A broadband and ultra-low power loss manganese-zinc ferrite material for 5G base stations
By adding specific dopants and step processing to the manganese-zinc ferrite material, the problem of high-frequency power loss in 5G base stations is solved, the heat resistance of the material is improved and the loss is reduced, and the broadband ultra-low power requirement of 5G base stations is achieved. Loss requirements.
Patent Information
- Application Number
- CN202410549435.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The manganese-zinc ferrite material of 5G base stations has high power loss at high frequencies and is difficult to meet low-power requirements. Existing technology has limited improvement in its performance.
The main formula and dopant formula of specific proportions are used, including Fe2O3, MnO, ZnO, etc., and are prepared through steps such as pre-calcination, ball milling, granulation and sintering, and dopants such as Co2O3, YBCO, CTAB are added to improve the material's properties. Heat resistance and magnetic induction strength, and reduce hysteresis loss through the combination of TiO2 and YBCO.
It significantly reduces the high-frequency loss of manganese-zinc ferrite materials, improves the material's heat resistance and magnetic induction intensity, and meets the broadband ultra-low power loss requirements of 5G base stations.
Smart Images

Figure BDA0004823809840000071 
Figure BDA0004823809840000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of ferrite technology, and in particular to a broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations. Background Art
[0002] 5G mobile communication is an advanced network technology that can greatly improve spectrum utilization, network communication speed and experience. In the construction and application of 5G technology, 5G base stations are one of the indispensable links in the industrial chain. Due to the large frequency bandwidth and high transmission power of 5G base stations, their power consumption will increase significantly compared to 4G base stations. In order to effectively reduce the high-frequency and low-loss of the switching power supply in 5G base stations, higher technical requirements are put forward for ferrite soft magnetic materials. Taking manganese-zinc ferrite as an example, it has the advantages of high saturation flux density and high initial magnetic permeability, but it is still necessary to study and manufacture a manganese-zinc ferrite material suitable for 5G base stations with ultra-low power loss. Summary of the invention
[0003] The purpose of the present invention is to provide a broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations, which has the effect of ultra-low power consumption.
[0004] The above technical objectives of the present invention are achieved through the following technical solutions: A broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations, including a main formula and a dopant formula, wherein the components and proportions of the main formula are:
[0005] Fe2O3 71~72mol%
[0006] MnO 20~21mol%
[0007] ZnO 7~9mol%
[0008] The total proportion of each main formula is 100 mol%;
[0009] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:
[0010] CaCO3 100~800PPM
[0011] SnO2 100~300PPM
[0012] Co2O3 50~80PPM
[0013] Bi2O3 50~100PPM
[0014] Nano-SiO2 50~100PPM
[0015] MoO3 50-200PPM
[0016] ZrO2 50-100PPM
[0017] Composite dopants 10-15PPM;
[0018] The preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 50-60 parts of YBCO, and 10-20 parts of CTAB are mixed, and then kept at 245-250° C. for 0.5-1 h to obtain the composite dopant.
[0019] The present invention is further configured as follows: wherein the components and proportions of the main formula are:
[0020] Fe2O3 71mol%
[0021] MnO 20mol%
[0022] ZnO 9mol%
[0023] The total proportion of each main formula is 100 mol%.
[0024] The present invention is further configured as follows: relative to the total amount of the main formula, the components and weight percentages in the dopant formula are respectively:
[0025] CaCO3 700PPM
[0026] SnO2 200PPM
[0027] Co2O3 50PPM
[0028] Bi2O3 50PPM
[0029] Nano-SiO2 80PPM
[0030] MoO3 200PPM
[0031] ZrO2 100PPM
[0032] Composite dopant 15PPM.
[0033] The present invention is further configured as follows: the preparation method comprises the following steps:
[0034] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO, SnO2 powder according to the ratio requirements, and preliminarily mix them evenly;
[0035] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;
[0036] Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain pre-sintered powder;
[0037] Step S4: secondary batching: adding CaCO3, SnO2, Co2O3, Bi2O3, nano-SiO2, MoO3, ZrO2, and composite dopants to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture;
[0038] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;
[0039] Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve;
[0040] Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device;
[0041] Step S8: Secondary sintering: The annular green billet is sintered in an air atmosphere to obtain a broadband ultra-low power loss manganese-zinc ferrite material targeted for 5G base stations.
[0042] The present invention is further configured as follows: the pre-burning temperature in step S3 is 950°C to 1000°C.
[0043] The present invention is further configured as follows: the sintering temperature in step S8 is 1000°C-1300°C.
[0044] The present invention is further configured as follows: the preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 55 parts of YBCO, and 10 parts of CTAB are taken, mixed, and then kept at 245-250°C for 0.5h to obtain the composite dopant.
[0045] The present invention is further configured as follows: step S5' is further included between step S5 and step S6: rapid high-temperature impurity removal: placing the mixture after the secondary ball milling in an oven and heating it for 20-30 minutes.
[0046] The present invention is further configured as follows: the mixture is placed in an oven and heated to 400° C.-500° C.
[0047] The present invention is further configured as follows: during granulation in step S6, a PVA solution with a binder content of 7 wt% to 10 wt% is added, and spray drying is performed to form small particles, which are then sieved.
[0048] The beneficial effects of the present invention are:
[0049] 1. Co2O3 is added to the dopant formula of the present invention. The metal ion doping in Co2O3 will replace the Fe at the B position of MnZn ferrite. 3+ and Mn 3+ , thereby increasing the AB super exchange effect, improving the heat resistance of the material, broadening the working temperature of the material, and increasing the Curie temperature of the material, which will also increase the density of the sintered ferrite and effectively improve the saturation magnetic induction intensity of the material.
[0050] 2. Although Co2O3 doping can improve the saturation flux density of soft magnets, it is easy to cause discontinuous growth of the microstructure of soft magnets, irregular crystallization, and the generation of bubbles in various areas inside the crystal, thereby affecting the initial magnetic permeability and power loss performance of the material. During sintering, the added YBCO can melt and penetrate preferentially to improve the connection between grains, make the material crystal form grow continuously, effectively reduce the generation of pores in the material, and effectively reduce the hysteresis loss of the material, so as to reduce the total power loss of the material under the condition of ensuring high Bs value by Co2O3 doping.
[0051] 3. In the prior art, after SnO2 enters into the manganese-zinc ferrite, Sn 4+ Ions can replace part of the Fe 3+ The ions enter the spinel lattice of the ferrite. Sn 4+ Will be with Fe 2+ Combination to form ion pairs, Fe 2+ ions to bind Fe 2+ Ions do not participate in the electron hopping mechanism, thus reducing high-frequency losses. 4+ As a commonly used dopant in the prior art, although it is helpful to reduce the loss of ferrite, its reduction is limited. The present invention mixes it with the raw materials of the main formula in advance and pre-sinters it to reduce the Sn at the grain boundary. 4+ The amount of ions is increased so that they can enter the crystal lattice as much as possible, which is conducive to obtaining smaller uniform grains, and can achieve better magnetic properties while further reducing high-frequency losses.
[0052] 4. Although TiO2 is a commonly used dopant to reduce losses, 4+ Mainly enter the lattice and replace part of Fe 3+ Ions enter the spinel lattice of ferrite and also react with Sn 4+ Will be with Fe 2+ Combining to form ion pairs to reduce high-frequency loss, but according to the law of charge conservation, it will inevitably produce a considerable amount of Fe 2+ , too much Fe 2+ This will cause the ferrite resistivity to decrease and the energy consumption to increase. 4+Basically, it will not remain at the grain boundary. The present invention creatively mixes TiO2 with YBCO and CTAB and then fires them. CTAB can combine TiO2 with YBCO to make Ti 4+ It can stay at the grain boundary as much as possible, significantly increase the resistance value at the grain boundary, and significantly reduce the high-frequency loss of the manganese-zinc ferrite material. DETAILED DESCRIPTION
[0053] The technical solutions in the embodiments are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0054] Embodiment 1: A broadband ultra-low power loss manganese-zinc ferrite material for a 5G base station, comprising a main formula and a dopant formula, wherein the components and proportions of the main formula are:
[0055] Fe2O3 71mol%
[0056] MnO 20mol%
[0057] ZnO 9mol%
[0058] The total proportion of each main formula is 100 mol%;
[0059] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:
[0060] CaCO3 700PPM
[0061] SnO2 200PPM
[0062] Co2O3 50PPM
[0063] Bi2O3 50PPM
[0064] Nano-SiO2 80PPM
[0065] MoO3 200PPM
[0066] ZrO2 100PPM
[0067] Composite dopant 15PPM.
[0068] The preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 55 parts of YBCO, and 10 parts of CTAB are mixed, and then kept at 245-250° C. for 0.5 h to obtain the composite dopant.
[0069] The preparation method of the broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations comprises the following steps:
[0070] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO, SnO2 powder according to the ratio requirements, and preliminarily mix them evenly;
[0071] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;
[0072] Step S3: pre-sintering: the powder obtained by ball milling in step S2 is heated to a certain temperature in an air atmosphere, kept at this temperature for 1 to 3 hours, and cooled in the furnace to obtain a pre-sintered powder; the pre-sintering temperature in step S3 is 950°C to 1000°C;
[0073] Step S4: secondary batching: adding CaCO3, SnO2, Co2O3, Bi2O3, nano-SiO2, MoO3, ZrO2, and composite dopants to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture;
[0074] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;
[0075] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;
[0076] Step S6: Granulation: Adding an adhesive to the mixture after the secondary ball milling to form small particles and then sieving; During the granulation of step S6, 7wt% to 10wt% of PVA solution as an adhesive is added, and spray drying is performed to form small particles and then sieving;
[0077] Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device;
[0078] Step S8: secondary sintering: the annular green billet is sintered in an air atmosphere to obtain a broadband ultra-low power loss manganese-zinc ferrite material targeted for 5G base stations. The sintering temperature in step S8 is 1000°C-1300°C.
[0079] Embodiment 2: A broadband ultra-low power loss manganese-zinc ferrite material for a 5G base station, comprising a main formula and a dopant formula, wherein the components and proportions of the main formula are:
[0080] Fe2O3 72mol%
[0081] MnO 21 mol%
[0082] ZnO 7mol%
[0083] The total proportion of each main formula is 100 mol%;
[0084] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:
[0085] CaCO3 200PPM
[0086] SnO2 150PPM
[0087] Co2O3 50PPM
[0088] Bi2O3 80PPM
[0089] Nano-SiO2 100PPM
[0090] MoO3 150PPM
[0091] ZrO2 50PPM
[0092] Composite dopant 10PPM.
[0093] The preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 55 parts of YBCO, and 10 parts of CTAB are mixed, and then kept at 245-250° C. for 0.5 h to obtain the composite dopant.
[0094] The preparation method of the broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations comprises the following steps:
[0095] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO, SnO2 powder according to the ratio requirements, and preliminarily mix them evenly;
[0096] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;
[0097] Step S3: pre-sintering: the powder obtained by ball milling in step S2 is heated to a certain temperature in an air atmosphere, kept at this temperature for 1 to 3 hours, and cooled in the furnace to obtain a pre-sintered powder; the pre-sintering temperature in step S3 is 950°C to 1000°C;
[0098] Step S4: secondary batching: adding CaCO3, SnO2, Co2O3, Bi2O3, nano-SiO2, MoO3, ZrO2, and composite dopants to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture;
[0099] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;
[0100] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;
[0101] Step S6: Granulation: Adding an adhesive to the mixture after the secondary ball milling to form small particles and then sieving; During the granulation of step S6, 7wt% to 10wt% of PVA solution as an adhesive is added, and spray drying is performed to form small particles and then sieving;
[0102] Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device;
[0103] Step S8: secondary sintering: the annular green billet is sintered in an air atmosphere to obtain a broadband ultra-low power loss manganese-zinc ferrite material targeted for 5G base stations. The sintering temperature in step S8 is 1000°C-1300°C.
[0104] Comparative Example 1: Example 1: A broadband ultra-low power loss manganese-zinc ferrite material for a 5G base station, comprising a main formula and a dopant formula, wherein the components and proportions of the main formula are:
[0105] Fe2O3 71mol%
[0106] MnO 20mol%
[0107] ZnO 9mol%
[0108] The total proportion of each main formula is 100 mol%;
[0109] The components and weight percentages of the dopant formula relative to the total amount of the main formula are:
[0110] CaCO3 700PPM
[0111] SnO2 200PPM
[0112] Co2O3 50PPM
[0113] Bi2O3 50PPM
[0114] Nano-SiO2 80PPM
[0115] MoO3 200PPM
[0116] ZrO2 100PPM
[0117] The preparation method of the broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations comprises the following steps:
[0118] Step S1: primary batching: weigh the materials required to prepare the main formula raw materials Fe2O3, MnO, ZnO, SnO2 powder according to the ratio requirements, and preliminarily mix them evenly;
[0119] Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder;
[0120] Step S3: pre-sintering: the powder obtained by ball milling in step S2 is heated to a certain temperature in an air atmosphere, kept at this temperature for 1 to 3 hours, and cooled in the furnace to obtain a pre-sintered powder; the pre-sintering temperature in step S3 is 950°C to 1000°C;
[0121] Step S4: secondary batching: adding CaCO3, SnO2, Co2O3, Bi2O3, nano-SiO2, MoO3, and ZrO2 to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture;
[0122] Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling;
[0123] Step S5': Rapid high-temperature impurity removal: Place the mixture after the secondary ball milling in an oven and heat it for 20-30 minutes; Place the mixture in an oven and heat it to 400°C-500°C;
[0124] Step S6: Granulation: Adding an adhesive to the mixture after the secondary ball milling to form small particles and then sieving; During the granulation of step S6, 7wt% to 10wt% of PVA solution as an adhesive is added, and spray drying is performed to form small particles and then sieving;
[0125] Step S7: pressing and molding: pressing the granulated small particles into annular green materials on a pressing device;
[0126] Step S8: secondary sintering: the annular green billet is sintered in an air atmosphere to obtain a broadband ultra-low power loss manganese-zinc ferrite material targeted for 5G base stations. The sintering temperature in step S8 is 1000°C-1300°C.
[0127] The magnetic properties of the standard ring samples of the soft ferrite materials prepared in Examples 1-2 and Comparative Example 1 with an outer diameter of 25×inner diameter of 15×height of 7.5 were tested and compared with the performance of TDK PC95 of a Japanese company. The results are shown in Table 1:
[0128] Table 1 Magnetic properties of each sample
[0129]
[0130]
Claims
1. A broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations, characterized in that: It includes a main formula and an adulterant formula, wherein the components and proportions of the main formula are: Fe2O371~72mol% MnO 20~21mol% ZnO 7~9mol% The total ratio of the main formula is 100 mol%; Relative to the total amount of the main formula, the components and weight percentages in the dopant formula are: CaCO3100~800PPM SnO2 100~300PPM Co2O3 50~80PPM Bi2O3 50~100PPM Nano-SiO2 50~100PPM MoO3 50-200PPM ZrO2 50-100PPM Composite dopants 10-15PPM; The preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 50-60 parts of YBCO, and 10-20 parts of CTAB are mixed and kept at 245-250° C. for 0.5-1 h to obtain the composite dopant.
2. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 1, characterized in that: The components and proportions of the main formula are: Fe2O371mol% MnO 20mol% ZnO 9mol% The total proportion of the main formula is 100 mol%.
3. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 2, characterized in that: Relative to the total amount of the main formula, the components and weight percentages in the dopant formula are: CaCO3700PPM SnO2 200PPM Co2O3 50PPM Bi2O3 50PPM Nano-SiO2 80PPM MoO3 200PPM ZrO2 100PPM Composite dopant 15PPM.
4. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 1, characterized in that: The preparation method comprises the following steps, including the following steps: Step S1: primary batching: weigh the main formula raw materials Fe2O3, MnO, and ZnO powder according to the ratio requirements, and preliminarily mix them evenly; Step S2: primary ball milling: putting the main formula powder preliminarily mixed in step S1 into a ball mill, and ball milling to obtain primary ball milled powder; Step S3: pre-sintering: heating the powder obtained by ball milling in step S2 to a certain temperature in an air atmosphere, keeping the temperature for 1 to 3 hours, and cooling with the furnace to obtain pre-sintered powder; Step S4: secondary batching: adding CaCO3, SnO2, Co2O3, Bi2O3, nano-SiO2, MoO3, ZrO2, and composite dopants to the pre-sintered powder, stirring and mixing to form a mixture, and then adding polysiloxane to the mixture, stirring and mixing to form a mixture; Step S5: Secondary ball milling: placing the mixture obtained in step S4 into a ball mill for secondary ball milling; Step S6: Granulation: Add a binder to the mixture after the secondary ball milling to form small particles and then sieve; Step S7: pressing and molding: pressing the granulated small particles into annular green billets on a pressing device; Step S8: Secondary sintering: The annular green body is sintered in an air atmosphere to obtain a broadband ultra-low power loss manganese-zinc ferrite material targeted for 5G base stations.
5. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 4, characterized in that: The pre-burning temperature in step S3 is 950°C to 1000°C.
6. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 4, characterized in that: The sintering temperature in step S8 is 1000°C-1300°C.
7. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 1, characterized in that: The preparation method of the composite dopant is as follows: by weight, 20 parts of TiO2, 55 parts of YBCO, and 10 parts of CTAB are mixed and kept at 245-250° C. for 0.5 h to obtain the composite dopant.
8. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 4, characterized in that: The method further includes step S5' between step S5 and step S6: rapid high-temperature impurity removal: placing the mixture after the second ball milling in an oven and heating it for 20-30 minutes.
9. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 8, characterized in that: The mixture is placed in an oven and heated to 400°C-500°C.
10. The broadband ultra-low power loss manganese-zinc ferrite material for 5G base stations according to claim 1, characterized in that: In step S6, 7 wt% to 10 wt% of a PVA solution as a binder is added during granulation, and spray drying is performed to form small particles, which are then sieved.
Citation Information
Patent Citations
Perovskite light emitting device containing exciton buffer layer and method for manufacturing same
CN107210366A
High-frequency wide-temperature ultralow-loss ferrite material and preparation process thereof
CN114685154A
Cited By
Preparation process of high-frequency low-loss manganese zinc ferrite material
CN120717782A