Highly weather-resistant photovoltaic backsheet adhesive and preparation method thereof

By using the reaction of diphenylmethane diisocyanate with specific polyether polyols and branched polyester polyols in the photovoltaic backsheet adhesive, and adding additives, the weather resistance and initial bonding strength of the photovoltaic backsheet adhesive are improved, solving the problem This solves the problem of poor weather resistance in the existing technology and achieves stability in harsh environments and long-term reliability.

CN118480168BActive Publication Date: 2024-10-01SHANDONG SHANGZHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410939767.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-01
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

After long-term outdoor exposure, the existing photovoltaic backsheet adhesive's weather resistance, high temperature resistance or humidity and heat resistance will gradually decline, resulting in component performance degradation and low initial adhesion, making it unable to meet the needs of long-term outdoor applications.

Method used

A highly weather-resistant photovoltaic backsheet adhesive is prepared by reacting diphenylmethane diisocyanate with polyether polyols and branched polyester polyols of specific molecular weights, and adding plasticizers, hydrolysis stabilizers, UV absorbers and fillers. , improve its mechanical properties and hydrolysis resistance.

Benefits of technology

After 2,000 hours of testing at 85°C and 85% relative humidity, this photovoltaic backsheet adhesive can still maintain a peeling strength of greater than 6N/cm² against fluorine films and polyester films, extending the service life of photovoltaic modules and having a relatively high High initial bonding force ensures stability and reliability in complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of photovoltaic backplane adhesive, and in particular to a highly weather-resistant photovoltaic backplane adhesive and a preparation method thereof. In order to solve the problems of poor weather resistance and low adhesion of photovoltaic backplane adhesive in the prior art, the present application provides a highly weather-resistant photovoltaic backplane adhesive and a preparation method thereof, which is prepared by using two branched polyester polyols of different molecular weights and a small amount of polyether polyols to react with diphenylmethane diisocyanate, and then with other additives. The method provided by the present application improves the mechanical properties of the backplane adhesive, increases its weather resistance and service life, and not only has a high initial adhesion, but also tests the peel strength of fluorine film and polyester film, and the peel strength can still be maintained greater than 6N / cm² after 2000h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of photovoltaic backplane adhesive, and in particular to a highly weather-resistant photovoltaic backplane adhesive and a preparation method thereof. Background Art

[0002] The solar backsheet is mainly composed of fluorine-containing fluorine film, polyester film and modified EVA or PE film. The fluorine film provides outer layer protection, the middle polyester film provides good insulation performance, and the modified EVA or PE film provides bonding performance. The three layers of film are bonded together by photovoltaic backsheet adhesive to form a whole.

[0003] Photovoltaic backplane adhesive is a key material specially used for backside encapsulation of solar photovoltaic modules. It is essential to improve the reliability and service life of modules. Backplane adhesive is mainly used to bond backplane materials such as PET, PVDF and other thin film layers with solar cell modules to form a protective barrier to prevent moisture penetration, mechanical damage and environmental erosion. It also has to have good electrical insulation properties to ensure that photovoltaic modules can work stably for a long time in complex and changeable outdoor environments.

[0004] There are many types of photovoltaic backplane adhesives, such as epoxy resin-based backplane adhesives, polyurethane backplane adhesives, silicone backplane adhesives, fluororesin backplane adhesives, and water-based backplane adhesives. After long-term outdoor exposure, the weather resistance, high temperature resistance, or humidity resistance of the backplane adhesive may gradually decrease, resulting in the degradation of component performance.

[0005] CN104017531A discloses a hydrolysis-resistant photovoltaic backplane adhesive and a preparation method thereof. The adhesive of the invention comprises two components, A and B. The component A comprises a self-synthesized novel polyester polyol and corresponding additives, and the component B is an isocyanate curing agent. The molar ratio of the isocyanate group in the component B to the hydroxyl group in the component A is 1 to 1.4: 1. However, the adhesive prepared by this method has a low initial bonding force, and the bonding force is greatly reduced after long-term use, which cannot meet the application requirements of long-term outdoor exposure. Summary of the invention

[0006] In order to solve the problems of poor weather resistance and low adhesion of photovoltaic backplane adhesive in the prior art, the present application provides a highly weather-resistant photovoltaic backplane adhesive and a preparation method thereof. The method provided in the present application improves the mechanical properties of the backplane adhesive, increases its weather resistance and service life.

[0007] The present application provides a method for preparing a highly weather-resistant photovoltaic backsheet adhesive, comprising the following steps:

[0008] S1, heating diphenylmethane diisocyanate to completely melt the diphenylmethane diisocyanate, adding polyether polyol A under nitrogen protection to react to obtain a prepolymer;

[0009] S2, cooling the prepolymer obtained in step S1, adding polyester polyol B and plasticizer under nitrogen protection, continuing polymerization reaction, then adding polyester polyol C, continuing polymerization reaction, after the NCO% content reaches 1.0-2.3, obtaining a polymerization product for standby use;

[0010] S3, adding a hydrolysis stabilizer, an ultraviolet absorber and a filler to the polymerized product obtained in S2, stirring and mixing the mixture evenly to obtain a product.

[0011] Furthermore, the polyether polyol A in step S1 is polyoxypropylene glycol with an average molecular weight of more than 7000, and the amount used is 1.5-2.2 times the mass of diphenylmethane diisocyanate.

[0012] Furthermore, in step S1, the heating temperature of diphenylmethane diisocyanate is 50-65° C., and the heating time is 25-40 min. After adding polyether polyol A, the reaction is carried out for 20-30 min, and then the temperature is uniformly raised to 85-90° C. within 25-35 min, and the reaction is continued for 2-4 hours.

[0013] Furthermore, in step S2, the prepolymer is cooled to 70-75° C., and after adding polyester polyol B and plasticizer, the temperature is controlled at 75-80° C., and the polymerization reaction is continued for 2-3 hours; polyester polyol C is added, and the polymerization reaction is continued for 2-3 hours.

[0014] Furthermore, the polyester polyol B in step S2 is a 2-functionality branched polyester polyol with an average molecular weight of 1500-2500, and the amount used is 1-1.2 times the mass of diphenylmethane diisocyanate; the polyester polyol C is a 3-functionality branched polyester polyol with an average molecular weight of 900-1100, and the amount used is 0.6-1.0 times the mass of diphenylmethane diisocyanate.

[0015] Furthermore, the plasticizer is N-methylpyrrolidone, and the amount used is 4-5 times the mass of diphenylmethane diisocyanate.

[0016] Furthermore, in step S3, the hydrolysis stabilizer is a carbodiimide stabilizer, and the amount used is 0.04-0.07 times the mass of diphenylmethane diisocyanate.

[0017] Furthermore, in step S3, the ultraviolet absorber is a benzophenone absorber or a hindered amine light stabilizer, and the amount used is 0.05-0.1 times the mass of diphenylmethane diisocyanate.

[0018] Furthermore, in step S3, the filler is fumed silica or white carbon black, and the amount used is 0.05-0.1 times the mass of diphenylmethane diisocyanate.

[0019] The beneficial effects of this application are:

[0020] After 2000 hours of testing under double 85 conditions, i.e. 85°C temperature and 85% relative humidity, the photovoltaic backplane adhesive can still maintain a peel strength of more than 6N / cm² against the fluorine film and polyester film, proving its excellent resistance to high temperature and high humidity, which is crucial for photovoltaic modules used outdoors for a long time and can effectively extend the service life of the modules.

[0021] By selecting branched polyester polyols with specific molecular weights and polyether polyols in combination with diphenylmethane diisocyanate, and adding other functional additives, the hydrolysis resistance and mechanical properties of the polyurethane adhesive are improved, thereby ensuring the stability and reliability of the adhesive in harsh environments. The reasonable ratio of these components and additives not only improves the overall performance of the adhesive, but also ensures its durability in complex environments. In addition to excellent weather resistance, the adhesive also has a high initial adhesion, which is necessary for a fast and effective bonding process and the structural stability of the final product. DETAILED DESCRIPTION

[0022] The technical scheme of the present invention and its effects are further described below by specific examples. The following examples are only used to illustrate the content of the present invention and are not used to limit the protection scope of the present invention. Simple changes made to the present invention by applying the concept of the present invention are all within the scope of the protection claimed by the present invention.

[0023] The equipment used in the preparation method of the present invention can all adopt the well-known equipment in the art. The raw materials used in the present invention are all commercially available unless otherwise specified. Polyether polyol A is DDL-8000 or DDL-12000 produced by Zibo Dexin Federal Chemical Industry Co., Ltd., polyester polyol B is BY3030 or BY3001F produced by Beijing Baiyuan Chemical, polyester polyol C is COA-SOV805 of BASF, hydrolysis stabilizer is anti-hydrolysis agent UN-736 produced by Shanghai Kailia Plastic Technology Co., Ltd. or HyMax®1010 produced by Shanghai Langyi New Material Technology Co., Ltd., and ultraviolet absorber is C-81 or Tinuvin 770DF produced by BASF.

[0024] Example 1

[0025] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 150g of DDL-8000 under nitrogen protection and react for 20min. Then slowly heat it to 85°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0026] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 100g BY3030 and 400g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, continuing the polymerization reaction for 2h, then adding 60g COA-SOV805, continuing the polymerization reaction for 2h, and obtaining a polymerization product after the NCO% content reaches 2.3 for standby use;

[0027] S3. Add 4 g UN-736, 5 g Tinuvin 770DF and 5 g fumed silica to the polymerized product obtained in S2, and stir to mix evenly to obtain a product.

[0028] Example 2

[0029] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 190g of DDL-8000 under nitrogen protection and react for 30min. Then slowly heat it to 90°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0030] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 110g BY3030 and 500g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, continuing the polymerization reaction for 2h, then adding 80g COA-SOV805, continuing the polymerization reaction for 2h, and obtaining a polymerization product after the NCO% content reaches 1.6 for standby use;

[0031] S3. Add 7 g HyMax®1010, 10 g C-81 and 10 g white carbon black to the polymerized product obtained in S2, and stir to mix well to obtain the product.

[0032] Example 3

[0033] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 220g of DDL-8000 under nitrogen protection and react for 30min. Then slowly heat it to 90°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0034] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 220g BY3030 and 450g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, continuing the polymerization reaction for 2h, then adding 100g COA-SOV805, continuing the polymerization reaction for 2h, and obtaining a polymerization product after the NCO% content reaches 1.0 for standby use;

[0035] S3. Add 5.5 g HyMax®1010, 8 g Tinuvin 770DF and 7 g fumed silica to the polymerized product obtained in S2, and stir to mix well to obtain a product.

[0036] Example 4

[0037] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 220g of DDL-12000 under nitrogen protection and react for 30min. Then slowly heat it to 90°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0038] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 120g BY3001F and 500g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, continuing the polymerization reaction for 2h, then adding 100g COA-SOV805, continuing the polymerization reaction for 2h, and obtaining a polymerization product after the NCO% content reaches 1.1 for standby use;

[0039] S3. Add 7 g UN-736, 10 g C-81 and 10 g white carbon black to the polymerization product obtained in S2, and stir to mix evenly to obtain the product.

[0040] Comparative Example 1

[0041] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 220g of DDL-8000 under nitrogen protection and react for 30min. Then slowly heat it to 90°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0042] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 300g BY3030 and 500g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, and continuing the polymerization reaction for 2h. After the NCO% content reaches 2.3, the polymerization product is obtained for standby use;

[0043] S3. Add 7 g UN-736, 10 g C-81 and 10 g fumed silica to the polymerized product obtained in S2, and stir to mix evenly to obtain the product.

[0044] Comparative Example 2

[0045] S1. Heat 100g of diphenylmethane diisocyanate to 50-65°C and keep it for 30min to completely melt the diphenylmethane diisocyanate. Add 150g of DDL-4000 under nitrogen protection and react for 30min. Then slowly heat it to 90°C over 30min and continue to react for 3 hours to obtain a prepolymer.

[0046] S2, cooling the prepolymer obtained in step S1 to 70°C, adding 50g XC-488 and 500g N-methylpyrrolidone under nitrogen protection, controlling the temperature at 75-80°C, continuing the polymerization reaction for 2h, then adding 60g COA-SOV805, continuing the polymerization reaction for 2h, and obtaining a polymerization product after the NCO% content reaches 1.3 for standby use;

[0047] S3. Add 7 g HyMax®1010, 10 g C-81 and 10 g fumed silica to the polymerized product obtained in S2, and stir to mix well to obtain a product.

[0048] Sample preparation: The highly weather-resistant photovoltaic backsheet adhesive prepared above was applied on one side of the PET film by scraper coating, with an adhesive coating amount of 9 g / m 2 , dried at 80°C for 10 minutes, the pretreated PVD film was placed on the side of the PET film coating, and the above-prepared high weather resistance photovoltaic backplane adhesive was coated on the other side of the PET film by scraper coating, with a coating amount of 9g / m 2 , dried at 80℃ for 10 minutes, the pretreated PVD film was placed on the side coated with the PET film, and composited on a flat press with a pressure of 1.0MPa, at a temperature of 55℃, pressed for 30 minutes, and the composite sheet was aged at 40℃ for 48 hours, and its performance was measured. Comparative Example 1 does not use branched polyester polyol to make photovoltaic backplane adhesive, Comparative Example 2 uses polyether polyol and polyester polyol with smaller molecular weight to make photovoltaic backplane adhesive, and Comparative Example 3 uses a commercially available photovoltaic backplane adhesive.

[0049] Evaluation method: 1. Peel strength test: Cut the composite sheet into 15mm wide samples and perform a 180° peel test at a speed of 50mm / min on a universal testing machine. The reference standard is the national standard GB / T2790 "Adhesive 180° Peel Strength Test Method Flexible Material to Rigid Material".

[0050] 2. Constant moisture and heat aging resistance: Under the conditions of 85°C, 85% relative humidity, and 3000h, the peel strength of 15*200mm specimens was measured before and after the test according to the national standard. Reference standard: National standard GB / T2790 "Adhesive 180° Peel Strength Test Method Flexible Material to Rigid Material".

[0051] 3. Hydrolysis resistance test: Cook at 121℃ for 48 hours, and measure the peel strength of 15*200mm specimens before and after the test.

[0052] Table 1 Sample application performance evaluation table

[0053]

Claims

1. A method for preparing a highly weather-resistant photovoltaic backsheet adhesive, characterized in that: The following steps are involved: S1, heating diphenylmethane diisocyanate to completely melt the diphenylmethane diisocyanate, adding polyether polyol A under nitrogen protection to react to obtain a prepolymer; the polyether polyol A is a polyoxypropylene glycol having an average molecular weight of more than 7000, and the amount used is 1.5-2.2 times the mass of diphenylmethane diisocyanate; S2, cooling the prepolymer obtained in step S1, adding polyester polyol B and plasticizer under nitrogen protection, continuing polymerization reaction, then adding polyester polyol C, continuing polymerization reaction, after NCO% content reaches 1.0-2.3, obtaining a polymer product for standby use; the polyester polyol B is a 2-functionality branched polyester polyol with an average molecular weight of 1500-2500, and the amount used is 1-1.2 times the mass of the diphenylmethane diisocyanate in step S1, and the polyester polyol C is a 3-functionality branched polyester polyol with an average molecular weight of 900-1100, and the amount used is 0.6-1.0 times the mass of the diphenylmethane diisocyanate in step S1; S3, adding a hydrolysis stabilizer, an ultraviolet absorber and a filler to the polymerized product obtained in S2, stirring and mixing the mixture evenly to obtain a product.

2. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: In step S1, the diphenylmethane diisocyanate is heated to a temperature of 50-65° C. for a heating time of 25-40 min. After adding polyether polyol A, the mixture is reacted for 20-30 min, then the temperature is uniformly raised to 85-90° C. within 25-35 min, and the reaction is continued for 2-4 hours.

3. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: In step S2, the prepolymer is cooled to 70-75° C., and after adding polyester polyol B and plasticizer, the temperature is controlled at 75-80° C. and the polymerization reaction is continued for 2-3 hours; polyester polyol C is added and the polymerization reaction is continued for 2-3 hours.

4. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: The plasticizer is N-methylpyrrolidone, and the amount used is 4-5 times the mass of diphenylmethane diisocyanate.

5. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: In step S3, the hydrolysis stabilizer is a carbodiimide stabilizer, and the amount used is 0.04-0.07 times the mass of diphenylmethane diisocyanate.

6. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: In step S3, the ultraviolet absorber is a benzophenone absorber or a hindered amine light stabilizer, and the amount used is 0.05-0.1 times the mass of diphenylmethane diisocyanate.

7. The method for preparing the highly weather-resistant photovoltaic backsheet adhesive according to claim 1, characterized in that: In step S3, the filler is fumed silica or white carbon black, and the amount used is 0.05-0.1 times the mass of diphenylmethane diisocyanate.

8. A highly weather-resistant photovoltaic backsheet adhesive, characterized in that: Prepared by the method according to any one of claims 1 to 7.