive environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118461232B_ABST
    Figure CN118461232B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of filter materials, and provides a multi-layer ultrafine polypropylene modified filter bag and a manufacturing method thereof, comprising a composite base fabric layer and a modified filter material layer stacked in sequence; the composite base fabric layer is woven from modified composite polypropylene fibers, the modified composite polypropylene fibers include composite polypropylene fibers, a polydopamine layer coated on the surface of the composite polypropylene fibers, and a MOFs material loaded on the surface of the polydopamine layer, and the composite polypropylene fibers are prepared by melt extrusion, cooling granulation, and melt spinning of polypropylene resin and chitosan in sequence; the modified filter material layer is formed by melt-blowing a resin mixture onto the surface of the composite base fabric layer through a melt-blowing device after the resin mixture is melted, and the resin mixture includes polylactic acid resin, polyethylene glycol, silicon dioxide / nanosilver aerogel, and modified activated carbon. The manufacturing method provided by the present invention can effectively improve the filtration efficiency and tensile strength of the filter bag, extend the service life of the filter bag, and also give the filter bag a certain antibacterial and antibacterial ability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of filter materials and relates to a multi-layer ultrafine polypropylene modified filter bag and a manufacturing method thereof. Background Art

[0002] In the production process of thermal power generation, steel and cement industries, a large amount of dust is generated, causing serious air pollution and environmental pollution. Bag dust removal is a widely used dust removal method. The filter bag is a key part of the operation of the bag dust collector and plays a key role in the dust removal effect of the bag dust collector.

[0003] When bag filters are used to filter high-temperature and highly corrosive dust-containing gases, the filter bags need to have excellent wear resistance, chemical stability and heat resistance. However, most existing filter bags are single-layer structures, and the friction between the filter bags causes serious wear. In addition, the high-temperature resistance of existing filter bags is poor. When used for a long time in a high-temperature environment, the aging of the filter bags will be accelerated, and the filtering effect of the filter bags will also be affected. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a multi-layer ultrafine polypropylene modified filter bag and a method for manufacturing the same. By compounding the composite base cloth layer and the modified filter material layer, the filtration efficiency and tensile strength of the filter bag can be effectively improved, the service life of the filter bag can be greatly extended, and the filter bag can also be endowed with certain antibacterial and antimicrobial capabilities.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides a multi-layer ultrafine polypropylene modified filter bag, wherein the multi-layer ultrafine polypropylene modified filter bag comprises a composite base fabric layer and a modified filter material layer stacked in sequence;

[0007] The composite base fabric layer is woven from modified composite polypropylene fibers, the modified composite polypropylene fibers include composite polypropylene fibers, a polydopamine layer coated on the surface of the composite polypropylene fibers, and a MOFs material loaded on the surface of the polydopamine layer, and the composite polypropylene fibers are prepared by sequentially melt extrusion, cooling granulation, and melt spinning of polypropylene resin and chitosan;

[0008] The modified filter material layer is formed by melt-blowing a resin mixture onto the surface of the composite base fabric layer through a melt-blowing device. The resin mixture includes polylactic acid resin, polyethylene glycol, silicon dioxide / nanosilver aerogel and modified activated carbon. The modified activated carbon is obtained by sequentially subjecting activated carbon to chemical oxidation modification, high-temperature oxidation modification and silane coupling agent surface modification.

[0009] The multi-layer ultrafine polypropylene modified filter bag provided by the present invention can effectively improve the filtration efficiency and tensile strength of the filter bag through the composite base cloth layer and the modified filter material layer, greatly prolong the service life of the filter bag, and also give the filter bag a certain antibacterial and antimicrobial ability.

[0010] As a preferred technical solution of the present invention, the warp density of the composite base fabric layer is 300-350 strands / 10cm, for example, it can be 300 strands / 10cm, 305 strands / 10cm, 310 strands / 10cm, 315 strands / 10cm, 320 strands / 10cm, 325 strands / 10cm, 330 strands / 10cm, 335 strands / 10cm, 340 strands / 10cm, 345 strands / 10cm or 350 strands / 10cm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0011] In some optional examples, the weft density of the composite base fabric layer is 250~300 strands / 10cm, for example, it can be 250 strands / 10cm, 255 strands / 10cm, 260 strands / 10cm, 265 strands / 10cm, 270 strands / 10cm, 275 strands / 10cm, 280 strands / 10cm, 285 strands / 10cm, 290 strands / 10cm, 295 strands / 10cm or 300 strands / 10cm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0012] In some optional examples, the thickness of the composite base fabric layer is 1~3 mm, for example, it can be 1.0 mm, 1.2 mm, 1.4 mm, 1.6 mm, 1.8 mm, 2.0 mm, 2.2 mm, 2.4 mm, 2.6 mm, 2.8 mm or 3.0 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] In some optional instances, the average pore size of the composite base fabric layer is 60-70 μm, for example, it may be 60 μm, 61 μm, 62 μm, 63 μm, 64 μm, 65 μm, 66 μm, 67 μm, 68 μm, 69 μm or 70 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0014] In some optional examples, the thickness of the modified filter material layer is 2~4mm, for example, it can be 2.0mm, 2.2mm, 2.4mm, 2.6mm, 2.8mm, 3.0mm, 3.2mm, 3.4mm, 3.6mm, 3.8mm or 4.0mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0015] In some optional examples, the average pore size of the modified filter material layer is 15~25μm, for example, it can be 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm or 25μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] In a second aspect, the present invention provides a method for manufacturing the multi-layer ultrafine polypropylene modified filter bag according to the first aspect, the manufacturing method comprising:

[0017] (I) adding a titanate coupling agent to an ethanol aqueous solution, mixing, stirring and heating to obtain a coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, mixing and stirring to obtain a composite modified solution; dry ball milling chitosan to obtain chitosan particles, dispersing the chitosan particles in the composite modified solution, mixing and stirring evenly, then filtering, washing and drying to obtain modified chitosan particles; mixing the modified chitosan particles and polypropylene resin, and then putting them into a first screw extruder for melt extrusion, cooling and granulating to obtain a composite polypropylene masterbatch, and melt spinning the composite polypropylene masterbatch to obtain a composite polypropylene fiber;

[0018] (II) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, immersing the composite polypropylene fiber obtained in step (I) in the dopamine solution to form a polydopamine layer on the surface of the composite polypropylene fiber, taking it out, washing, and drying it to obtain a coated polypropylene fiber; preparing a zinc nitrate solution and a 2-methylimidazole solution respectively, immersing the coated polypropylene fiber in the zinc nitrate solution, and then dripping the 2-methylimidazole solution, stirring continuously during the dripping process to in-situ generate MOFs material on the surface of the polydopamine layer, taking it out, washing, and drying it to obtain a modified composite polypropylene fiber, and weaving the modified composite polypropylene fiber to form a composite base fabric layer;

[0019] (III) mixing tetraethyl orthosilicate with an ethanol aqueous solution to obtain a tetraethyl orthosilicate solution, adding a nitric acid solution to the tetraethyl orthosilicate solution to adjust its pH value to obtain a precursor solution; heating the precursor solution in a water bath to obtain a silica sol; dropping the silica sol into a silver nitrate solution, stirring the reaction under light-proof conditions to obtain a silica / nanosilver sol, adding a mixed solution consisting of ammonia water, ethanol and deionized water to the silica / nanosilver sol, mixing, stirring and heating to gel the silica / nanosilver sol to form a silica / nanosilver gel; standing, aging and washing the silica / nanosilver gel in sequence, immersing the washed silica / nanosilver gel in a polydimethylsiloxane solution for hydrophobic modification, and finally washing, drying and grinding to obtain a silica / nanosilver aerogel powder;

[0020] (IV) impregnating activated carbon in an acid solution, filtering, washing and drying after the impregnation to obtain chemically oxidized activated carbon; placing the chemically oxidized activated carbon in a tubular furnace, introducing a mixed gas composed of oxygen and nitrogen into the tubular furnace, and subjecting the chemically oxidized activated carbon to high-temperature oxidation treatment to obtain composite oxidized activated carbon; dispersing the composite oxidized activated carbon in cyclohexane to form an activated carbon suspension, adding a silane coupling agent solution to the activated carbon suspension under stirring conditions, mixing, stirring and heating to react to obtain a reaction product, and filtering, washing and drying the reaction product to obtain modified activated carbon;

[0021] (V) mixing the silica / nanosilver aerogel obtained in step (III), the modified activated carbon obtained in step (IV) and deionized water, and then dispersing them by ultrasonic dispersion to obtain a composite filler solution; putting polylactic acid resin, polyethylene glycol and the composite filler solution into a melt-blowing device, and melt-blowing the surface of the composite base fabric layer obtained in step (II) by the melt-blowing device to form a modified filter material layer; then, subjecting the composite layer composed of the modified filter material layer and the composite base fabric layer to a corona electret treatment to obtain the multi-layer ultrafine polypropylene modified filter bag.

[0022] The invention ball-mills chitosan to obtain chitosan microparticles, then composite-modifies the chitosan microparticles with a titanate coupling agent and sodium dodecylbenzene sulfonate to obtain modified chitosan microparticles, and then mixes the modified chitosan microparticles with a polypropylene resin and performs melt extrusion, cooling granulation and melt spinning to obtain composite polypropylene fibers. The modification method provided by the invention can significantly improve the mechanical properties of the composite polypropylene fibers. This is because, the present invention adopts sodium dodecylbenzene sulfonate as anionic surfactant, adsorbs it on the surface of chitosan particles through solution treatment to obtain modified chitosan particles, and the sodium dodecylbenzene sulfonate forms a coating layer on the surface of the chitosan particles, which can effectively improve the dispersibility and stability of the chitosan particles in the polypropylene resin melt, reduce the agglomeration of the chitosan particles, thereby improving the interface compatibility between the modified chitosan particles and the polypropylene resin matrix, which is beneficial to the improvement of the mechanical properties of the composite polypropylene fiber; in addition, sodium dodecylbenzene sulfonate can reduce the surface energy of the polypropylene crystal, and the modified chitosan particles coated with sodium dodecylbenzene sulfonate can be used as a nucleating agent for the polypropylene resin after blending and melting with the polypropylene resin, thereby increasing the possibility of nucleation, reducing the growth rate of the polypropylene crystal, and the crystal nucleus has sufficient time and space to grow, so the crystal size of the composite polypropylene fiber finally obtained is significantly increased, and the mechanical properties are significantly improved.

[0023] The present invention adds modified chitosan particles into the polypropylene resin melt, which can not only improve the mechanical properties of the composite polypropylene fiber, but also give the composite base fabric layer a certain antibacterial ability. On the one hand, the addition of modified chitosan particles increases the tensile stress of the blended melt composed of modified chitosan particles and polypropylene resin, and as the tensile strain rate increases, the degree of increase in the tensile stress of the blended melt is more obvious. The tensile strain rate orients the polypropylene macromolecular chains along the direction of the force, increases the probability of the polypropylene molecular chains being arranged in parallel along the direction of the force, and thus enhances the resistance of the blended melt to further stretching. During the melt spinning process, the internal defects of the spinning fine flow of the blended melt can be compensated and homogenized during the molding and stretching process, and the resulting composite polypropylene fiber has fewer internal defects and greatly improved mechanical properties. On the other hand, the modified chitosan particles are a natural antibacterial material, and the -NH3 on the chitosan molecules + The functional groups and the negative charges on the cell surface attract each other, hindering the exchange of substances inside and outside the cell, and at the same time affecting the charge distribution on the cell wall or cell membrane, causing an imbalance in the synthesis and dissolution of the bacterial cell wall or cell membrane, thereby playing an antibacterial and bactericidal role; in addition, chitosan can penetrate into the bacterial cell membrane in the form of molecules, -NH3 + The functional groups adsorb anionic substances in the cells, disrupting the normal physiological activities in the cells and killing bacteria.

[0024] The present invention uses polydopamine to modify the surface of the composite polypropylene fiber, and uses the oxidative self-polymerization reaction of dopamine monomer at room temperature to form a polydopamine layer on the surface of the composite polypropylene fiber to obtain a coated polypropylene fiber coated with the polydopamine layer; due to the presence of catechol functional groups in the polydopamine molecular chain, the polydopamine has super strong adhesion performance and can be easily deposited and firmly attached to the surface of the coated polypropylene fiber; then, the coated polypropylene fiber is immersed in a zinc nitrate solution and a 2-methylimidazole solution is added dropwise to coat the surface of the polypropylene fiber. The polydopamine can react with zinc ions, and the catechol functional groups in the polydopamine molecular chain can form stable chemical bonds with zinc ions, providing stable nucleation points for the growth of MOFs materials. The MOFs material is in situ generated and firmly loaded on the surface of the coated polypropylene fiber through the solvent thermal synthesis reaction of zinc nitrate solution and 2-methylimidazole solution, and finally a modified composite polypropylene fiber loaded with MOFs material is prepared. The present invention significantly improves the loading fastness of the MOFs material on the surface of the coated polypropylene fiber through polydopamine coating.

[0025] In addition, the present invention can also significantly improve the mechanical properties of the modified composite polypropylene fiber through polydopamine coating. This is because dopamine gradually self-polymerizes to form polydopamine in an alkaline environment. Polydopamine can produce strong hydrogen bonding with the composite polypropylene fiber, so that it has strong surface adhesion and can stably adhere to the surface of the composite polypropylene fiber. On the one hand, the polydopamine particles formed by deposition on the surface of the modified composite polypropylene fiber improve the surface roughness of the fiber, and can enhance the surface friction of the fiber when the modified composite polypropylene fiber is stretched by an external force, thereby improving the tensile strength of the modified composite polypropylene fiber; on the other hand, when the modified composite polypropylene fiber is woven to form a composite base fabric layer, polydopamine adheres between the fibers to form cross-linking points between the fibers, thereby enhancing the force between the fibers; at the same time, the MOFs material and the polydopamine particles between the fibers play a bridging role, thereby coating the cross-stacked parts between the modified composite polypropylene fibers to form connection points, forming a mesh structure, so that the overall structure of the composite base fabric layer woven from the modified composite polypropylene fibers is more stable, and its mechanical properties are further improved.

[0026] The purpose of loading MOFs material on the surface of modified composite polypropylene fiber in the present invention is: (1) after loading MOFs material, the surface of modified composite polypropylene fiber becomes rough, so that the pore size of the woven composite base fabric layer is reduced. When flue gas containing fine particles such as dust flows into the filter bag, the fine particles in the airflow will not have time to bypass the modified composite polypropylene fiber due to inertia. The fine particles in the flue gas will collide with the MOFs material and deposit on the surface of the filter bag. By loading MOFs material, the fine particles carried in the flue gas cannot smoothly pass through the gaps between the fibers, thereby increasing the probability of the fine particles being deposited. (2) The defects of MOFs material will cause the surface of the fine particles to be polarized. The polarized fine particles are easy to interact with the MOFs material. In this process, the unbalanced metal ions in the MOFs material will provide positive charges. Thereby, the ability of the composite base fabric layer to capture fine particles is enhanced; at the same time, during the solvent thermal synthesis process, due to the incomplete growth of the crystal part of the nano-scale MOFs material, the crystal defects of the MOFs material increase, which is conducive to capturing more fine particles; (3) The surface of the MOFs material contains a large number of active functional groups such as hydroxyl groups, which can react with fine particles carrying polar functional groups in the flue gas, thereby capturing them; (4) Since the MOFs material has a large specific surface area, after loading the MOFs material, the total specific surface area of ​​the composite base fabric layer increases, which is conducive to improving the surface energy of the composite base fabric layer, and the fine particles in the flue gas are more easily deposited on the surface of the composite base fabric layer; (5) The MOFs material has a large cavity, abundant gas adsorption sites, organic adsorption sites and open metal sites, which endows the composite base fabric layer with excellent fine particle adsorption capacity.

[0027] The present invention adopts silica / nanosilver aerogel and modified activated carbon to melt-blend and modify the polylactic acid resin, which can not only improve the problems of slow crystallization rate and poor mechanical properties of polylactic acid, but also increase the specific surface area of ​​the polylactic acid matrix, thereby improving the filtration performance of the multi-layer ultrafine polypropylene modified filter bag and giving it excellent antibacterial and mechanical properties.

[0028] Silica aerogel has a high porosity and a large specific surface area. Adding it to a polylactic acid resin mixture can improve the adsorption performance of the modified filter material layer on fine particles. Furthermore, the present invention performs in-situ doping modification of the silica aerogel with silver nanoparticles, which can make it have both adsorption performance and antibacterial function. In order to make the silica / nanosilver aerogel evenly dispersed in the resin matrix, the present invention uses tetraethyl orthosilicate as the silicon source and adopts the sol-gel method to prepare silica sol; then, using silver nitrate as the silver nanoparticle precursor, the silica sol is dripped into the silver nitrate solution, and the silica / nanosilver gel is prepared by in-situ doping; finally, polydimethylsiloxane is used as a hydrophobic modifier to hydrophobically modify the silica / nanosilver gel.

[0029] The present invention utilizes an acid solution to perform chemical oxidation treatment on activated carbon, and the acid modification can increase the number of acidic functional groups on the surface of the activated carbon; at the same time, the strong oxidizing property of the acid solution can open the closed micropores inside the activated carbon, increase the number of micropores inside the activated carbon, increase the specific surface area and total pore volume of the activated carbon, and thus improve the adsorption capacity for fine particles; in addition, the surface hydrophilicity of the activated carbon and the affinity for polar organic matter can be enhanced after the acid modification treatment, thereby improving the dispersion uniformity of the modified activated carbon in the polylactic acid resin melt.

[0030] The present invention further performs high-temperature oxidation treatment on the activated carbon on the basis of chemical oxidation modification treatment, and the chemical oxidation modification by acid solution is conducive to the continued increase of the pore volume of the activated carbon micropores and the secondary formation of the activated carbon micropores during the high-temperature oxidation treatment. After the composite oxidation treatment, more oxygen-containing acidic functional groups will be produced on the surface of the activated carbon. During the high-temperature oxidation process, the presence of these oxygen-containing acidic functional groups will redivide the adsorption space inside the activated carbon, so that the larger adsorption space inside the activated carbon that is not conducive to capturing volatile organic compounds is divided into smaller adsorption spaces, forming more micropores below 0.7nm, while expanding the pore volume of the activated carbon micropores, shortening the distance between the pollutant molecules and the oxygen-containing acidic functional groups, and enhancing the molecular interaction between each other, thereby increasing the saturated adsorption capacity of the modified activated carbon.

[0031] As a preferred technical solution of the present invention, in step (I), the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9):1, for example, it can be 8.0:1, 8.1:1, 8.2:1, 8.3:1, 8.4:1, 8.5:1, 8.6:1, 8.7:1, 8.8:1, 8.9:1 or 9.0:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] In some optional examples, the stirring time of the titanate coupling agent and the ethanol aqueous solution is 0.5 to 1.5 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h or 1.5 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] In some optional examples, the heating temperature of the titanate coupling agent and the ethanol aqueous solution is 50-60°C, for example, it can be 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] In some optional examples, the concentration of the titanate coupling agent in the coupling agent solution is 1-5 g / L, for example, 1.0 g / L, 1.5 g / L, 2.0 g / L, 2.5 g / L, 3.0 g / L, 3.5 g / L, 4.0 g / L, 4.5 g / L or 5.0 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] In some optional examples, the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate in the coupling agent solution is (1.5-2.5):1, for example, it can be 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2.0:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1 or 2.5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] In some optional examples, the stirring time of the coupling agent solution and the sodium dodecylbenzene sulfonate is 10 to 30 min, for example, 10 min, 12 min, 14 min, 16 min, 18 min, 20 min, 22 min, 24 min, 26 min, 28 min or 30 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] In some optional examples, the ball milling time of the chitosan is 3 to 5 hours, for example, it can be 3.0h, 3.2h, 3.4h, 3.6h, 3.8h, 4.0h, 4.2h, 4.4h, 4.6h, 4.8h or 5.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Chitosan is subjected to mechanical action such as shearing and rolling during ball milling. Sufficient mechanical energy will destroy the van der Waals force between chitosan molecules and a small number of macromolecular chains, causing the size of chitosan to decrease rapidly. As the ball milling time increases, the particle size of chitosan particles decreases, the particle size distribution becomes narrower, the layered structure decreases, and a morphology similar to "erosion" is formed. After ball milling, the molecular weight of chitosan decreases, the crystalline structure of chitosan is destroyed, and it tends to be amorphous, but its deacetylation degree and molecular structure do not change significantly. The hygroscopicity and water solubility of the obtained chitosan particles are significantly enhanced. When the ball milling time reaches 5h, the particle size of chitosan particles reaches the ball milling limit. If the ball milling time is further extended, the particle size of chitosan particles cannot be significantly reduced.

[0039] In some optional examples, the ball milling speed of the chitosan is 300-400 rpm, for example, it can be 300 rpm, 310 rpm, 320 rpm, 330 rpm, 340 rpm, 350 rpm, 360 rpm, 370 rpm, 380 rpm, 390 rpm or 400 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] In some optional examples, the particle size of the chitosan particles is 20-30 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm or 30 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] In some optional examples, the mass ratio of the chitosan particles to the titanate coupling agent in the composite modified solution is 1:(0.1-0.2), for example, it can be 1:0.1, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15, 1:0.16, 1:0.17, 1:0.18, 1:0.19 or 1:0.2, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] In some optional examples, the stirring time of the chitosan particles and the composite modified solution is 1 to 3 hours, for example, it can be 1.0h, 1.2h, 1.4h, 1.6h, 1.8h, 2.0h, 2.2h, 2.4h, 2.6h, 2.8h or 3.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] In some optional examples, the mass ratio of the modified chitosan particles to the polypropylene resin is (0.02-0.03):1, for example, it can be 0.02:1, 0.021:1, 0.022:1, 0.023:1, 0.024:1, 0.025:1, 0.026:1, 0.027:1, 0.028:1, 0.029:1 or 0.03:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In some optional instances, the extrusion temperature of the first screw extruder is 190-200°C, for example, it can be 190°C, 191°C, 192°C, 193°C, 194°C, 195°C, 196°C, 197°C, 198°C, 199°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] In some optional examples, the screw speed of the first screw extruder is 100~200r / min, for example, it can be 100r / min, 110r / min, 120r / min, 130r / min, 140r / min, 150r / min, 160r / min, 170r / min, 180r / min, 190r / min or 200r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] As a preferred technical solution of the present invention, in step (II), the mass fraction of dopamine hydrochloride in the dopamine solution is 5-10 g / L, for example, it can be 5.0 g / L, 5.5 g / L, 6.0 g / L, 6.5 g / L, 7.0 g / L, 7.5 g / L, 8.0 g / L, 8.5 g / L, 9.0 g / L, 9.5 g / L or 10.0 g / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] In some optional examples, the immersion time of the composite polypropylene fiber in the dopamine solution is 10 to 15 hours, for example, it can be 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours, 14 hours, 14.5 hours or 15 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0048] In some optional examples, the zinc nitrate solution consists of zinc nitrate hexahydrate and methanol.

[0049] In some optional examples, the concentration of zinc nitrate hexahydrate in the zinc nitrate solution is 0.1-0.2 g / mL, for example, 0.1 g / mL, 0.11 g / mL, 0.12 g / mL, 0.13 g / mL, 0.14 g / mL, 0.15 g / mL, 0.16 g / mL, 0.17 g / mL, 0.18 g / mL, 0.19 g / mL or 0.2 g / mL, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] In some optional examples, the 2-methylimidazole solution consists of 2-methylimidazole and methanol.

[0051] In some optional examples, the concentration of 2-methylimidazole in the 2-methylimidazole solution is 0.15~0.25g / mL, for example, it can be 0.15g / mL, 0.16g / mL, 0.17g / mL, 0.18g / mL, 0.19g / mL, 0.2g / mL, 0.21g / mL, 0.22g / mL, 0.23g / mL, 0.24g / mL or 0.25g / mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0052] In some optional examples, the mass ratio of the coated polypropylene fiber to the zinc nitrate hexahydrate in the zinc nitrate solution is 1:(20~30), for example, it can be 1:20, 1:21, 1:22, 1:23, 1:24, 1:25, 1:26, 1:27, 1:28, 1:29 or 1:30, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] After the MOFs material was loaded on the surface of the coated polypropylene fiber, a rough structure was formed on the fiber surface, which increased the contact area between the composite polypropylene fiber and fine particles, increased the effective filtration area on the surface of the composite base fabric layer, enhanced the capture ability of fine particles, and greatly improved the filtration efficiency. In addition, after loading the MOFs material, the modified composite polypropylene fiber has a stronger electrostatic force, which is conducive to further improving the filtration performance of the composite base fabric layer. Since the surface of fine particles in the flue gas contains a large number of highly polar functional groups, such as CO, C=O, CN, etc., the unbalanced metal ions and defects of the MOFs material provide positive charges, which polarize the surface of the fine particles, enhance the electrostatic interaction between the fine particles and the modified composite polypropylene fiber, and improve the capture ability of the composite base fabric layer for fine particles.

[0054] The present invention specifically limits the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate to 1: (20-30). When the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is within the numerical range defined by the present invention, it is possible to ensure that the surface of the coated polypropylene fiber is loaded with an appropriate amount of MOFs material, and the mechanical properties of the composite base fabric layer will not be affected while the filtration performance of the composite base fabric layer is improved. When the amount of zinc nitrate hexahydrate added exceeds the upper limit of the range defined by the present invention, the loading amount of the MOFS material on the surface of the coated polypropylene fiber will be too high, and the particle size will be too large, so that the MOFS material will agglomerate and accumulate on the surface of the coated polypropylene fiber to form cracked blocks. When the composite base fabric layer is subjected to external tensile force, the agglomerated MOFS blocks are easily detached from the surface of the coated polypropylene fiber, thereby affecting the mechanical properties and filtration performance of the composite base fabric layer.

[0055] In some optional examples, the immersion time of the coated polypropylene fiber in the zinc nitrate solution is 50 to 60 minutes, for example, it can be 50 minutes, 51 minutes, 52 minutes, 53 minutes, 54 minutes, 55 minutes, 56 minutes, 57 minutes, 58 minutes, 59 minutes or 60 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0056] The immersion time of the coated polypropylene fiber in the zinc nitrate solution will also directly affect the loading amount of the MOFs material on the surface of the coated polypropylene fiber. For this reason, the present invention specifically limits the immersion time of the coated polypropylene fiber in the zinc nitrate solution to 50-60 minutes. When the immersion time of the coated polypropylene fiber in the zinc nitrate solution exceeds 60 minutes, the loading amount of the MOFS material on the surface of the coated polypropylene fiber will be too high, the particle size will be too large, and some MOFs materials will agglomerate and accumulate in some areas of the surface of the coated polypropylene fiber to form large pieces of hardened particles. On the one hand, the large pieces of particles accumulated on the surface of the coated polypropylene fiber will cause the surface of the composite base fabric layer to be blocked, resulting in a decrease in the air permeability of the composite base fabric layer, an increase in the filtration resistance, and a negative impact on the filtration efficiency of the composite base fabric layer; on the other hand, the large pieces of hardened particles will make the coated polypropylene fiber brittle. At the same time, the uneven distribution of the large pieces of particles will also weaken the mechanical structure of the coated polypropylene fiber, thereby causing a significant decrease in the tensile strength of the composite base fabric layer obtained after weaving.

[0057] In some optional examples, the molar ratio of zinc nitrate hexahydrate in the zinc nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 1:(3~4), for example, it can be 1:3.0, 1:3.1, 1:3.2, 1:3.3, 1:3.4, 1:3.5, 1:3.6, 1:3.7, 1:3.8, 1:3.9 or 1:4.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] In some optional examples, the dropping speed of the 2-methylimidazole solution is 1~5mL / min, for example, it can be 1.0mL / min, 1.5mL / min, 2.0mL / min, 2.5mL / min, 3.0mL / min, 3.5mL / min, 4.0mL / min, 4.5mL / min or 5.0mL / min, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] In some optional examples, after all the 2-methylimidazole solution is added dropwise, stirring is continued for 1 to 2 hours, for example, 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] As a preferred technical solution of the present invention, in step (III), the volume ratio of ethanol to water in the ethanol aqueous solution is 1:(1-2), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0061] In some optional examples, the volume ratio of the tetraethyl orthosilicate to the ethanol aqueous solution is 1:(4~5), for example, it can be 1:4.0, 1:4.1, 1:4.2, 1:4.3, 1:4.4, 1:4.5, 1:4.6, 1:4.7, 1:4.8, 1:4.9 or 1:5.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] In some optional examples, the nitric acid solution is added dropwise to adjust the pH value of the tetraethyl orthosilicate solution to 2-3, for example, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9 or 3.0, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] In some optional instances, the concentration of the nitric acid solution is 1~2 mol / L, for example, it can be 1.0 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.7 mol / L, 1.8 mol / L, 1.9 mol / L or 2.0 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0064] In some optional instances, the water bath heating temperature of the precursor solution is 40-60°C, for example, it can be 40°C, 42°C, 44°C, 46°C, 48°C, 50°C, 52°C, 54°C, 56°C, 58°C or 60°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0065] In some optional examples, the water bath heating time of the precursor solution is 80 to 120 min, for example, it can be 80 min, 85 min, 90 min, 95 min, 100 min, 105 min, 110 min, 115 min or 120 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] In some optional examples, the concentration of the silver nitrate solution is 0.08~0.1mol / L, for example, it can be 0.08mol / L, 0.082mol / L, 0.084mol / L, 0.086mol / L, 0.088mol / L, 0.09mol / L, 0.092mol / L, 0.094mol / L, 0.096mol / L, 0.098mol / L or 0.1mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0067] In some optional examples, the ratio of silver nitrate in the silver nitrate solution to the tetraethyl orthosilicate is (3~5) mg:1mL, for example, it can be 3.0 mg:1mL, 3.2 mg:1mL, 3.4 mg:1mL, 3.6 mg:1mL, 3.8 mg:1mL, 4.0 mg:1mL, 4.2 mg:1mL, 4.4 mg:1mL, 4.6 mg:1mL, 4.8 mg:1mL or 5.0 mg:1mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] In some optional examples, the reaction time of the silica sol and the silver nitrate solution is 1 to 3 hours, for example, it can be 1.0h, 1.2h, 1.4h, 1.6h, 1.8h, 2.0h, 2.2h, 2.4h, 2.6h, 2.8h or 3.0h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] In some optional examples, the volume ratio of ammonia water, ethanol and deionized water in the mixed solution is 1:(20~30):(2~3), for example, it can be 1:20:2, 1:21:2.1, 1:22:2.2, 1:23:2.3, 1:24:2.4, 1:25:2.5, 1:26:2.6, 1:27:2.7, 1:28:2.8, 1:29:2.9 or 1:30:3, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0070] In some optional examples, the volume ratio of the tetraethyl orthosilicate to the ammonia water in the mixed solution is 1:(100~150), for example, it can be 1:100, 1:105, 1:110, 1:115, 1:120, 1:125, 1:130, 1:135, 1:140, 1:145 or 1:150, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0071] In some optional instances, the mass fraction of the aqueous ammonia is 25 to 30 wt%, for example, it may be 25 wt%, 25.5 wt%, 26 wt%, 26.5 wt%, 27 wt%, 27.5 wt%, 28 wt%, 28.5 wt%, 29 wt%, 29.5 wt% or 30 wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0072] In some optional examples, the stirring time of the silica / nanosilver sol and the mixed solution is 5 to 6 hours, for example, it can be 5.0 hours, 5.1 hours, 5.2 hours, 5.3 hours, 5.4 hours, 5.5 hours, 5.6 hours, 5.7 hours, 5.8 hours, 5.9 hours or 6.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0073] In some optional examples, the heating temperature of the silica / nanosilver sol and the mixed solution is 30-40°C, for example, it can be 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C or 40°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0074] In some optional examples, the standing time of the silica / nanosilver gel is 24 to 48 hours, for example, it can be 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, 38 hours, 40 hours, 42 hours, 44 hours, 46 hours or 48 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0075] In some optional examples, the silica / nanosilver gel is immersed in anhydrous ethanol for 24 to 48 hours for aging, for example, it can be 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, 38 hours, 40 hours, 42 hours, 44 hours, 46 hours or 48 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0076] In some optional examples, the polydimethylsiloxane solution consists of polydimethylsiloxane and n-hexane.

[0077] In some optional examples, the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution is 10-20wt%, for example, it can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0078] In some optional examples, the ratio of the silica / nanosilver gel to the polydimethylsiloxane solution is 1g:(100~200)mL, for example, it can be 1g:100mL, 1g:110mL, 1g:120mL, 1g:130mL, 1g:140mL, 1g:150mL, 1g:160mL, 1g:170mL, 1g:180mL, 1g:190mL or 1g:200mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0079] In some optional examples, the immersion time of the silica / nanosilver gel in the polydimethylsiloxane solution is 1 to 2 hours, for example, it can be 1.0 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h, 1.5 h, 1.6 h, 1.7 h, 1.8 h, 1.9 h or 2.0 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0080] As a preferred technical solution of the present invention, in step (IV), the mass fraction of the acid solution is 30-40wt%, for example, it can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt%, 35wt%, 36wt%, 37wt%, 38wt%, 39wt% or 40wt%, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0081] In some optional examples, the acid solution is any one of hydrochloric acid solution, phosphoric acid solution, nitric acid solution, sulfuric acid solution, or a combination of at least two thereof.

[0082] In some optional examples, the ratio of the activated carbon to the acid in the acid solution is 1g:(2~3)mL, for example, it can be 1g:2.0mL, 1g:2.1mL, 1g:2.2mL, 1g:2.3mL, 1g:2.4mL, 1g:2.5mL, 1g:2.6mL, 1g:2.7mL, 1g:2.8mL, 1g:2.9mL or 1g:3.0mL, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0083] In some optional examples, the activated carbon is immersed in the acid solution for 3 to 5 hours, for example, 3.0 hours, 3.2 hours, 3.4 hours, 3.6 hours, 3.8 hours, 4.0 hours, 4.2 hours, 4.4 hours, 4.6 hours, 4.8 hours or 5.0 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0084] In some optional examples, the volume ratio of oxygen to nitrogen in the mixed gas is 1:(15~20), for example, it can be 1:15, 1:15.5, 1:16, 1:16.5, 1:17, 1:17.5, 1:18, 1:18.5, 1:19, 1:19.5 or 1:20, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0085] In some optional examples, the heating temperature of the high temperature oxidation treatment is 600~700℃, for example, it can be 600℃, 610℃, 620℃, 630℃, 640℃, 650℃, 660℃, 670℃, 680℃, 690℃ or 700℃, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0086] In some optional examples, the heating time of the high temperature oxidation treatment is 30 to 50 minutes, for example, it can be 30 minutes, 32 minutes, 34 minutes, 36 minutes, 38 minutes, 40 minutes, 42 minutes, 44 minutes, 46 minutes, 48 ​​minutes or 50 minutes, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0087] The oxygen-containing acidic functional groups on the surface of activated carbon are produced by the combined action of chemical oxidation modification and high-temperature oxidation modification. The present invention can increase the micropore volume of the activated carbon and enrich its surface with a sufficient number of acidic oxygen-containing functional groups by controlling the process conditions of high-temperature oxidation treatment and selecting reasonable heating temperature and heating time, thereby comprehensively improving the adsorption capacity of the modified activated carbon for pollutants, especially volatile organic compounds.

[0088] The present invention specifically limits the heating temperature of the high-temperature oxidation treatment to 600-700°C. During the high-temperature oxidation treatment, the oxygen-containing acidic functional groups on the surface of the activated carbon will decompose; at the same time, the carbon and oxygen on the surface of the activated carbon will undergo an oxidation reaction to generate oxygen-containing acidic functional groups. When the heating temperature of the high-temperature oxidation treatment is lower than 600°C, the decomposition amount of the oxygen-containing acidic functional groups is greater than the generation amount thereof, so that the net increase amount of the oxygen-containing acidic functional groups decreases. When the heating temperature of the high-temperature oxidation treatment is within the range of 600-700°C, the oxidation reaction between the carbon and oxygen on the surface of the activated carbon intensifies, and a larger number of oxygen-containing acidic functional groups can be generated in the same time. The generation amount of the oxygen-containing acidic functional groups is greater than the decomposition amount, so that the net increase amount of the oxygen-containing acidic functional groups increases.

[0089] The present invention specifically limits the heating time of the high-temperature oxidation treatment to 30 to 50 minutes. When the heating time of the high-temperature oxidation treatment is within the numerical range defined by the present invention, as the oxidation reaction time is prolonged, the microporous structure of the activated carbon collapses and rearranges, generating new micropores; at the same time, a large number of oxygen-containing acidic functional groups are generated inside and on the surface of the activated carbon. The oxygen-containing acidic functional groups will occupy a certain adsorption space, but the larger adsorption space can also be divided into smaller adsorption spaces, which is more conducive to the adsorption of volatile organic compounds. When the heating time of the high-temperature oxidation treatment exceeds 50 minutes, an excessive amount of oxygen-containing acidic functional groups will be generated on the surface and inside of the activated carbon. While occupying the adsorption space, the internal shrinkage phenomenon will also occur in the activated carbon, resulting in a decrease in the micropore volume of the activated carbon as the heating time is prolonged. Therefore, extending the heating time is conducive to the expansion of the micropore volume of the activated carbon, but too long a modification time will cause a decrease in the micropore volume of the activated carbon.

[0090] In some optional examples, the mass fraction of the composite oxidized activated carbon in the activated carbon suspension is 20~30wt%, for example, it can be 20wt%, 21wt%, 22wt%, 23wt%, 24wt%, 25wt%, 26wt%, 27wt%, 28wt%, 29wt% or 30wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0091] In some optional examples, the mass fraction of the silane coupling agent solution is 10-20wt%, for example, it can be 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt% or 20wt%, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0092] In some optional examples, the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent in the silane coupling agent solution is 1:(1.5~2.5), for example, it can be 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2.0, 1:2.1, 1:2.2, 1:2.3, 1:2.4 or 1:2.5, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0093] In some optional examples, the stirring time of the activated carbon suspension and the silane coupling agent solution is 5 to 6 hours, for example, it can be 5.0 hours, 5.1 hours, 5.2 hours, 5.3 hours, 5.4 hours, 5.5 hours, 5.6 hours, 5.7 hours, 5.8 hours, 5.9 hours or 6.0 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0094] In some optional examples, the heating temperature of the activated carbon suspension and the silane coupling agent solution is 70-80°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0095] As a preferred technical solution of the present invention, in step (V), the mass ratio of the silica / nanosilver aerogel, the modified activated carbon and the deionized water is (30-40):(8-10):100, for example, it can be 30:8:100, 31:8.2:100, 32:8.4:100, 33:8.6:100, 34:8.8:100, 35:9:100, 36:9.2:100, 37:9.4:100, 38:9.6:100, 39:9.8:100 or 40:10:100, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0096] The present invention can significantly improve the filtering performance of the modified filter material layer by adding silicon dioxide / nano-silver aerogel to the resin mixture, because the silicon dioxide / nano-silver aerogel has a porous structure, so that the specific surface area of ​​the modified filter material layer is increased, and pollutants and particulate matter can be efficiently adsorbed. In addition, the addition of silicon dioxide / nano-silver aerogel is also conducive to improving the mechanical properties of the modified filter material layer, because silicon dioxide / nano-silver aerogel has a certain mechanical strengthening effect on the modified filter material layer as an inorganic filler, and at the same time, silicon dioxide / nano-silver aerogel also plays the role of a nucleating agent in the melt-blown process of the polylactic acid resin mixture, promotes the heterogeneous nucleation of the polylactic acid resin, thereby improving the crystallinity of the polylactic acid resin mixture, so that the tensile strength of the melt-blown fiber is further improved. In addition, since the addition of silicon dioxide / nano-silver aerogel limits the movement of the polylactic acid macromolecular chain, the glass transition temperature of the polylactic acid resin mixture is increased, which helps to improve the thermal stability of the melt-blown fiber.

[0097] The present invention particularly defines the mass ratio of silica / nano-silver aerogel, modified activated carbon and deionized water as (30-40):(8-10):100. When the amount of silica / nano-silver aerogel added exceeds the upper limit of the numerical range defined by the present invention, the mechanical properties of the modified filter material layer will be reduced. This is because excessive silica / nano-silver aerogel will inhibit the crystallization of polylactic acid resin to a certain extent, so that the crystallinity of the polylactic acid resin mixture is reduced, which has an adverse effect on the mechanical properties of the melt-blown fiber. At the same time, excessive silica / nano-silver aerogel will agglomerate in the polylactic acid resin matrix, and the agglomerated silica / nano-silver aerogel will generate stress concentration in the melt-blown fiber, which is not conducive to improving the tensile strength of the modified filter material layer. In addition, excessive silica / nano-silver aerogel will also affect the filtration performance of the modified filter material layer. This is because, on the one hand, when the silica / nano-silver aerogel exceeds the upper limit of the range specified in the present invention, the average diameter of the melt-blown fibers will be too large, and the average pore size of the modified filter material layer formed after melt-blowing will increase, making it impossible to effectively intercept pollutants and particulate matter, ultimately resulting in a decrease in the filtration efficiency of the modified filter material layer; on the other hand, excessive silica / nano-silver aerogel will clog the microporous channels of the modified activated carbon, resulting in a decrease in the saturated adsorption capacity of the modified activated carbon, ultimately affecting the adsorption capacity of the modified filter material layer for volatile organic compounds.

[0098] In some optional examples, the ultrasonic power of the ultrasonic dispersion after mixing the silica / nanosilver aerogel, the modified activated carbon and the deionized water is 600~700W, for example, it can be 600W, 610W, 620W, 630W, 640W, 650W, 660W, 670W, 680W, 690W or 700W, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0099] In some optional examples, the ultrasonic dispersion time of the silica / nanosilver aerogel, the modified activated carbon and the deionized water after mixing is 10 to 12 hours, for example, it can be 10 hours, 10.2 hours, 10.4 hours, 10.6 hours, 10.8 hours, 11 hours, 11.2 hours, 11.4 hours, 11.6 hours, 11.8 hours or 12 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0100] In some optional examples, the mass ratio of the polylactic acid resin, the polyethylene glycol and the composite filler solution is 100:(5~10):(20~30), for example, it can be 100:5:20, 100:5.5:21, 100:6:22, 100:6.5:23, 100:7:24, 100:7.5:25, 100:8:26, 100:8.5:27, 100:9:28, 100:9.5:29 or 100:10:30, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0101] The pure polylactic acid resin melt has poor fluidity and is not easily stretched and refined when flowing through the meltblowing nozzle, so that the meltblown fiber formed by meltblowing has a larger diameter. The meltblown fiber with a larger diameter will cause the modified filter material layer formed after meltblowing to have a higher porosity and a larger pore size, so that the air permeability of the multi-layer ultrafine polypropylene modified filter bag is higher, the filtration efficiency is reduced, and pollutants and particulate matter cannot be effectively intercepted. The present invention adds polyethylene glycol to the polylactic acid resin, so that the fluidity of the polylactic acid resin melt after compounding is enhanced, the diameter of the meltblown fiber is reduced, the arrangement between the meltblown fibers is more closely, the porosity of the prepared modified filter material layer is reduced and the pore size is reduced, so that the filtration efficiency of the modified filter material layer is significantly improved.

[0102] As a preferred technical solution of the present invention, in step (V), the meltblowing equipment includes a screw extruder, a metering pump and a meltblowing head connected in sequence, a row of meltblowing ports are provided at the bottom of the meltblowing head, and air inlets connected to the meltblowing ports are symmetrically provided at the two side walls of the meltblowing head. A winding assembly consisting of a unwinding roller and a winding roller is provided below the meltblowing head, and the composite base fabric layer is wound between the unwinding roller and the winding roller; during the meltblowing process, the composite base fabric layer is driven by the winding assembly to be connected to the bottom of the meltblowing head. The polylactic acid resin, the polyethylene glycol and the composite filler solution are continuously transported, and are put into a second screw extruder. After being melted and extruded by the second screw extruder, a mixed melt is formed. The mixed melt is injected into the meltblowing head through a metering pump, and high-pressure hot air is injected into the meltblowing head through the air inlet. Under the stretching effect of the high-pressure hot air, the mixed melt passes through the meltblowing port to form a melt fine flow curtain and falls onto the surface of the continuously transported composite base fabric layer. After cooling and self-bonding, a modified filter material layer is formed on the surface of the composite base fabric layer.

[0103] In some optional examples, the interior of the barrel of the second screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction.

[0104] In some optional instances, the temperature of the first zone is 160-180°C, for example, it may be 160°C, 162°C, 164°C, 166°C, 168°C, 170°C, 172°C, 174°C, 176°C, 178°C or 180°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0105] In some optional instances, the temperature of the second zone is 180-200°C, for example, it may be 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, 192°C, 194°C, 196°C, 198°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0106] In some optional instances, the temperature of the third zone is 200-210°C, for example, it may be 200°C, 201°C, 202°C, 203°C, 204°C, 205°C, 206°C, 207°C, 208°C, 209°C or 210°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0107] In some optional instances, the temperature of the fourth zone is 210-220°C, for example, it may be 210°C, 211°C, 212°C, 213°C, 214°C, 215°C, 216°C, 217°C, 218°C, 219°C or 220°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0108] In some optional instances, the temperature of the fifth zone is 220-230°C, for example, it may be 220°C, 221°C, 222°C, 223°C, 224°C, 225°C, 226°C, 227°C, 228°C, 229°C or 230°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0109] In some optional examples, the screw speed of the second screw extruder is 100~200r / min, for example, it can be 100r / min, 110r / min, 120r / min, 130r / min, 140r / min, 150r / min, 160r / min, 170r / min, 180r / min, 190r / min or 200r / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0110] In some optional instances, the temperature of the high-pressure hot air is 180-200°C, for example, it may be 180°C, 182°C, 184°C, 186°C, 188°C, 190°C, 192°C, 194°C, 196°C, 198°C or 200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0111] In some optional instances, the pressure of the high-pressure hot air is 0.2~0.3MPa, for example, it can be 0.2MPa, 0.21MPa, 0.22MPa, 0.23MPa, 0.24MPa, 0.25MPa, 0.26MPa, 0.27MPa, 0.28MPa, 0.29MPa or 0.3MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0112] In some optional instances, the flow rate of the metering pump is 80~90g / min, for example, it can be 80g / min, 81g / min, 82g / min, 83g / min, 84g / min, 85g / min, 86g / min, 87g / min, 88g / min, 89g / min or 90g / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0113] As a preferred technical solution of the present invention, in step (V), the electric field intensity of the corona electret treatment is 9-10 kV / cm, for example, it can be 9.0 kV / cm, 9.1 kV / cm, 9.2 kV / cm, 9.3 kV / cm, 9.4 kV / cm, 9.5 kV / cm, 9.6 kV / cm, 9.7 kV / cm, 9.8 kV / cm, 9.9 kV / cm or 10.0 kV / cm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are equally applicable.

[0114] In some optional instances, the DC voltage of the corona electret treatment is 90~100kV, for example, can be 90kV, 91kV, 92kV, 93kV, 94kV, 95kV, 96kV, 97kV, 98kV, 99kV or 100kV, but is not limited to the enumerated numerical values, and other unenumerated numerical values ​​within the numerical range are equally applicable.

[0115] In some optional examples, the charging distance of the corona electret treatment is 9 to 10 cm, for example, it can be 9.0 cm, 9.1 cm, 9.2 cm, 9.3 cm, 9.4 cm, 9.5 cm, 9.6 cm, 9.7 cm, 9.8 cm, 9.9 cm or 10.0 cm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0116] In some optional examples, the corona electret treatment charging time is 30 to 40 s, for example, it can be 30 s, 31 s, 32 s, 33 s, 34 s, 35 s, 36 s, 37 s, 38 s, 39 s or 40 s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0117] Compared with the prior art, the present invention has the following beneficial effects:

[0118] The multi-layer ultrafine polypropylene modified filter bag prepared by the present invention consists of a composite base fabric layer and a modified filter material layer. By adding modified chitosan particles, not only the mechanical properties of the composite polypropylene fiber can be improved, but also a certain antibacterial ability can be given to the composite base fabric layer.

[0119] The present invention uses polydopamine to modify the surface of composite polypropylene fiber, utilizes the oxidative self-polymerization reaction of dopamine monomer at room temperature to form a polydopamine layer on the surface of the composite polypropylene fiber, and generates and firmly loads MOFs material on the surface of the coated polypropylene fiber in situ through the solvent thermal synthesis reaction of zinc nitrate solution and 2-methylimidazole solution, and finally prepares modified composite polypropylene fiber loaded with MOFs material. The present invention significantly improves the loading fastness of MOFs material on the surface of the coated polypropylene fiber through polydopamine coating.

[0120] The present invention adopts silica / nanosilver aerogel and modified activated carbon to melt-blend and modify the polylactic acid resin, which can not only improve the problems of slow crystallization rate and poor mechanical properties of polylactic acid, but also increase the specific surface area of ​​the polylactic acid matrix, thereby improving the filtration performance of the multi-layer ultrafine polypropylene modified filter bag and giving it excellent antibacterial and mechanical properties.

[0121] The present invention adopts chemical oxidation treatment and high-temperature oxidation treatment to carry out joint modification treatment on activated carbon, which is helpful to increase the pore volume of activated carbon micropores and secondary formation of activated carbon micropores, so that the saturated adsorption capacity of modified activated carbon can be increased, which is beneficial to improve the adsorption capacity of filter bags for pollutants. BRIEF DESCRIPTION OF THE DRAWINGS

[0122] Figure 1 A process flow chart of the manufacturing process of the multi-layer ultrafine polypropylene modified filter bag provided in Examples 1-5 of the present invention;

[0123] Figure 2 This is a schematic diagram of the structure of a multi-layer ultrafine polypropylene modified filter bag prepared in Examples 1-5 of the present invention;

[0124] Figure 3 A schematic structural diagram of a meltblowing device provided in one embodiment of the present invention;

[0125] Among them, 1-composite base fabric layer; 2-modified filter material layer; 3-screw extruder; 4-metering pump; 5-melt spray head; 6-unwinding roller; 7-winding roller; 8-air inlet; 9-melt spray outlet;

[0126] Figure 4 The following are scanning electron microscope images of the surface microstructures of the unmodified polypropylene fiber and the modified composite polypropylene fiber prepared in Example 1 of the present invention; wherein (a) is a scanning electron microscope image of the surface microstructure of the unmodified polypropylene fiber, and (b) is a scanning electron microscope image of the surface microstructure of the modified composite polypropylene fiber prepared in Example 1;

[0127] Figure 5 The infrared spectra of the silica aerogel and the silica / nanosilver aerogel prepared in Example 1 of the present invention;

[0128] Figure 6 The figures are colony culture pictures of Staphylococcus aureus by silica aerogel and silica / nanosilver aerogel prepared in Example 1 of the present invention, wherein (a) is a colony culture picture of Staphylococcus aureus by silica aerogel, and (b) is a colony culture picture of Staphylococcus aureus by silica / nanosilver aerogel prepared in Example 1;

[0129] Figure 7The figures are colony culture pictures of Escherichia coli on silica aerogel and silica / nanosilver aerogel prepared in Example 1 of the present invention, wherein (a) is a colony culture picture of Escherichia coli on silica aerogel, and (b) is a colony culture picture of Escherichia coli on silica / nanosilver aerogel prepared in Example 1;

[0130] Figure 8 The figures are scanning electron microscope images of untreated activated carbon and modified activated carbon prepared in Example 1 of the present invention, wherein (a) is a scanning electron microscope image of untreated activated carbon, and (b) is a scanning electron microscope image of modified activated carbon prepared in Example 1;

[0131] Fig. 9 This is a scanning electron microscope image of the surface micromorphology of the melt-blown fibers of the modified filter material layer prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0132] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and their accompanying drawings. The embodiments recorded herein are specific embodiments of the present invention, which are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limitations on the embodiments of the present invention and the scope of protection of the present invention. In addition to the embodiments recorded herein, those skilled in the art can also adopt other obvious technical solutions based on the contents disclosed in the claims of this application and its specification, including technical solutions that adopt any obvious replacements and modifications to the embodiments recorded herein.

[0133] In one embodiment, the present invention provides a melt-blown device for carrying out the method for manufacturing the multi-layer ultra-fine polypropylene modified filter bag provided by the present invention, such as Figure 3 As shown, it includes a screw extruder 3, a metering pump 4 and a meltblowing head 5 connected in sequence, a row of meltblowing ports 9 are provided at the bottom of the meltblowing head 5, and air inlets 8 connected to the meltblowing ports 9 are symmetrically provided at the two side walls of the meltblowing head 5. A winding assembly consisting of a discharge roller 6 and a winding roller 7 is provided below the meltblowing head 5, and a composite base fabric layer 1 is wound between the discharge roller 6 and the winding roller 7; during the meltblowing process, the composite base fabric layer 1 is continuously transmitted below the meltblowing head 5 through the winding assembly to transfer the polyurethane emulsion. Acid resin, polyethylene glycol and composite filler solution are put into the second screw extruder, and a mixed melt is formed after melt extrusion by the second screw extruder. The mixed melt is injected into the meltblowing head 5 through the metering pump 4, and high-pressure hot air is injected into the meltblowing head 5 through the air inlet 8. Under the stretching effect of the high-pressure hot air, the mixed melt passes through the meltblowing port 9 to form a melt fine flow curtain and falls onto the surface of the continuously transmitted composite base fabric layer 1. After cooling and self-adhesion, a modified filter material layer 2 is formed on the surface of the composite base fabric layer 1.

[0134] It should be noted that the chemical reagents used in the embodiments and comparative examples provided by the present invention are all commercially available products, and their brands and manufacturers are as follows:

[0135] Titanate coupling agent: JY-201, purchased from Nanjing Feiteng New Materials Technology Co., Ltd.;

[0136] Ethanol: purity >99%, purchased from Shandong Feier New Materials Co., Ltd.;

[0137] Sodium dodecylbenzene sulfonate: S15013-250g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0138] Chitosan: S11064-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0139] Polypropylene: S51655-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0140] Dopamine hydrochloride: RWE20232016, purchased from Hunan Ruiweier Biotechnology Co., Ltd.;

[0141] Tris-HCl buffer: FT-LG1039, purchased from Shanghai Fantai Biotechnology Co., Ltd.;

[0142] Zinc nitrate hexahydrate: purity >99%, purchased from Hubei Rishengchang New Materials Technology Co., Ltd.;

[0143] 2-Methylimidazole: S25048-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0144] Methanol: purity >99%, purchased from Fuchen (Tianjin) Chemical Reagent Co., Ltd.;

[0145] Tetraethyl orthosilicate: purity>99%, purchased from Wuhan Jiyesheng Chemical Co., Ltd.;

[0146] Nitric acid: purity>99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0147] Silver nitrate: S116264-5g, Shanghai Aladdin Biochemical Technology Co., Ltd.;

[0148] Ammonia: industrial grade, purchased from Shenyang Elex Chemical Co., Ltd.

[0149] Polydimethylsiloxane: T22990-100g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0150] Activated carbon: HBWS-H127, purchased from Hubei Weideli Chemical Technology Co., Ltd.;

[0151] Hydrochloric acid: purity>99%, purchased from Nanjing Chemical Reagent Co., Ltd.;

[0152] Cyclohexane: HG010, purchased from Jinan Chuangshi Chemical Co., Ltd.;

[0153] Silane coupling agent KH550: S15028-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0154] Silane coupling agent KH560: S15029-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0155] Silane coupling agent KH570: S15030-500ml, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0156] Polylactic acid resin: S30789-1g, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0157] Polyethylene glycol 1000: purity > 99%, purchased from Fuchen (Tianjin) Chemical Reagent Co., Ltd.;

[0158] Polyethylene glycol 2000: purity > 99%, purchased from Fuchen (Tianjin) Chemical Reagent Co., Ltd.

[0159] Example 1

[0160] This embodiment provides a method for manufacturing a multi-layer ultra-fine polypropylene modified filter bag, such as Figure 1 As shown, the manufacturing method specifically comprises the following steps:

[0161] (1) Adding a titanate coupling agent to an ethanol aqueous solution (wherein the volume ratio of ethanol to deionized water is 8:1), mixing and stirring at 50° C. for 1.5 h to obtain a 1 g / L coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, wherein the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate is 1.5:1, and mixing and stirring for 10 min to obtain a composite modified solution;

[0162] Chitosan was dry-milled at a speed of 300 rpm for 5 hours to obtain chitosan particles with a particle size of 20 nm, and the chitosan particles were dispersed in a composite modified solution, the mass ratio of chitosan particles to titanate coupling agent in the composite modified solution was 1:0.1, mixed and stirred for 1 hour, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin were mixed and put into a first screw extruder for melt extrusion, the extrusion temperature was 190°C, the screw speed was 100 r / min, and composite polypropylene masterbatch was obtained after cooling and granulation, and the composite polypropylene masterbatch was melt-spun to obtain composite polypropylene fiber;

[0163] (2) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, wherein the mass fraction of dopamine hydrochloride in the dopamine solution is 5 g / L, immersing the composite polypropylene fiber obtained in step (1) in the dopamine solution for 15 h to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing, and drying to obtain a coated polypropylene fiber;

[0164] Zinc nitrate hexahydrate and methanol are mixed in proportion to prepare a zinc nitrate solution with a concentration of 0.1 g / mL; 2-methylimidazole and methanol are mixed in proportion to prepare a 2-methylimidazole solution with a concentration of 0.15 g / mL; the coated polypropylene fiber is immersed in the zinc nitrate solution for 60 minutes, and the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is 1:20; then, the 2-methylimidazole solution is dripped in a molar ratio of zinc nitrate hexahydrate to 2-methylimidazole of 1:3, and the dripping speed is 1 mL / min. During the dripping process, stirring is continued to generate MOFs material in situ on the surface of the polydopamine layer. After all the dripping is completed, stirring is continued for 2 hours, and then taken out, washed, and dried to obtain a modified composite polypropylene fiber, and the modified composite polypropylene fiber is woven to form a composite base fabric layer 1 with a thickness of 1 mm and an average pore size of 70 μm, and the warp density of the composite base fabric layer 1 is 300 strands / 10 cm, and the weft density is 250 strands / 10 cm;

[0165] (3) mixing tetraethyl orthosilicate with an ethanol aqueous solution (wherein the volume ratio of ethanol to water is 1:1) to obtain a tetraethyl orthosilicate solution, wherein the volume ratio of tetraethyl orthosilicate to the ethanol aqueous solution is 1:4, adding 1 mol / L nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value of the tetraethyl orthosilicate solution to 3, thereby obtaining a precursor solution; heating the precursor solution in a water bath at a water bath temperature of 40° C. for 120 min, and obtaining a silica sol after the water bath heating is completed;

[0166] The silica sol was dropped into a 0.08 mol / L silver nitrate solution, wherein the ratio of silver nitrate to tetraethyl orthosilicate was 3 mg:1 mL, and the reaction was stirred for 3 h under light-proof conditions to obtain a silica / nanosilver sol. A mixed solution consisting of ammonia water, ethanol and deionized water was added to the silica / nanosilver sol (wherein the mass fraction of ammonia water was 25 wt %, the volume ratio of ammonia water, ethanol and deionized water was 1:20:2, and the volume ratio of tetraethyl orthosilicate to ammonia water in the mixed solution was 1:100), and the mixed solution was mixed and stirred at 30° C. for 6 h to gel the silica / nanosilver sol to form a silica / nanosilver gel;

[0167] The silica / nanosilver gel was allowed to stand for 24 hours, and then immersed in anhydrous ethanol for 24 hours for aging. The washed silica / nanosilver gel was immersed in a polydimethylsiloxane solution at a ratio of 1 g:100 mL for 2 hours for hydrophobic modification, wherein the polydimethylsiloxane solution consisted of polydimethylsiloxane and n-hexane, and the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution was 20 wt %. Finally, the silica / nanosilver aerogel powder was obtained after washing, drying and grinding.

[0168] (4) The activated carbon is immersed in a 30wt% hydrochloric acid solution for 5 hours, wherein the ratio of the activated carbon to the hydrochloric acid in the hydrochloric acid solution is 1g:2mL. After the immersion is completed, the activated carbon is filtered, washed and dried to obtain chemically oxidized activated carbon; the chemically oxidized activated carbon is placed in a tubular furnace, and a mixed gas composed of oxygen and nitrogen is introduced into the tubular furnace, wherein the volume ratio of oxygen to nitrogen in the mixed gas is 1:15, and the chemically oxidized activated carbon is subjected to high-temperature oxidation treatment, wherein the heating temperature of the high-temperature oxidation treatment is 600°C and the heating time is 50min, and after the high-temperature oxidation treatment, a composite oxidized activated carbon is obtained;

[0169] The composite oxidized activated carbon is dispersed in cyclohexane to form a 20wt% activated carbon suspension, and a 20wt% silane coupling agent KH550 solution is added to the activated carbon suspension under stirring conditions, wherein the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent KH550 in the silane coupling agent KH550 solution is 1:1.5, and the activated carbon suspension and the silane coupling agent KH550 solution are mixed and stirred at 70°C for 6h to react to obtain a reaction product, and the reaction product is filtered, washed and dried to obtain a modified activated carbon;

[0170] (5) mixing the silica / nanosilver aerogel obtained in step (3), the modified activated carbon obtained in step (4) and deionized water in a mass ratio of 30:8:100, and performing ultrasonic dispersion at an ultrasonic power of 600 W for 12 h during the mixing process to obtain a composite filler solution;

[0171] Polylactic acid resin, polyethylene glycol 1000 and composite filler solution are put into a melt-blowing device in a mass ratio of 100:5:20, and the surface of the composite base fabric layer 1 obtained in step (2) is melt-blown by the melt-blowing device to form a modified filter material layer 2 with a thickness of 2 mm and an average pore size of 15 μm; wherein the temperature of the first zone of the second screw extruder is 160°C, the temperature of the second zone is 180°C, the temperature of the third zone is 200°C, the temperature of the fourth zone is 210°C, the temperature of the fifth zone is 220°C, and the screw speed is 100 r / min; the temperature of the high-pressure hot air is 180°C, and the pressure is 0.2 MPa; the flow rate of the metering pump 4 is 80 g / min; then, the composite layer composed of the modified filter material layer 2 and the composite base fabric layer 1 is subjected to corona electret treatment, the electric field intensity of the corona electret treatment is 9 kV / cm, the DC voltage is 90 kV, the charging distance is 9 cm, the electret time is 30 s, and after the corona electret treatment, the following is obtained Figure 2 Multi-layer ultra-fine polypropylene modified filter bag shown.

[0172] Figure 4 The scanning electron microscope images are surface micromorphologies of unmodified polypropylene fiber and modified composite polypropylene fiber prepared in Example 1 of the present invention. As can be seen from (a), the surface of the unmodified polypropylene fiber is relatively smooth; as can be seen from (b), the surface of the modified composite polypropylene fiber is loaded with MOFs material particles, and the surface roughness of the fiber is improved.

[0173] Figure 5 The infrared spectra of the silica aerogel and the silica / nanosilver aerogel prepared in Example 1 of the present invention are shown in FIG. Figure 5 It can be seen that in the infrared spectrum of silica aerogel, 800cm -1 and 1080cm -1 The symmetrical stretching vibration peak and asymmetrical stretching vibration peak of Si-O-Si are shown in the infrared spectrum of silica / nanosilver aerogel at 1275 cm -1 and 2980cm -1 The asymmetric stretching vibration peaks of Si-CH3 and antisymmetric stretching vibration peaks of -CH3 appeared at 1625cm -1 and 3458cm -1 The -OH absorption peak is greatly weakened in the infrared spectra of silica aerogel and silica / nanosilver aerogel, indicating that most of the -OH on the surface of silica / nanosilver aerogel is replaced by -CH3.

[0174] Figure 6 The following are colony culture pictures of Staphylococcus aureus by silica aerogel and silica / nanosilver aerogel prepared in Example 1 of the present invention. Figure 7The following are pictures of the bacterial colony culture of Escherichia coli by silica aerogel and silica / nanosilver aerogel prepared in Example 1 of the present invention. Figure 6 and Figure 7 It can be seen that silica aerogel does not show antibacterial activity against Staphylococcus aureus and Escherichia coli; while silica / nanosilver aerogel shows obvious antibacterial activity against both Staphylococcus aureus and Escherichia coli, and the antibacterial rates against both Staphylococcus aureus and Escherichia coli reach 99.9%, achieving high antibacterial efficiency.

[0175] Figure 8 The scanning electron microscope images of untreated activated carbon and modified activated carbon prepared in Example 1 of the present invention show that a large number of pore structures appear on the surface of the modified activated carbon, and the specific surface area and pore volume of the modified activated carbon are increased by comparing (a) and (b).

[0176] Fig. 9 This is a scanning electron microscope image of the microscopic morphology of the fiber surface of the modified filter material layer 2 prepared in Example 1 of the present invention. It can be seen that the fiber surface of the modified filter material layer 2 is loaded with silicon dioxide / nanosilver gel and modified activated carbon.

[0177] Example 2

[0178] This embodiment provides a method for manufacturing a multi-layer ultra-fine polypropylene modified filter bag, such as Figure 1 As shown, the manufacturing method specifically comprises the following steps:

[0179] (1) adding a titanate coupling agent to an ethanol aqueous solution (wherein the volume ratio of ethanol to deionized water is 8.2:1), mixing and stirring at 52°C for 1.2 hours to obtain a 2 g / L coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, wherein the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate is 1.8:1, and mixing and stirring for 15 minutes to obtain a composite modified solution;

[0180] Chitosan was dry-milled at a speed of 320 rpm for 4.5 hours to obtain chitosan particles with a particle size of 22 nm, and the chitosan particles were dispersed in a composite modified solution, the mass ratio of chitosan particles to titanate coupling agent in the composite modified solution was 1:0.12, and mixed and stirred for 1.5 hours, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin were mixed and put into a first screw extruder for melt extrusion, the extrusion temperature was 192°C, the screw speed was 120 r / min, and composite polypropylene masterbatch was obtained after cooling and granulation, and the composite polypropylene masterbatch was melt-spun to obtain composite polypropylene fiber;

[0181] (2) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, wherein the mass fraction of dopamine hydrochloride in the dopamine solution is 6 g / L, immersing the composite polypropylene fiber obtained in step (1) in the dopamine solution for 14 h to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing, and drying to obtain a coated polypropylene fiber;

[0182] Zinc nitrate hexahydrate and methanol are mixed in proportion to prepare a zinc nitrate solution with a concentration of 0.12 g / mL; 2-methylimidazole and methanol are mixed in proportion to prepare a 2-methylimidazole solution with a concentration of 0.18 g / mL; the coated polypropylene fiber is immersed in the zinc nitrate solution for 58 minutes, and the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is 1:22; then, the 2-methylimidazole solution is dropped according to the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole of 1:3.2, and the dropping speed is 2 mL / min. During the dropping process, stirring is continued to generate MOFs material in situ on the surface of the polydopamine layer. After all the dropping is completed, stirring is continued for 1.8 hours, and then taken out, washed, and dried to obtain a modified composite polypropylene fiber, and the modified composite polypropylene fiber is woven to form a composite base fabric layer 1 with a thickness of 1.5 mm and an average pore size of 68 μm, and the warp density of the composite base fabric layer 1 is 310 strands / 10 cm and the weft density is 260 strands / 10 cm;

[0183] (3) mixing tetraethyl orthosilicate with an ethanol aqueous solution (wherein the volume ratio of ethanol to water is 1:1.2) to obtain a tetraethyl orthosilicate solution, wherein the volume ratio of tetraethyl orthosilicate to the ethanol aqueous solution is 1:4.2, adding 1.2 mol / L nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value of the tetraethyl orthosilicate solution to 2.8, thereby obtaining a precursor solution; heating the precursor solution in a water bath at a water bath temperature of 45° C. for 110 min, and obtaining a silica sol after the water bath heating;

[0184] The silica sol was dropped into a 0.085 mol / L silver nitrate solution, the ratio of silver nitrate to tetraethyl orthosilicate was 3.5 mg:1 mL, and the reaction was stirred for 2.5 h under light-proof conditions to obtain a silica / nanosilver sol. A mixed solution consisting of ammonia water, ethanol and deionized water was added to the silica / nanosilver sol (wherein the mass fraction of ammonia water was 26 wt %, the volume ratio of ammonia water, ethanol and deionized water was 1:22:2.2, and the volume ratio of tetraethyl orthosilicate to ammonia water in the mixed solution was 1:120. The mixed solution was mixed and stirred at 32° C. for 5.8 h to gel the silica / nanosilver sol to form a silica / nanosilver gel;

[0185] The silica / nanosilver gel was allowed to stand for 30 hours, and then immersed in anhydrous ethanol for 30 hours for aging, and the washed silica / nanosilver gel was immersed in a polydimethylsiloxane solution at a ratio of 1g:120mL for 1.8 hours for hydrophobic modification, wherein the polydimethylsiloxane solution consists of polydimethylsiloxane and n-hexane, and the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution is 18wt%, and finally, the silica / nanosilver aerogel powder was obtained after washing, drying and grinding;

[0186] (4) The activated carbon was immersed in a 32 wt % phosphoric acid solution for 4.5 h, wherein the ratio of the activated carbon to the phosphoric acid in the phosphoric acid solution was 1 g:2.2 mL. After the immersion, the activated carbon was filtered, washed and dried to obtain chemically oxidized activated carbon. The chemically oxidized activated carbon was placed in a tubular furnace, and a mixed gas composed of oxygen and nitrogen was introduced into the tubular furnace. The volume ratio of oxygen and nitrogen in the mixed gas was 1:16. The chemically oxidized activated carbon was subjected to high-temperature oxidation treatment. The heating temperature of the high-temperature oxidation treatment was 620° C. and the heating time was 45 min. After the high-temperature oxidation treatment, composite oxidized activated carbon was obtained.

[0187] The composite oxidized activated carbon is dispersed in cyclohexane to form a 22wt% activated carbon suspension, and an 18wt% silane coupling agent KH560 solution is added to the activated carbon suspension under stirring conditions, wherein the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent KH560 in the silane coupling agent KH560 solution is 1:1.8, and the activated carbon suspension and the silane coupling agent KH560 solution are mixed and stirred at 72°C for 5.8h to react to obtain a reaction product, and the reaction product is filtered, washed and dried to obtain a modified activated carbon;

[0188] (5) mixing the silica / nanosilver aerogel obtained in step (3), the modified activated carbon obtained in step (4) and deionized water in a mass ratio of 32:8.5:100, and performing ultrasonic dispersion at an ultrasonic power of 620 W for 11.5 h during the mixing process to obtain a composite filler solution;

[0189] Polylactic acid resin, polyethylene glycol 1000 and composite filler solution are put into a melt-blowing device in a mass ratio of 100:6:22, and the surface of the composite base fabric layer 1 obtained in step (2) is melt-blown by the melt-blowing device to form a modified filter material layer 2 with a thickness of 2.5 mm and an average pore size of 18 μm; wherein the temperature of the first zone of the second screw extruder is 165°C, the temperature of the second zone is 185°C, the temperature of the third zone is 202°C, the temperature of the fourth zone is 212°C, the temperature of the fifth zone is 222°C, and the screw speed is 120 r / min; the temperature of the high-pressure hot air is 185°C, and the pressure is 0.22 MPa; the flow rate of the metering pump 4 is 82 g / min; then, the composite layer composed of the modified filter material layer 2 and the composite base fabric layer 1 is subjected to corona electret treatment, the electric field intensity of the corona electret treatment is 9.2 kV / cm, the DC voltage is 92 kV, the charging distance is 9.2 cm, the electret time is 32 s, and after the corona electret treatment, the following is obtained Figure 2 Multi-layer ultra-fine polypropylene modified filter bag shown.

[0190] Example 3

[0191] This embodiment provides a method for manufacturing a multi-layer ultra-fine polypropylene modified filter bag, such as Figure 1 As shown, the manufacturing method specifically comprises the following steps:

[0192] (1) adding a titanate coupling agent to an ethanol aqueous solution (wherein the volume ratio of ethanol to deionized water is 8.5:1), mixing and stirring at 55°C for 1 hour to obtain a 3 g / L coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, wherein the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate is 2:1, and mixing and stirring for 20 minutes to obtain a composite modified solution;

[0193] Chitosan was dry-milled at a speed of 350 rpm for 4 hours to obtain chitosan particles with a particle size of 25 nm, and the chitosan particles were dispersed in a composite modified solution, the mass ratio of chitosan particles to titanate coupling agent in the composite modified solution was 1:0.15, mixed and stirred for 2 hours, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin were mixed and put into a first screw extruder for melt extrusion, the extrusion temperature was 195°C, the screw speed was 150 r / min, and composite polypropylene masterbatch was obtained after cooling and granulation, and the composite polypropylene masterbatch was melt-spun to obtain composite polypropylene fiber;

[0194] (2) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, wherein the mass fraction of dopamine hydrochloride in the dopamine solution is 7 g / L, immersing the composite polypropylene fiber obtained in step (1) in the dopamine solution for 13 h to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing, and drying to obtain a coated polypropylene fiber;

[0195] Zinc nitrate hexahydrate and methanol are mixed in proportion to prepare a zinc nitrate solution with a concentration of 0.15 g / mL; 2-methylimidazole and methanol are mixed in proportion to prepare a 2-methylimidazole solution with a concentration of 0.2 g / mL; the coated polypropylene fiber is immersed in the zinc nitrate solution for 55 minutes, and the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is 1:25; then, the 2-methylimidazole solution is dropped according to the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole of 1:3.5, and the dropping speed is 3 mL / min. During the dropping process, stirring is continued to generate MOFs material in situ on the surface of the polydopamine layer. After all the dropping is completed, stirring is continued for 1.5 hours, and then taken out, washed and dried to obtain modified composite polypropylene fiber, and the modified composite polypropylene fiber is woven to form a composite base fabric layer 1 with a thickness of 2 mm and an average pore size of 65 μm, and the warp density of the composite base fabric layer 1 is 320 strands / 10 cm and the weft density is 270 strands / 10 cm;

[0196] (3) mixing tetraethyl orthosilicate with an ethanol aqueous solution (wherein the volume ratio of ethanol to water is 1:1.5) to obtain a tetraethyl orthosilicate solution, wherein the volume ratio of tetraethyl orthosilicate to the ethanol aqueous solution is 1:4.5, adding 1.5 mol / L nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value of the tetraethyl orthosilicate solution to 2.5, thereby obtaining a precursor solution; heating the precursor solution in a water bath at a water bath temperature of 50° C. for 100 min, and obtaining a silica sol after the water bath heating is completed;

[0197] The silica sol is dropped into a 0.09 mol / L silver nitrate solution, the ratio of silver nitrate to tetraethyl orthosilicate is 4 mg:1 mL, and the reaction is stirred for 2 h under light-proof conditions to obtain a silica / nanosilver sol, and a mixed solution consisting of ammonia water, ethanol and deionized water is added to the silica / nanosilver sol (wherein the mass fraction of ammonia water is 27 wt %, the volume ratio of ammonia water, ethanol and deionized water is 1:25:2.5, and the volume ratio of tetraethyl orthosilicate to ammonia water in the mixed solution is 1:130, and the mixed solution is mixed and stirred at 35° C. for 5.5 h to gel the silica / nanosilver sol to form a silica / nanosilver gel;

[0198] The silica / nanosilver gel was allowed to stand for 36 hours, and then immersed in anhydrous ethanol for 36 hours for aging. The washed silica / nanosilver gel was immersed in a polydimethylsiloxane solution at a ratio of 1 g:150 mL for 1.5 hours for hydrophobic modification, wherein the polydimethylsiloxane solution consisted of polydimethylsiloxane and n-hexane, and the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution was 15 wt %. Finally, the silica / nanosilver aerogel powder was obtained after washing, drying and grinding.

[0199] (4) The activated carbon is immersed in a 35wt% nitric acid solution for 4 hours, wherein the ratio of the activated carbon to the nitric acid in the nitric acid solution is 1g:2.5mL. After the immersion is completed, the activated carbon is filtered, washed and dried to obtain chemically oxidized activated carbon; the chemically oxidized activated carbon is placed in a tubular furnace, and a mixed gas composed of oxygen and nitrogen is introduced into the tubular furnace, wherein the volume ratio of oxygen to nitrogen in the mixed gas is 1:17, and the chemically oxidized activated carbon is subjected to high-temperature oxidation treatment, wherein the heating temperature of the high-temperature oxidation treatment is 650°C and the heating time is 40min, and after the high-temperature oxidation treatment, a composite oxidized activated carbon is obtained;

[0200] The composite oxidized activated carbon is dispersed in cyclohexane to form a 25wt% activated carbon suspension, and a 15wt% silane coupling agent KH560 solution is added to the activated carbon suspension under stirring conditions, wherein the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent KH560 in the silane coupling agent KH560 solution is 1:2, and the activated carbon suspension and the silane coupling agent KH560 solution are mixed and stirred at 75°C for 5.5h to react to obtain a reaction product, and the reaction product is filtered, washed and dried to obtain a modified activated carbon;

[0201] (5) mixing the silica / nanosilver aerogel obtained in step (3), the modified activated carbon obtained in step (4) and deionized water in a mass ratio of 35:9:100, and performing ultrasonic dispersion at an ultrasonic power of 650 W for 11 hours during the mixing process to obtain a composite filler solution;

[0202] Polylactic acid resin, polyethylene glycol 2000 and composite filler solution are put into a melt-blowing device in a mass ratio of 100:7:25, and the surface of the composite base fabric layer 1 obtained in step (2) is melt-blown by the melt-blowing device to form a modified filter material layer 2 with a thickness of 3 mm and an average pore size of 20 μm; wherein the temperature of the first zone of the second screw extruder is 170°C, the temperature of the second zone is 190°C, the temperature of the third zone is 205°C, the temperature of the fourth zone is 215°C, the temperature of the fifth zone is 225°C, and the screw speed is 150 r / min; the temperature of the high-pressure hot air is 190°C, and the pressure is 0.25 MPa; the flow rate of the metering pump 4 is 85 g / min; then, the composite layer composed of the modified filter material layer 2 and the composite base fabric layer 1 is subjected to corona electret treatment, the electric field intensity of the corona electret treatment is 9.5 kV / cm, the DC voltage is 95 kV, the charging distance is 9.5 cm, the electret time is 35 s, and after the corona electret treatment, the following is obtained Figure 2 Multi-layer ultra-fine polypropylene modified filter bag shown.

[0203] Example 4

[0204] This embodiment provides a method for manufacturing a multi-layer ultra-fine polypropylene modified filter bag, such as Figure 1As shown, the manufacturing method specifically comprises the following steps:

[0205] (1) adding a titanate coupling agent to an ethanol aqueous solution (wherein the volume ratio of ethanol to deionized water is 8.8:1), mixing and stirring at 58°C for 0.8h to obtain a 4 g / L coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, wherein the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate is 2.2:1, and mixing and stirring for 25min to obtain a composite modified solution;

[0206] Chitosan was dry-milled at a speed of 380 rpm for 3.5 hours to obtain chitosan particles with a particle size of 28 nm, and the chitosan particles were dispersed in a composite modified solution, the mass ratio of chitosan particles to titanate coupling agent in the composite modified solution was 1:0.18, and mixed and stirred for 2.5 hours, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin were mixed and put into a first screw extruder for melt extrusion, the extrusion temperature was 198°C, the screw speed was 180 r / min, and composite polypropylene masterbatch was obtained after cooling and granulation, and the composite polypropylene masterbatch was melt-spun to obtain composite polypropylene fiber;

[0207] (2) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, wherein the mass fraction of dopamine hydrochloride in the dopamine solution is 8 g / L, immersing the composite polypropylene fiber obtained in step (1) in the dopamine solution for 12 h to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing, and drying to obtain a coated polypropylene fiber;

[0208] Zinc nitrate hexahydrate and methanol are mixed in proportion to prepare a zinc nitrate solution with a concentration of 0.18 g / mL; 2-methylimidazole and methanol are mixed in proportion to prepare a 2-methylimidazole solution with a concentration of 0.22 g / mL; the coated polypropylene fiber is immersed in the zinc nitrate solution for 52 minutes, and the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is 1:28; then, the 2-methylimidazole solution is dropped according to the molar ratio of zinc nitrate hexahydrate to 2-methylimidazole of 1:3.8, and the dropping speed is 4 mL / min. During the dropping process, stirring is continued to generate MOFs material in situ on the surface of the polydopamine layer. After all the dropping is completed, stirring is continued for 1.2 hours, and then taken out, washed and dried to obtain modified composite polypropylene fiber, and the modified composite polypropylene fiber is woven to form a composite base fabric layer 1 with a thickness of 2.5 mm and an average pore size of 62 μm, and the warp density of the composite base fabric layer 1 is 330 strands / 10 cm and the weft density is 280 strands / 10 cm;

[0209] (3) mixing tetraethyl orthosilicate with an ethanol aqueous solution (wherein the volume ratio of ethanol to water is 1:1.8) to obtain a tetraethyl orthosilicate solution, wherein the volume ratio of tetraethyl orthosilicate to the ethanol aqueous solution is 1:4.8, adding 1.8 mol / L nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value of the tetraethyl orthosilicate solution to 2.2, thereby obtaining a precursor solution; heating the precursor solution in a water bath at a water bath temperature of 55° C. for 90 min, and obtaining a silica sol after the water bath heating;

[0210] The silica sol was dropped into a 0.095 mol / L silver nitrate solution, the ratio of silver nitrate to tetraethyl orthosilicate was 4.5 mg:1 mL, and the reaction was stirred for 1.5 h under light-proof conditions to obtain a silica / nanosilver sol. A mixed solution consisting of ammonia water, ethanol and deionized water was added to the silica / nanosilver sol (wherein the mass fraction of ammonia water was 28 wt %, the volume ratio of ammonia water, ethanol and deionized water was 1:28:2.8, and the volume ratio of tetraethyl orthosilicate to ammonia water in the mixed solution was 1:140. The mixed solution was mixed and stirred at 38° C. for 5.2 h to gel the silica / nanosilver sol to form a silica / nanosilver gel;

[0211] The silica / nanosilver gel was allowed to stand for 42 hours, and then immersed in anhydrous ethanol for 42 hours for aging. The washed silica / nanosilver gel was immersed in a polydimethylsiloxane solution at a ratio of 1 g:180 mL for 1.2 hours for hydrophobic modification, wherein the polydimethylsiloxane solution consisted of polydimethylsiloxane and n-hexane, and the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution was 12 wt %. Finally, the silica / nanosilver aerogel powder was obtained after washing, drying and grinding.

[0212] (4) The activated carbon was immersed in a 38 wt% nitric acid solution for 3.5 h, wherein the ratio of the activated carbon to the nitric acid in the nitric acid solution was 1 g:2.8 mL. After the immersion, the activated carbon was filtered, washed and dried to obtain chemically oxidized activated carbon. The chemically oxidized activated carbon was placed in a tubular furnace, and a mixed gas composed of oxygen and nitrogen was introduced into the tubular furnace. The volume ratio of oxygen and nitrogen in the mixed gas was 1:18. The chemically oxidized activated carbon was subjected to high-temperature oxidation treatment. The heating temperature of the high-temperature oxidation treatment was 680°C and the heating time was 35 min. After the high-temperature oxidation treatment, composite oxidized activated carbon was obtained.

[0213] The composite oxidized activated carbon is dispersed in cyclohexane to form a 28 wt % activated carbon suspension, and a 12 wt % silane coupling agent KH570 solution is added to the activated carbon suspension under stirring conditions, wherein the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent KH570 in the silane coupling agent KH570 solution is 1:2.3, and the activated carbon suspension and the silane coupling agent KH570 solution are mixed and stirred at 78° C. for 5.2 h to react to obtain a reaction product, and the reaction product is filtered, washed and dried to obtain a modified activated carbon;

[0214] (5) mixing the silica / nanosilver aerogel obtained in step (3), the modified activated carbon obtained in step (4) and deionized water in a mass ratio of 38:9.5:100, and performing ultrasonic dispersion at an ultrasonic power of 680 W for 10.5 h during the mixing process to obtain a composite filler solution;

[0215] Polylactic acid resin, polyethylene glycol 2000 and composite filler solution are put into a melt-blowing device in a mass ratio of 100:8:28, and the surface of the composite base fabric layer 1 obtained in step (2) is melt-blown by the melt-blowing device to form a modified filter material layer 2 with a thickness of 3.5 mm and an average pore size of 22 μm; wherein the temperature of the first zone of the second screw extruder is 175°C, the temperature of the second zone is 195°C, the temperature of the third zone is 208°C, the temperature of the fourth zone is 218°C, the temperature of the fifth zone is 228°C, and the screw speed is 180 r / min; the temperature of the high-pressure hot air is 195°C, and the pressure is 0.28 MPa; the flow rate of the metering pump 4 is 88 g / min; then, the composite layer composed of the modified filter material layer 2 and the composite base fabric layer 1 is subjected to corona electret treatment, the electric field intensity of the corona electret treatment is 9.8 kV / cm, the DC voltage is 98 kV, the charging distance is 9.8 cm, the electret time is 38 s, and after the corona electret treatment, the following is obtained Figure 2 Multi-layer ultra-fine polypropylene modified filter bag shown.

[0216] Example 5

[0217] This embodiment provides a method for manufacturing a multi-layer ultra-fine polypropylene modified filter bag, such as Figure 1 As shown, the manufacturing method specifically comprises the following steps:

[0218] (1) adding a titanate coupling agent to an ethanol aqueous solution (wherein the volume ratio of ethanol to deionized water is 9:1), mixing and stirring at 60°C for 0.5 h to obtain a 5 g / L coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, wherein the mass ratio of the titanate coupling agent to the sodium dodecylbenzene sulfonate is 2.5:1, and mixing and stirring for 30 min to obtain a composite modified solution;

[0219] Chitosan was dry-milled at a speed of 400 rpm for 3 hours to obtain chitosan particles with a particle size of 30 nm, and the chitosan particles were dispersed in a composite modified solution, the mass ratio of chitosan particles to titanate coupling agent in the composite modified solution was 1:0.2, mixed and stirred for 3 hours, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin were mixed and put into a first screw extruder for melt extrusion, the extrusion temperature was 200°C, the screw speed was 200 r / min, and composite polypropylene masterbatch was obtained after cooling and granulation, and the composite polypropylene masterbatch was melt-spun to obtain composite polypropylene fiber;

[0220] (2) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, wherein the mass fraction of dopamine hydrochloride in the dopamine solution is 10 g / L, immersing the composite polypropylene fiber obtained in step (1) in the dopamine solution for 10 h to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing, and drying to obtain a coated polypropylene fiber;

[0221] Zinc nitrate hexahydrate and methanol are mixed in proportion to prepare a zinc nitrate solution with a concentration of 0.2 g / mL; 2-methylimidazole and methanol are mixed in proportion to prepare a 2-methylimidazole solution with a concentration of 0.25 g / mL; the coated polypropylene fiber is immersed in the zinc nitrate solution for 50 minutes, and the mass ratio of the coated polypropylene fiber to zinc nitrate hexahydrate is 1:30; then, the 2-methylimidazole solution is dripped in a molar ratio of zinc nitrate hexahydrate to 2-methylimidazole of 1:4, and the dripping speed is 5 mL / min. During the dripping process, stirring is continued to generate MOFs material in situ on the surface of the polydopamine layer. After all the dripping is completed, stirring is continued for 1 hour, and then taken out, washed and dried to obtain a modified composite polypropylene fiber, and the modified composite polypropylene fiber is woven to form a composite base fabric layer 1 with a thickness of 3 mm and an average pore size of 60 μm, and the warp density of the composite base fabric layer 1 is 350 strands / 10 cm and the weft density is 300 strands / 10 cm;

[0222] (3) mixing tetraethyl orthosilicate with an ethanol aqueous solution (wherein the volume ratio of ethanol to water is 1:2) to obtain a tetraethyl orthosilicate solution, wherein the volume ratio of tetraethyl orthosilicate to the ethanol aqueous solution is 1:5, adding a 2 mol / L nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value of the tetraethyl orthosilicate solution to 2, thereby obtaining a precursor solution; heating the precursor solution in a water bath at a water bath temperature of 60° C. for 80 min, and obtaining a silica sol after the water bath heating is completed;

[0223] The silica sol is dropped into a 0.1 mol / L silver nitrate solution, the ratio of silver nitrate to tetraethyl orthosilicate is 5 mg:1 mL, and the reaction is stirred for 1 h under light-proof conditions to obtain a silica / nanosilver sol. A mixed solution consisting of ammonia water, ethanol and deionized water is added to the silica / nanosilver sol (wherein the mass fraction of ammonia water is 30 wt %, the volume ratio of ammonia water, ethanol and deionized water is 1:30:3, and the volume ratio of tetraethyl orthosilicate to ammonia water in the mixed solution is 1:150), and the mixed solution is mixed and stirred at 40° C. for 5 h to gel the silica / nanosilver sol to form a silica / nanosilver gel;

[0224] The silica / nanosilver gel was allowed to stand for 48 hours, and then immersed in anhydrous ethanol for 48 hours for aging. The washed silica / nanosilver gel was immersed in a polydimethylsiloxane solution at a ratio of 1 g:200 mL for 1 hour for hydrophobic modification, wherein the polydimethylsiloxane solution consisted of polydimethylsiloxane and n-hexane, and the mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution was 10 wt %. Finally, the silica / nanosilver aerogel powder was obtained after washing, drying and grinding.

[0225] (4) The activated carbon is immersed in a 40wt% sulfuric acid solution for 3h, the ratio of the activated carbon to the sulfuric acid in the sulfuric acid solution is 1g:3mL, and after the immersion is completed, it is filtered, washed and dried to obtain chemically oxidized activated carbon; the chemically oxidized activated carbon is placed in a tubular furnace, and a mixed gas composed of oxygen and nitrogen is introduced into the tubular furnace, and the volume ratio of oxygen and nitrogen in the mixed gas is 1:20, and the chemically oxidized activated carbon is subjected to high-temperature oxidation treatment, the heating temperature of the high-temperature oxidation treatment is 700°C, and the heating time is 30min. After the high-temperature oxidation treatment, a composite oxidized activated carbon is obtained;

[0226] The composite oxidized activated carbon is dispersed in cyclohexane to form a 30wt% activated carbon suspension, and a 10wt% silane coupling agent KH570 solution is added to the activated carbon suspension under stirring conditions, wherein the mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent KH570 in the silane coupling agent KH570 solution is 1:2.5, and the activated carbon suspension and the silane coupling agent KH570 solution are mixed and stirred at 80°C for 5h to react to obtain a reaction product, and the reaction product is filtered, washed and dried to obtain a modified activated carbon;

[0227] (5) mixing the silica / nanosilver aerogel obtained in step (3), the modified activated carbon obtained in step (4) and deionized water in a mass ratio of 40:10:100, and performing ultrasonic dispersion at an ultrasonic power of 700 W for 10 h during the mixing process to obtain a composite filler solution;

[0228] Polylactic acid resin, polyethylene glycol 2000 and composite filler solution are put into a melt-blowing device in a mass ratio of 100:10:30, and the surface of the composite base fabric layer 1 obtained in step (2) is melt-blown by the melt-blowing device to form a modified filter material layer 2 with a thickness of 4 mm and an average pore size of 25 μm; wherein the temperature of the first zone of the second screw extruder is 180°C, the temperature of the second zone is 200°C, the temperature of the third zone is 210°C, the temperature of the fourth zone is 220°C, the temperature of the fifth zone is 230°C, and the screw speed is 200 r / min; the temperature of the high-pressure hot air is 200°C, and the pressure is 0.3 MPa; the flow rate of the metering pump 4 is 90 g / min; then, the composite layer composed of the modified filter material layer 2 and the composite base fabric layer 1 is subjected to corona electret treatment, the electric field intensity of the corona electret treatment is 10 kV / cm, the DC voltage is 100 kV, the charging distance is 10 cm, and the electret time is 40 s. After the corona electret treatment, the following is obtained Figure 2 Multi-layer ultra-fine polypropylene modified filter bag shown.

[0229] Comparative Example 1

[0230] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag, which differs from Example 1 in that, in step (2), the mass ratio of the coated polypropylene fiber to the zinc nitrate hexahydrate in the zinc nitrate solution is adjusted to 1:15, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0231] Comparative Example 2

[0232] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag, which differs from Example 1 in that, in step (2), the mass ratio of the coated polypropylene fiber to the zinc nitrate hexahydrate in the zinc nitrate solution is adjusted to 1:35, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0233] Comparative Example 3

[0234] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag. The difference from Example 1 is that in step (4), the heating temperature of the high-temperature oxidation treatment is adjusted to 550° C., and the other process parameters and operating steps are exactly the same as those in Example 1.

[0235] Comparative Example 4

[0236] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag. The difference from Example 1 is that in step (4), the heating temperature of the high-temperature oxidation treatment is adjusted to 750° C., and the other process parameters and operating steps are exactly the same as those in Example 1.

[0237] Comparative Example 5

[0238] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag. The difference from Example 1 is that in step (4), the heating time of the high-temperature oxidation treatment is adjusted to 20 minutes, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0239] Comparative Example 6

[0240] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag. The difference from Example 1 is that in step (4), the heating time of the high-temperature oxidation treatment is adjusted to 60 minutes, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0241] Comparative Example 7

[0242] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag, which differs from Example 1 in that in step (5), the mass ratio of silica / nanosilver aerogel, modified activated carbon and deionized water is adjusted to 25:8:100, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0243] Comparative Example 8

[0244] This comparative example provides a method for manufacturing a multi-layer ultrafine polypropylene modified filter bag, which differs from Example 1 in that, in step (5), the mass ratio of silica / nanosilver aerogel, modified activated carbon and deionized water is adjusted to 45:8:100, and the other process parameters and operating steps are exactly the same as those in Example 1.

[0245] The filtration performance and mechanical properties of the multi-layer ultrafine polypropylene modified filter bags provided in Examples 1-5 and Comparative Examples 1-8 were tested, and the specific test steps are as follows:

[0246] (1) Filtration performance

[0247] The full-particle dust filtration efficiency of the multi-layer ultrafine polypropylene modified filter bag was tested with reference to GB / T 38019-2019 “Test method for dust filtration performance of industrial filter cloth”. The test results are shown in Table 1.

[0248] (2) Mechanical properties

[0249] Referring to GB / T 24218.3-2010 “Test Methods for Nonwoven Fabrics”, the tensile strength of the multi-layer ultrafine polypropylene modified filter bag was tested at room temperature and pressure using a universal material testing machine. The sample was cut to 150mm×50mm, the clamping distance was set to 100mm, and the tensile speed was set to 100mm / min; each sample was tested 5 times and the average value was taken. The test results are shown in Table 1.

[0250] Table 1 Test results of multi-layer ultrafine polypropylene modified filter bags provided in Examples 1-5 and Comparative Examples 1-8

[0251]

[0252] It can be seen from the test data provided in Table 1 that the multi-layer ultra-fine polypropylene modified filter bags prepared in Examples 1-5 have a higher full-particle dust filtration efficiency than Comparative Examples 1-8, which indicates that the multi-layer ultra-fine polypropylene modified filter bags prepared by the manufacturing method provided by the present invention have excellent filtration performance. In addition, the tensile strength of the multi-layer ultra-fine polypropylene modified filter bags prepared in Examples 1-5 is higher than that of Comparative Examples 1-8, which indicates that the multi-layer ultra-fine polypropylene modified filter bags prepared by the manufacturing method provided by the present invention have excellent mechanical properties.

[0253] It can be seen from the test data of Example 1, Comparative Example 1 and Comparative Example 2 that the full-particle dust filtration efficiency and tensile strength of the multi-layer ultrafine polypropylene modified filter bags prepared in Comparative Examples 1 and 2 are lower than those in Example 1. This is because the amount of zinc nitrate hexahydrate used in Comparative Example 1 is too low, resulting in insufficient loading of the MOFs material coated on the surface of the polypropylene fiber, affecting the filtration performance and mechanical properties of the filter bag; while the amount of zinc nitrate hexahydrate used in Comparative Example 2 is too high, resulting in the MOFs material coated on the surface of the polypropylene fiber agglomerating and accumulating to form lumps. When the filter bag is stretched by external force, the MOFs material agglomerates are easily detached from the surface of the coated polypropylene fiber, which not only affects the filtration performance of the filter bag, but also affects the mechanical properties of the filter bag.

[0254] It can be seen from the test data of Example 1, Comparative Example 3 and Comparative Example 4 that the full-particle dust filtration efficiency of the multi-layer ultrafine polypropylene modified filter bags prepared in Comparative Examples 3 and 4 is lower than that in Example 1. This is because the heating temperature of the high-temperature oxidation treatment in Comparative Example 3 is too low to form abundant micropores on the surface of the activated carbon, thereby affecting the adsorption capacity of the modified activated carbon, and ultimately leading to a decrease in the filtration performance of the filter bag; while the heating temperature of the high-temperature oxidation treatment in Comparative Example 4 is too high, which will cause the generated micropores to collapse, resulting in a decrease in the micropore volume of the activated carbon, and ultimately leading to a decrease in the filtration performance of the filter bag.

[0255] It can be seen from the test data of Example 1, Comparative Example 5 and Comparative Example 6 that the full-particle dust filtration efficiency of the multi-layer ultrafine polypropylene modified filter bags prepared in Comparative Examples 5 and 6 is lower than that in Example 1. This is because the heating time of the high-temperature oxidation treatment in Comparative Example 5 is too short, and abundant micropores cannot be formed on the surface of the activated carbon, which in turn affects the adsorption capacity of the modified activated carbon, and ultimately leads to a decrease in the filtration performance of the filter bag; and the heating time of the high-temperature oxidation treatment in Comparative Example 6 is too long, which will cause the generated micropores to collapse, resulting in a decrease in the micropore volume of the activated carbon, and ultimately leads to a decrease in the filtration performance of the filter bag.

[0256] It can be seen from the test data of Example 1, Comparative Example 7 and Comparative Example 8 that the full-particle dust filtration efficiency and tensile strength of the multi-layer ultrafine polypropylene modified filter bags prepared in Comparative Examples 7 and 8 are lower than those in Example 1. This is because the amount of silica / nanosilver aerogel added in Comparative Example 7 is too low, and the mechanical enhancement and pollutant adsorption effects of silica / nanosilver aerogel cannot be fully exerted, resulting in the mechanical properties and filtration performance of the modified filter material layer 2 formed after melt-blowing are low; while the amount of silica / nanosilver aerogel added in Comparative Example 8 is too high, which will inhibit the crystallization of polylactic acid resin to a certain extent, and will also cause agglomeration in the polylactic acid resin matrix, resulting in a decrease in the mechanical properties of the modified filter material layer 2 formed after melt-blowing; in addition, excessive silica / nanosilver aerogel will cause the average diameter of the melt-blown fibers to be too large, and the average pore size of the modified filter material layer 2 will increase, and pollutants and particulate matter cannot be effectively intercepted, resulting in a decrease in the filtration performance of the modified filter material layer 2 formed after melt-blowing.

[0257] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A multi-layer ultra-fine polypropylene modified filter bag, characterized in that: The multi-layer ultrafine polypropylene modified filter bag comprises a composite base fabric layer and a modified filter material layer stacked in sequence; The composite base fabric layer is woven from modified composite polypropylene fibers, the modified composite polypropylene fibers include composite polypropylene fibers, a polydopamine layer coated on the surface of the composite polypropylene fibers, and a MOFs material loaded on the surface of the polydopamine layer, and the composite polypropylene fibers are prepared by sequentially melt extrusion, cooling granulation, and melt spinning of polypropylene resin and chitosan; The modified filter material layer is formed by melt-blowing a resin mixture onto the surface of the composite base fabric layer through a melt-blowing device, wherein the resin mixture includes polylactic acid resin, polyethylene glycol, silicon dioxide / nanosilver aerogel and modified activated carbon, and the modified activated carbon is obtained by sequentially subjecting activated carbon to chemical oxidation modification, high-temperature oxidation modification and silane coupling agent surface modification; The multi-layer ultrafine polypropylene modified filter bag is specifically prepared by the following method: (I) adding a titanate coupling agent to an ethanol aqueous solution, mixing, stirring and heating to obtain a coupling agent solution, then adding sodium dodecylbenzene sulfonate to the coupling agent solution, mixing and stirring to obtain a composite modified solution; Chitosan is dry-milled to obtain chitosan particles, the chitosan particles are dispersed in the composite modified solution, mixed and stirred evenly, and then filtered, washed and dried to obtain modified chitosan particles; the modified chitosan particles and polypropylene resin are mixed and put into a first screw extruder for melt extrusion, and composite polypropylene masterbatch is obtained after cooling and granulation, and the composite polypropylene masterbatch is melt-spun to obtain composite polypropylene fiber; (II) mixing dopamine hydrochloride with Tris-HCl buffer to obtain a dopamine solution, immersing the composite polypropylene fiber obtained in step (I) in the dopamine solution to form a polydopamine layer on the surface of the composite polypropylene fiber, taking out, washing and drying, and obtaining a coated polypropylene fiber; A zinc nitrate solution and a 2-methylimidazole solution are prepared respectively, and the coated polypropylene fiber is immersed in the zinc nitrate solution, wherein the mass ratio of the coated polypropylene fiber to the zinc nitrate hexahydrate in the zinc nitrate solution is 1:(20-30), and the coated polypropylene fiber is immersed in the zinc nitrate solution for 50-60 minutes; then the 2-methylimidazole solution is dripped into the solution, and stirring is continued during the dripping process to generate MOFs material in situ on the surface of the polydopamine layer, and the modified composite polypropylene fiber is obtained after washing and drying, and the modified composite polypropylene fiber is woven to form a composite base fabric layer; (III) mixing tetraethyl orthosilicate with an ethanol aqueous solution to obtain a tetraethyl orthosilicate solution, and adding a nitric acid solution to the tetraethyl orthosilicate solution to adjust the pH value thereof to obtain a precursor solution; The precursor solution is heated in a water bath to obtain a silica sol; the silica sol is dripped into a silver nitrate solution, and the reaction is stirred under light-proof conditions to obtain a silica / nanosilver sol; a mixed solution consisting of ammonia water, ethanol and deionized water is added to the silica / nanosilver sol, and the mixture is stirred and heated to gel the silica / nanosilver sol to form a silica / nanosilver gel; the silica / nanosilver gel is allowed to stand, aged and washed in sequence, and the washed silica / nanosilver gel is immersed in a polydimethylsiloxane solution for hydrophobic modification, and finally the silica / nanosilver aerogel powder is obtained after washing, drying and grinding; (IV) impregnating activated carbon in an acid solution, filtering, washing and drying after the impregnation to obtain chemically oxidized activated carbon; placing the chemically oxidized activated carbon in a tubular furnace, introducing a mixed gas composed of oxygen and nitrogen into the tubular furnace, and subjecting the chemically oxidized activated carbon to high-temperature oxidation treatment to obtain composite oxidized activated carbon, wherein the heating temperature of the high-temperature oxidation treatment is 600-700° C., and the heating time of the high-temperature oxidation treatment is 30-50 min; dispersing the composite oxidized activated carbon in cyclohexane to form an activated carbon suspension, adding a silane coupling agent solution to the activated carbon suspension under stirring conditions, mixing, stirring and heating to react to obtain a reaction product, and filtering, washing and drying the reaction product to obtain modified activated carbon; (V) mixing the silica / nanosilver aerogel obtained in step (III), the modified activated carbon obtained in step (IV) and deionized water, and then ultrasonically dispersing them to obtain a composite filler solution, wherein the mass ratio of the silica / nanosilver aerogel, the modified activated carbon and the deionized water is (30-40):(8-10):100; putting polylactic acid resin, polyethylene glycol and the composite filler solution into a melt-blowing device, and melt-blowing the surface of the composite base fabric layer obtained in step (II) through the melt-blowing device to form a modified filter material layer; then, subjecting the composite layer composed of the modified filter material layer and the composite base fabric layer to a corona electret treatment to obtain the multi-layer ultrafine polypropylene modified filter bag.

2. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: The warp density of the composite base fabric layer is 300-350 yarns / 10cm; The weft density of the composite base fabric layer is 250-300 threads / 10cm; The thickness of the composite base fabric layer is 1-3 mm; The average pore size of the composite base fabric layer is 60-70 μm; The thickness of the modified filter material layer is 2-4 mm; The average pore size of the modified filter material layer is 15-25 μm.

3. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (I), the volume ratio of ethanol to deionized water in the ethanol aqueous solution is (8-9):1; The stirring time of the titanate coupling agent and the ethanol aqueous solution is 0.5 to 1.5 hours; The heating temperature of the titanate coupling agent and the ethanol aqueous solution is 50-60° C.; The concentration of the titanate coupling agent in the coupling agent solution is 1-5 g / L; The mass ratio of the titanate coupling agent in the coupling agent solution to the sodium dodecylbenzene sulfonate is (1.5-2.5):1; The stirring time of the coupling agent solution and the sodium dodecylbenzene sulfonate is 10 to 30 minutes; The ball milling time of the chitosan is 3 to 5 hours; The ball milling speed of the chitosan is 300-400 rpm; The particle size of the chitosan particles is 20-30 nm; The mass ratio of the chitosan particles to the titanate coupling agent in the composite modified solution is 1:(0.1-0.2); The stirring time of the chitosan particles and the composite modified solution is 1 to 3 hours; The mass ratio of the modified chitosan particles to the polypropylene resin is (0.02-0.03):1; The extrusion temperature of the first screw extruder is 190-200°C; The screw speed of the first screw extruder is 100-200 r / min.

4. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (II), the mass fraction of dopamine hydrochloride in the dopamine solution is 5-10 g / L; The composite polypropylene fiber is immersed in the dopamine solution for 10 to 15 hours; The zinc nitrate solution consists of zinc nitrate hexahydrate and methanol; The concentration of zinc nitrate hexahydrate in the zinc nitrate solution is 0.1-0.2 g / mL; The 2-methylimidazole solution consists of 2-methylimidazole and methanol; The concentration of 2-methylimidazole in the 2-methylimidazole solution is 0.15-0.25 g / mL; The molar ratio of zinc nitrate hexahydrate in the zinc nitrate solution to 2-methylimidazole in the 2-methylimidazole solution is 1:(3-4); The dropping speed of the 2-methylimidazole solution is 1-5 mL / min; After all the 2-methylimidazole solution was added dropwise, stirring was continued for 1 to 2 hours.

5. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (III), the volume ratio of ethanol to water in the ethanol aqueous solution is 1:(1-2); The volume ratio of the tetraethyl orthosilicate to the ethanol aqueous solution is 1:(4-5); Adding the nitric acid solution dropwise to adjust the pH value of the tetraethyl orthosilicate solution to 2-3; The concentration of the nitric acid solution is 1-2 mol / L; The water bath heating temperature of the precursor solution is 40-60°C; The water bath heating time of the precursor solution is 80 to 120 minutes; The concentration of the silver nitrate solution is 0.08-0.1 mol / L; The ratio of silver nitrate in the silver nitrate solution to the tetraethyl orthosilicate is (3-5) mg:1 mL; The reaction time of the silica sol and the silver nitrate solution is 1 to 3 hours; The volume ratio of ammonia water, ethanol and deionized water in the mixed solution is 1:(20-30):(2-3); The volume ratio of the tetraethyl orthosilicate to the ammonia water in the mixed solution is 1:(100-150); The mass fraction of the ammonia water is 25-30wt%; The stirring time of the silica / nanosilver sol and the mixed solution is 5 to 6 hours; The heating temperature of the silica / nanosilver sol and the mixed solution is 30-40° C.; The silica / nanosilver gel is allowed to stand for 24 to 48 hours. The silicon dioxide / nanosilver gel is immersed in anhydrous ethanol for 24 to 48 hours for aging; The polydimethylsiloxane solution consists of polydimethylsiloxane and n-hexane; The mass fraction of polydimethylsiloxane in the polydimethylsiloxane solution is 10-20wt%; The ratio of the silicon dioxide / nanosilver gel to the polydimethylsiloxane solution is 1 g: (100-200) mL; The immersion time of the silicon dioxide / nanosilver gel in the polydimethylsiloxane solution is 1 to 2 hours.

6. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (IV), the mass fraction of the acid solution is 30-40wt%; The acid solution is any one of hydrochloric acid solution, phosphoric acid solution, nitric acid solution, and sulfuric acid solution, or a combination of at least two thereof; The ratio of the activated carbon to the acid in the acid solution is 1 g: (2-3) mL; The activated carbon is immersed in the acid solution for 3 to 5 hours; The volume ratio of oxygen to nitrogen in the mixed gas is 1:(15-20); The mass fraction of the composite oxidized activated carbon in the activated carbon suspension is 20-30wt%; The mass fraction of the silane coupling agent solution is 10-20wt%; The mass ratio of the composite oxidized activated carbon in the activated carbon suspension to the silane coupling agent in the silane coupling agent solution is 1:(1.5-2.5); The stirring time of the activated carbon suspension and the silane coupling agent solution is 5 to 6 hours; The heating temperature of the activated carbon suspension and the silane coupling agent solution is 70-80°C.

7. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (V), the ultrasonic power of the ultrasonic dispersion after the silica / nanosilver aerogel, the modified activated carbon and the deionized water are mixed is 600-700W; The ultrasonic dispersion time of the silica / nanosilver aerogel, the modified activated carbon and the deionized water after mixing is 10 to 12 hours; The mass ratio of the polylactic acid resin, the polyethylene glycol and the composite filler solution is 100:(5-10):(20-30).

8. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (V), the meltblowing equipment includes a screw extruder, a metering pump and a meltblowing head connected in sequence, a row of meltblowing ports are provided at the bottom of the meltblowing head, and air inlets connected to the meltblowing ports are symmetrically provided at the two side walls of the meltblowing head. A winding assembly consisting of a unwinding roller and a winding roller is provided below the meltblowing head, and the composite base fabric layer is wound between the unwinding roller and the winding roller; during the meltblowing process, the composite base fabric layer is continuously transported below the meltblowing head by the winding assembly to transfer the composite base fabric layer to the meltblowing head. The lactic acid resin, the polyethylene glycol and the composite filler solution are put into a second screw extruder, and a mixed melt is formed after being melt-extruded by the second screw extruder. The mixed melt is injected into the meltblowing head through a metering pump, and high-pressure hot air is injected into the meltblowing head through the air inlet. Under the stretching effect of the high-pressure hot air, the mixed melt passes through the meltblowing port to form a melt fine flow curtain and falls onto the surface of the continuously transmitted composite base fabric layer, and after cooling and self-bonding, a modified filter material layer is formed on the surface of the composite base fabric layer; The interior of the barrel of the second screw extruder is divided into a first zone, a second zone, a third zone, a fourth zone and a fifth zone with different temperatures along the material flow direction; The temperature of the first zone is 160-180°C; The temperature of the second zone is 180-200°C; The temperature of the third zone is 200-210°C; The temperature of the fourth zone is 210-220°C; The temperature of the fifth zone is 220-230°C; The screw speed of the second screw extruder is 100-200 r / min; The temperature of the high pressure hot air is 180-200°C; The pressure of the high-pressure hot air is 0.2~0.3MPa; The flow rate of the metering pump is 80-90 g / min.

9. The multi-layer ultrafine polypropylene modified filter bag according to claim 1, characterized in that: In step (V), the electric field intensity of the corona electret treatment is 9-10 kV / cm; The DC voltage of the corona electret treatment is 90-100 kV; The charging distance of the corona electret treatment is 9 to 10 cm; The corona electret treatment has a charging time of 30 to 40 seconds.